A kind of foamed polyethylene particles and molded parts using the same
Through the high-temperature and autoclave foaming method and water vapor sintering molding technology of composite particles, the problems of dense cells and poor apparent quality during the molding process of EPE particles are solved, and foaming with softness, excellent resilience and low energy consumption is achieved. Polyethylene molded parts meet the packaging market's demand for materials with excellent appearance.
Patent Information
- Application Number
- CN202410443270.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-12
AI Technical Summary
Existing expanded polyethylene (EPE) particles easily lead to a dense cell structure during the molding process, which affects the apparent quality and resilience of the parts. Moreover, the appearance quality of the parts is poor and cannot meet the packaging market's demand for softness and appearance. Excellent material requirements.
It is prepared using composite particles through a high-temperature and autoclave foaming method. The core layer contains 85-97% linear low-density polyethylene and 3-10% thermoplastic elastomer, and the skin layer contains 80-100% low-density polyethylene and 0- 20% easy heat sealable polyolefin The elastomer is combined with diatomite and zeolite powder as expansion aids. Composite particles are prepared through a co-extruder and foamed using CO2 in an autoclave. The temperature and pressure in the autoclave are controlled to obtain a uniformly expanded cell structure. Finally, Formed by steam sintering.
It achieves soft texture, excellent resilience and excellent surface quality of the parts, reduces molding energy consumption, avoids the problems of dense cells and surface pits or gaps, and improves the molding density and appearance performance of EPE particles.
Smart Images

Figure GHA0000006640820000051 
Figure GHA0000006640820000061 
Figure GHA0000006640820000062
Abstract
Description
Technical Field
[0001] The invention belongs to the field of foamed polyethylene materials, and in particular relates to foamed polyethylene particles and products using the same. Background Art
[0002] Expanded polyethylene (EPE) particles and their molded products are soft in texture, have excellent resilience, and have a variety of structural shapes. They are suitable for bonding and protecting various electronic devices and fragile parts, and have broad prospects for use in the packaging field.
[0003] The known EPE particle technology methods CN105037912B and CN109651695A both add HDPE components to EPE foamed particles, which affects the unique softness of EPE. The technology method CN107312233A prepares multi-component EPE particles. Although the compression strength of the molded body is high, the overly dense pore structure may lead to poor apparent quality of the molded parts.
[0004] In view of the packaging market's demand for soft and high-quality special-shaped EPE materials, the present technology provides a method for preparing foamed polyethylene particles and molded parts thereof, which can obtain EPE particles with soft texture, excellent resilience and low molding energy consumption. The molded parts thereof have excellent appearance, i.e., there are very few or very small pits or gaps on the surface of the parts. Summary of the invention
[0005] One of the purposes of the present invention is to provide a foamed polyethylene particle and a preparation method thereof.
[0006] Another object of the present invention is to provide a molded article containing the above-mentioned foamed polyethylene particles and a method for preparing the same.
[0007] Another object of the present invention is to provide the use of the above product.
[0008] In order to achieve the above-mentioned invention object, the present application adopts the following technical solutions:
[0009] A foamed polyethylene particle is a composite particle prepared by a high-temperature and high-pressure autoclave foaming method. The composite particle comprises a core layer and a skin layer, wherein the skin layer is coated on the surface of the core layer, the core layer comprises at least 85-97 parts by weight of polyethylene A, 3-10 parts by weight of thermoplastic elastomer C, and 0.1-5 parts by weight of an expansion aid, and the skin layer comprises at least 80-100 parts by weight of polyethylene B and 0-20 parts by weight of thermoplastic elastomer D.
[0010] Polyethylene A, linear low density polyethylene, melt index 0.1-7 g / 10 min (190°C, 2.16 kg), melting point 115-130°C; preferably melt index 0.3-6 g / 10 min (190°C, 2.16 kg), melting point 116-127°C.
[0011] Thermoplastic elastomer C is one or more of SBS, SEBS and SEPS, and has a Shore hardness of 50-85A.
[0012] Polyethylene B, low density polyethylene, melt index 4-12g / 10min (190°C, 2.16kg), melting point 95-115°C; preferably melt index 5-10g / 10min (190°C, 2.16kg), melting point 97-113°C.
[0013] Thermoplastic elastomer D is a heat-sealable polyolefin elastomer with a melt index of
[0014] 4-12g / 10min (230℃, 2.16kg), melting point 55-85℃.
[0015] The expansion aid is one or both of diatomaceous earth and zeolite powder, and the average particle size is 1-15 microns.
[0016] The core layer also contains a cell nucleating agent, which is one or more of silicon dioxide, zinc borate, talcum powder, and calcium carbonate, with an average particle size of 10-15 microns, accounting for 0.01-0.15 parts by weight of the core layer material.
[0017] Composite particle preparation:
[0018] (1) Polyethylene A, thermoplastic elastomer C, cell nucleating agent, and expansion aid are mixed in a certain proportion and melt-granulated in an extruder to obtain a core layer masterbatch; the temperature of the heating section of the extruder is 200°C-240°C.
[0019] (2) After polyethylene B and thermoplastic elastomer D are uniformly mixed, they are melt-granulated in an extruder to obtain a skin masterbatch; the temperature of the heating section of the extruder is 200°C-240°C.
[0020] (3) The core layer masterbatch and the skin layer masterbatch are added to the core layer extruder and the skin layer extruder of the twin-single screw co-extruder unit respectively, and after plasticization, they are simultaneously discharged through the co-extrusion die for granulation to obtain composite particles of the skin layer covering the core layer. The temperature of the heating section of the extruder is 200°C-240°C.
[0021] Preferably, the weight percentage of the skin layer in the composite particles is 3-10%; the length of the composite particles is 1.2-3.5 mm, and the unit weight is 1-5 mg. More preferably, the length of the composite particles is 1.5-3 mm, and the unit weight is 1.2-3 mg.
[0022] Preparation of foamed particles: Add composite particles, dispersant and water into the autoclave together, seal and add CO2. Stir continuously, raise the temperature of the reactor to the foaming temperature of 115℃-133℃, adjust the pressure in the reactor to the foaming pressure of 2.2-4.4MPa, maintain under this temperature and pressure condition for 10-60min, release the pressure and discharge the material into the foaming pipe for foaming, the atmosphere temperature in the foaming pipe is 80-95℃, the atmosphere pressure in the foaming pipe is 0.01-0.08MPa, the time the material spends in the foaming pipe is 10-50s, and finally obtain foamed polyethylene particles with a bulk density of 15-120g / L, and the melting peak endothermic enthalpy value of the foamed particles in the first DSC melting curve that is higher than the inherent melting point is 20-50J / g.
[0023] A molded part of foamed polyethylene particles: obtained by sintering the foamed polyethylene particles as described above through steam, and the specific steps are: the foamed particles are pressurized by air and then steam molded.
[0024] The molding pressure of the molded part is lower than 1.2 bar, and the molded part can be produced on an EPS molding machine. The molded part has a soft texture, excellent resilience and excellent surface quality. The density of the molded part is 25-30g / L, the surface hardness is 25-35A, and the permanent compression deformation is lower than 10%.
[0025] Beneficial effects:
[0026] 1. Containing 0.1-5% of nano-microporous structure expansion aid, it helps the material absorb foaming gases such as carbon dioxide and water vapor, which is beneficial to the uniform expansion of EPE pores in the kettle foaming process, and is beneficial to improving technical problems such as high EPE foaming pressure, uneven pores, and overly dense or small pores, and is beneficial to obtaining molded parts with excellent apparent quality.
[0027] 2. The core layer is a foaming layer; the core layer contains 3-10 parts by weight of thermoplastic elastomer C, which can more effectively improve the resilience and softness of EPE. If the content is less than 3 parts by weight, the improvement effect is not obvious; if the content is higher than 10 parts by weight, the heat resistance of EPE is reduced.
[0028] 3. The skin layer is a non-foamed or slightly foamed layer; the mixture of polyethylene B and thermoplastic elastomer D in the skin layer is a material that is easily melted by heat. It is coated on the surface of the foamed core layer, giving the foamed particles an easy-to-sinter property, and the thermoplastic elastomer D helps to make the surface of the molded part soft.
[0029] In the kettle foaming process, the atmospheric pressure and temperature process parameters in the foaming pipe are conducive to the uniform foaming, expansion and shaping of EPE particles, improving the problems of difficulty in reducing density and easy shrinkage during the foaming process of EPE particles. Example
[0030] The present invention is further described below by way of examples. It should be understood that the methods described in the examples of the present invention are only used to illustrate the present invention, rather than to limit the present invention, and simple improvements to the preparation methods of the present invention under the premise of the concept of the present invention belong to the scope of protection claimed in the present invention. All raw materials and solvents used in the examples are commercially available products of corresponding purity.
[0031] Preparation Example of Foamed Polyethylene Particles:
[0032] (1) Polyethylene A, thermoplastic elastomer C, cell nucleating agent, and expansion aid are mixed in a certain proportion, and melt-granulated in an extruder to obtain a core layer masterbatch; the temperature of the heating section of the extruder is 210° C.;
[0033] (2) After polyethylene B and thermoplastic elastomer D are uniformly mixed, they are melt-granulated in an extruder to obtain a skin masterbatch; the temperature of the heating section of the extruder is 210°C;
[0034] (3) adding the core layer masterbatch and the skin layer masterbatch to the core layer extruder and the skin layer extruder of the twin-single screw co-extruder unit, respectively, and after plasticization, simultaneously passing through the co-extrusion die to form filaments and granulate to obtain composite particles of the skin layer covering the core layer; the temperature of the heating section of the extruder is 210° C.;
[0035] (4) Add the composite particles together with the dispersant and water into an autoclave, seal it, add CO2, stir continuously, raise the temperature of the autoclave to a foaming temperature of 115°C-133°C, adjust the pressure in the autoclave to a foaming pressure of 2.2-4.4MPa, maintain it under this temperature and pressure condition for 10-60min, release the pressure and discharge the material into a foaming pipe for foaming, the atmosphere temperature in the foaming pipe is 80-95°C, the atmosphere pressure in the foaming pipe is 0.01-0.08MPa, the time the material spends in the foaming pipe is 10-50s, and finally obtain foamed polyethylene particles.
[0036] The products of Examples 1-5 and Comparative Examples 1-6 and 8-9 were prepared according to the above preparation method.
[0037] Table 1 Main raw material manufacturers and performance parameters used in this application
[0038]
[0039] Table 2 Formulation parameters of composite particles S1-S5 and D1-D8
[0040]
[0041] Table 3 Parameters of expanded polyethylene beads and properties of molded parts of Examples 1-5 and Comparative Examples 1-9
[0042]
[0043]
[0044] Example of molding preparation:
[0045] The foamed polyethylene particles prepared in Examples 1-5 were filled into a rectangular mold (450 mm long, 350 mm wide, and 60 mm thick) after being subjected to 0.5 MPa air pressure for 8 h, and then steam molded.
[0046] Among them, the minimum molding pressure is the minimum steam sintering pressure required for the proportion of particles with destroyed cells on the broken surface of the foamed polyethylene particle molding to be more than 95%.
[0047] Permanent compression deformation: The molded parts are cut into samples with a length of 100mm, a width of 100mm, and a thickness of 50mm; in a flat compression mold, the sample is compressed by 25% in the thickness direction and maintained for 22 hours; then the compression mold is opened, and the sample is allowed to recover freely for 2 hours. The average thickness of the sample is measured as L. The larger the L (37.5mm≤L≤50mm), the better the resilience of the part; the above tests are all carried out in a laboratory with a temperature of 25℃ and a humidity of 50%. The permanent compression deformation tested on this basis is [(50-L) / 50]×100%. The smaller the value, the better the resilience of the material.
[0048] Apparent quality of parts: Indicates that there are many pits or gaps on the surface of the workpiece; Indicates a small amount of pits or gaps on the surface of the workpiece; It means that there are no or very few or very small pits or gaps on the surface of the workpiece.
[0049] The products of Examples 1-5 are all within the technical requirements, showing excellent low-pressure moldability, softness, high resilience and excellent surface quality.
[0050] In comparative example 1, the skin material does not contain thermoplastic elastomer D, the energy consumption of foaming bead molding increases, and a small amount of pits appear on the surface of the molded part; the steam pressure increases during the molding process, which is not conducive to the preservation of the closed pores inside the beads, and the permanent compression deformation increases. In comparative example 2, the skin material only contains thermoplastic elastomer D, and its extremely easy heat-sealing property causes the surface of the molded part to be easily sintered, which to a certain extent prevents the steam from penetrating the inside of the part, and easily causes poor sintering inside the part, and the overall molding energy consumption increases, resulting in a small amount of pits on the surface of the part; the steam pressure increases during the molding process, which is not conducive to the preservation of the closed pores inside the beads, and the permanent compression deformation increases. In comparative example 3, the outer layer of the beads does not contain a skin material that is easy to sinter, the molding energy consumption is high, and there are a small amount of pits on the surface of the part; the steam pressure increases during the molding process, which is not conducive to the preservation of the closed pores inside the beads, and the permanent compression deformation increases. In comparative example 4, the foaming core layer does not contain thermoplastic elastomer C, which is not conducive to the molding expansion of the beads to a certain extent, the molding energy consumption increases, and the softness and resilience of the material decrease, resulting in an increase in the surface hardness and permanent compression deformation of the molded part. Compared with Example 1, comparative example 5 does not contain an auxiliary expansion agent, which is not conducive to density reduction and uniform pores during the foaming process, and the molding expansion of the foamed beads is worse, resulting in high molding energy consumption and more pits and gaps on the surface of the part; the steam pressure increases during the molding process, which is not conducive to the preservation of the closed cells inside the beads, and the permanent compression deformation increases. In comparative example 6, excessive auxiliary expansion agents are added to the material, which has a reinforcing effect on the material to a certain extent, but has an adverse effect on the resilience of the material; in addition, it causes the molding expansion performance of the foamed beads to deteriorate, the molding energy consumption increases slightly, and a small amount of gaps appear on the surface of the part. In comparative example 7, during the foaming process, without the post-foaming process at an atmosphere temperature of 80-95°C, the density of the foamed beads is difficult to reduce, and the volume of the foamed beads is uneven, resulting in more gaps and pits on the surface of the molded parts. In comparative example 8, the foamed core layer is thermoplastic elastomer C3. Compared with Example 3, its molding expansion and resilience are worse, the molding energy consumption is slightly increased, the molded parts have a small number of pits, the permanent compression deformation increases, and the surface hardness increases; in comparative example 9, the skin material is thermoplastic elastomer D3. Compared with Example 3, the molding energy consumption is increased, the molded parts have a small number of pits, and the permanent compression deformation increases.
Claims
1. A foamed polyethylene particle, characterized in that: The particles are prepared from composite particles, the composite particles include a core layer and a skin layer, the skin layer is coated on the surface of the core layer, the core layer includes at least 85-97 parts by weight of polyethylene A, 3-10 parts by weight of thermoplastic elastomer C, and 0.1-5 parts by weight of an expansion aid, and the skin layer includes at least 80-100 parts by weight of polyethylene B and 0-20 parts by weight of thermoplastic elastomer D; The expansion aid is selected from one or both of diatomaceous earth and zeolite powder, with an average particle size of 1-15 microns; The preparation method of the foamed polyethylene particles comprises: (1) mixing polyethylene A, thermoplastic elastomer C, cell nucleating agent and expansion aid in a certain proportion, and then melting and granulating the mixture in an extruder to obtain a core layer masterbatch; the heating section temperature of the extruder is 200° C.-240° C.; (2) After polyethylene B and thermoplastic elastomer D are uniformly mixed, they are melt-granulated in an extruder to obtain a skin masterbatch; the temperature of the heating section of the extruder is 200° C.-240° C.; (3) adding the core layer masterbatch and the skin layer masterbatch to the core layer extruder and the skin layer extruder of the twin-single screw co-extruder unit respectively, and after plasticization, filaments are discharged through the co-extrusion die to obtain composite particles of the skin layer covering the core layer; the temperature of the heating section of the extruder is 200° C.-240° C.; (4) Add the composite particles together with the dispersant and water into an autoclave, seal it, add CO2, stir continuously, raise the temperature of the autoclave to a foaming temperature of 115°C-133°C, adjust the pressure in the autoclave to a foaming pressure of 2.2-4.4MPa, maintain it under this temperature and pressure condition for 10-60min, release the pressure and discharge the material into a foaming pipe for foaming, the atmosphere temperature in the foaming pipe is 80-95°C, the atmosphere pressure in the foaming pipe is 0.01-0.08MPa, the time the material spends in the foaming pipe is 10-50s, and finally obtain foamed polyethylene particles with a bulk density of 15-120g / L, and the melting peak endothermic enthalpy value higher than the intrinsic melting point in the first DSC melting curve of the foamed particles is 20-50J / g.
2. The foamed polyethylene particles according to claim 1, characterized in that: The polyethylene A is a linear low-density polyethylene with a melt index of 0.1-7 g / 10min (190°C, 2.16kg) and a melting point of 115-130°C; the thermoplastic elastomer C is selected from one or more of SBS, SEBS, and SEPS, with a Shore hardness of 50-85A; the polyethylene B is a low-density polyethylene with a melt index of 4-12 g / 10min (190°C, 2.16kg) and a melting point of 95-115°C; the thermoplastic elastomer D is a heat-sealable polyolefin elastomer with a melt index of 4-12 g / 10min (230°C, 2.16kg) and a melting point of 55-85°C.
3. The foamed polyethylene particles according to claim 2, characterized in that: The polyethylene A has a melt index of 0.3-6 g / 10 min (190° C., 2.16 kg) and a melting point of 116-127° C.; the polyethylene B preferably has a melt index of 5-10 g / 10 min (190° C., 2.16 kg) and a melting point of 97-113° C.
4. The foamed polyethylene particles according to claim 1, characterized in that: The core layer further comprises a cell nucleating agent, which is selected from one or more of silicon dioxide, zinc borate, talcum powder, and calcium carbonate, with an average particle size of 10-15 microns and 0.01-0.15 parts by weight.
5. The foamed polyethylene particles according to claim 1, characterized in that: The weight percentage of the cortex in the composite particles is 3-10%; the length of the composite particles is 1.2-3.5 mm, and the unit weight is 1-5 mg.
6. The foamed polyethylene particles according to claim 5, characterized in that: The length of the composite particles is 1.5-3 mm, and the unit weight is 1.2-3 mg.
7. A molded article, characterized in that: It contains the foamed polyethylene particles according to any one of claims 1 to 6.
8. The method for preparing a molded article according to claim 7, characterized in that: The method comprises steam sintering and molding, and the specific steps are: the foamed particles are pressurized by air and then steam molded.
9. Use of the foamed polyethylene particles according to any one of claims 1 to 6 in the field of packaging.
Citation Information
Patent Citations
A low-shrinkage, high-resilience EPE bead and its preparation method
CN105037912B
Polyethylene composition, foamed bead and preparation method thereof, and foamed bead molding body
CN107312233A
Easily melted foamed polyethylene bead with strong temperature tolerance and preparation method thereof
CN109651695A
Process for producing molded body of expanded polyolefin resin particles, and molded body of expanded polyolefin resin particles