CNTs in-situ doping of lithium iron phosphate battery cathode materials

The in-situ synthesis of CNTs on the surface of lithium iron phosphate by CVD method solved the problem of poor CNT dispersion, achieved uniform dispersion of CNTs and improved conductivity, thus improving the electrochemical performance of lithium battery cathode materials.

CN118324113BActive Publication Date: 2024-11-15UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410755236.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-15
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

In the existing technology, the CNTs of lithium iron phosphate cathode materials have poor dispersion and controllability, and the dispersion and controllability of cathode materials formed by mechanical miscibility need to be further improved.

Method used

CNTs were synthesized in situ on the surface of lithium iron phosphate particles using chemical vapor deposition (CVD). By controlling the water vapor and carbon source content, uniform dispersion of CNTs was achieved, and the content of amorphous carbon was controlled to improve conductivity.

Benefits of technology

This method achieves uniform dispersion of CNTs, maintains the integrity of the three-dimensional conductive network structure, reduces battery resistance, and improves the electrochemical performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118324113B_ABST
    Figure CN118324113B_ABST
Patent Text Reader

Abstract

CNTs in-situ doped lithium iron phosphate battery positive electrode material, the preparation method thereof includes: placing lithium iron phosphate into the central working area of ​​a tube furnace; placing ferrocene in the upstream area of ​​the tube furnace, the upstream area of ​​the tube furnace and the central working area form heat insulation but keep the gas interconnected; introducing inert gas into the tube furnace, and heating the central working area of ​​the tube furnace; when the central working area of ​​the tube furnace is heated to a predetermined decomposition temperature, starting the heater coated on the quartz tube of the tube furnace to heat the ferrocene therein to a predetermined sublimation temperature; and when the central working area of ​​the tube furnace continues to be heated to the working temperature, introducing working gas into the tube furnace to CVD form CNTs on lithium iron phosphate particles. The present invention uses CVD to synthesize CNTs in-situ on the surface of lithium iron phosphate, thereby simply and controllably achieving uniform dispersion of CNTs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a positive electrode material for a lithium battery. Background Art

[0002] The electrode materials of lithium-ion batteries are crucial to battery performance. At present, commercial lithium-ion battery cathode materials include lithium iron phosphate, lithium cobalt oxide, nickel-cobalt-manganese ternary materials, etc. Among them, olivine-structured lithium iron phosphate (LiFePO 4 ) The material has the advantages of good thermal stability, long cycle life, environmental friendliness, and abundant raw material sources.

[0003] In order to increase the conductivity of lithium iron phosphate positive electrode materials, carbon nanotubes (CNTs) are usually doped therein by a miscible method, such as disclosed in CN 114843473 A, CN103236544A, CN109244421A, CN114436234B, CN114438358B, etc. However, the dispersibility and controllability of the positive electrode materials formed by this mechanical miscible method need to be further improved. Summary of the invention

[0004] The purpose of the present invention is to provide an improved method for preparing a positive electrode material for a lithium battery.

[0005] According to one aspect of the present invention, there is provided a method for preparing a positive electrode material for a lithium battery, comprising:

[0006] Provide lithium iron phosphate particles;

[0007] Placing lithium iron phosphate particles into the central working area of ​​a CVD tube furnace;

[0008] Placing ferrocene in an upstream region of a CVD tube furnace, wherein the upstream region of the CVD tube furnace is thermally insulated from a central working region of the CVD tube furnace but the gases are kept in communication with each other;

[0009] Inert gas is introduced into the CVD tube furnace, and the central working area of ​​the CVD tube furnace is heated and heated;

[0010] When the central working area of ​​the CVD tube furnace is heated to a predetermined decomposition temperature, a heater coated on the quartz tube of the tube furnace is started to heat the ferrocene therein to a predetermined sublimation temperature; and

[0011] When the central working area of ​​the CVD tube furnace continues to be heated to the CVD working temperature, a working gas is introduced into the CVD tube furnace to form CNTs on the lithium iron phosphate particles by CVD.

[0012] According to the preparation method of the present invention, the average particle size of the lithium iron phosphate particles is preferably 5-15 μm.

[0013] According to the preparation method of the present invention, the predetermined decomposition temperature is preferably 590°C to 610°C, for example, about 600°C.

[0014] According to the preparation method of the present invention, the predetermined sublimation temperature is preferably 150°C to 200°C, for example, about 175°C.

[0015] According to the preparation method of the present invention, the CVD working temperature is preferably 630° C. to 650° C., for example, about 640° C.

[0016] According to the preparation method of the present invention, the mass ratio of lithium iron phosphate to ferrocene is preferably 1.2-2, for example, about 1.6.

[0017] According to the preparation method of the present invention, argon gas with a flow rate of 800-1200 sccm is preferably continuously introduced into the CVD tube furnace before the central working area of ​​the CVD tube furnace is heated to the CVD working temperature.

[0018] The preparation method according to the present invention further comprises: after the ferrocene in the heater is sublimated or when the central working area of ​​the CVD tube furnace is heated to the CVD working temperature, the heater is turned off. The heater can be in the form of an electric heating belt.

[0019] According to the preparation method of the present invention, the working gas is composed of ethylene, hydrogen, water vapor and argon, for example: 80~120 sccm of ethylene; 1800~2200 sccm of hydrogen; 150~250 sccm of argon carrying water vapor (the content of water vapor is about 1500~2500 ppm); and 250~350 sccm of high-purity argon.

[0020] According to the preparation method of the present invention, the heating temperature rise rate of the central working area of ​​the CVD tube furnace can be about 10°C / min before reaching the decomposition temperature, and can be adjusted to about 2°C / min until the CVD working temperature after reaching the decomposition temperature. In addition, the CVD time can be about 30 minutes. After the CVD is completed, other gases can be stopped and only argon can be kept, and then the CVD tube furnace can be cooled to room temperature at a rate of about 10°C / min.

[0021] According to another aspect of the present invention, a positive electrode material for a lithium battery is also provided, which is prepared according to the above method.

[0022] The present invention utilizes chemical vapor deposition (CVD) to in-situ synthesize CNTs on the surface of lithium iron phosphate, thereby solving the problem of poor dispersibility of CNTs and achieving uniform dispersion of CNTs.

[0023] In addition, the present invention can also control the water vapor and / or carbon source (C2 H 4 ) content, thereby controlling the content of amorphous carbon (for example, 2500ppm of water vapor can basically eliminate the presence of amorphous carbon) and the content of CNTs, thereby further improving the bonding between CNTs and lithium iron phosphate and the conductive properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic structural diagram of an embodiment of a chemical vapor deposition device used according to the present invention is shown;

[0025] Figure 2 The following is a scanning electron microscope photograph of the positive electrode material prepared according to an embodiment of the present invention. DETAILED DESCRIPTION

[0026] The present invention will be described in detail below with reference to the accompanying drawings.

[0027] Figure 1 FIG. 1 is a schematic diagram showing a structure of an embodiment of a chemical vapor deposition device used in the present invention. Figure 1 As shown, the device generally includes a tubular furnace 4, an external heating device 1, an air inlet manifold 5, and an air outlet pipe 3.

[0028] The tube furnace 4 is a quartz tube furnace for performing chemical vapor deposition, arranged horizontally, and its left and right ends are sealed by flanges. The external heating device 1 is arranged on the outside of the tube furnace 4 around the central working area of ​​the tube furnace 4. An insulating plug 42 is arranged between the upstream area (left side of the figure) inside the tube furnace 4 and the central working area. An air gap 43 is left between the insulating plug 42 and the inner wall of the tube furnace 4 and / or the insulating plug 42 itself is provided with a vent (not specifically shown in the figure) to enable the upstream area inside the tube furnace 4 to form a gas connection with the central working area. A heater 41 is also arranged in the upstream area inside the tube furnace 4, which and the external heating device 1 both adopt a controllable electric heating method. The heater 41 can, for example, be in the form of an electric heating belt to heat the catalyst substance ferrocene coated therein and enable the corresponding sublimation gas to escape freely from it. A quartz boat 44 in the form of a shallow tray (5×10 cm) is arranged in the central working area inside the tube furnace 4 to lay the lithium iron phosphate object to be deposited therein.

[0029] The gas inlet main pipe 5 enters the interior of the tubular furnace 4 from the left end thereof and is connected to each gas source 7 through corresponding valves 6 .

[0030] The gas outlet pipe 3 enters the interior of the tubular furnace 4 from the right end and is equipped with an exhaust valve 2.

[0031] Embodiment: A quartz boat 44 containing 0.32g of lithium iron phosphate is placed in the central working area inside the tube furnace 4, and a 0.2g ferrocene bag is placed in the heater 41. After the two ends of the tube furnace 4 are sealed, the corresponding valve 6 is opened, and argon gas is passed through the air intake manifold 5 for 5 minutes in advance to exhaust the air inside the quartz tube furnace 4, with a flow rate of 1000sccm. The external heating device 1 is started, and the heating rate of the tube furnace 4 is controlled to be 10℃ / min. When the tube furnace is heated to 600℃, the heating rate is adjusted to 2℃ / min; the heater 41 is started to start heating, and the heating temperature is set to 175℃. 1000sccm of argon gas is kept flowing throughout the entire heating stage. When the temperature inside the tube furnace 4 rises to 640℃, the heater 41 is turned off, the corresponding valve 6 is opened, and the working gas is passed through the air intake manifold 5, and CNTs are synthesized in situ by CVD on the lithium iron phosphate particles. The working gas composition is: 100sccm ethylene, 2000sccm hydrogen, 200sccm argon with water vapor (the volume ratio of water vapor to argon is 1:10) and 300sccm high-purity argon. The CVD in-situ synthesis time is set to 30min, during which the temperature of the tube furnace is kept at 640℃. After the CVD in-situ synthesis is completed, ethylene and hydrogen are turned off, and the tube furnace 4 is cooled to room temperature at 10℃ / min. Finally, the argon is turned off and the sample is taken out. The scanning electron microscope image is as follows Figure 2 All tail gas or exhaust gas in the process is discharged from the outlet pipe 3 and can be discharged into the atmosphere after proper treatment.

[0032] The scanning electron microscope photo of the prepared positive electrode material is shown in Figure 2 .from Figure 2 It can be seen that CNTs are evenly distributed on the surface of the lithium iron phosphate particle matrix.

[0033] Comparative Example: The lithium iron phosphate / CNTs positive electrode material was prepared by a traditional mechanical mixing method.

[0034] 15.08 g FePO 4 , 3.69 g Li 2 CO 3 , 2.36g glucose, 0.079g acidified CNTs, and 150mL deionized water were added to a sand mill, and the mixture was ball-milled at 2500 r / min for 6 h to obtain a uniformly dispersed liquid slurry. The obtained liquid slurry was dried while stirring on a magnetic stirrer to obtain an LFP / CNTs precursor. The precursor powder was placed in a quartz sintered boat, heated to 700 °C in a tube furnace at a heating rate, and kept at this temperature for 8 h. After it was naturally cooled to room temperature, a composite positive electrode material of carbon nanotubes coated with LFPCNTs was obtained.

[0035] The performance test results of the positive electrode material prepared according to the embodiment of the present invention and the positive electrode material prepared according to the comparative example are shown in Table 1.

[0036] The preparation method of the present invention is completely different from the traditional mechanical miscibility method. The present invention adopts the CVD process, by thermally separating the CVD working area and the upstream area inside the tube furnace and keeping the gas interconnected, so that the catalyst ferrocene can be simply and controllably introduced into the CVD working area in a gas phase, thereby perfectly achieving uniform synthesis of CNTs. Specifically, the CVD working principle of the present invention can be briefly described as follows.

[0037] Ferrocene can be significantly sublimated at about 100°C, and the decomposition temperature of ferrocene is 470°C. Therefore, after the ferrocene gas sublimated at a predetermined sublimation temperature (e.g., 175°C) enters the tubular furnace 4, it will immediately decompose into cyclopentadiene molecules and iron atoms at a predetermined decomposition temperature (600°C). The iron atoms are then uniformly deposited on the surface of lithium iron phosphate and aggregated to form catalytic iron nanoparticles (as a CVD synthesis catalyst for CNTs). After reaching the CVD working temperature, the working gas is introduced to synthesize CNTs in situ on the lithium iron phosphate particles by CVD under the catalytic action of the iron nanoparticles.

[0038] In summary, the present invention utilizes chemical vapor deposition (CVD) to synthesize CNTs in situ on the surface of lithium iron phosphate. On the one hand, the CNTs are dispersed more evenly. The in-situ synthesis ensures the uniform dispersion of CNTs. At the same time, it also avoids the structural damage of CNTs by the traditional ball milling process, reduces the three-dimensional conductive network structure characteristics of CNTs, and thus destroys the high-speed electron transmission path. After the in-situ synthesized CNTs are doped with this process, ball milling is not required, and the three-dimensional network structure of CNTs and the structural integrity of CNTs can be retained, effectively reducing the resistance of the battery and improving the electrochemical performance of the material. On the other hand, the preparation process of the present invention is easier to control, and the content of CNTs and amorphous carbon can be effectively controlled by controlling the amount of catalyst, carbon source and water vapor content, thereby improving the performance of the composite electrode.

Claims

1. A method for preparing a positive electrode material for a lithium battery, comprising: Provide lithium iron phosphate particles; Placing lithium iron phosphate particles into the central working area of ​​a CVD tube furnace; Placing ferrocene in an upstream region of a quartz tube of a CVD tube furnace, wherein the upstream region of the CVD tube furnace is thermally insulated from a central working region of the CVD tube furnace but the gases are kept in communication with each other; Inert gas is introduced into the CVD tube furnace, and the central working area of ​​the CVD tube furnace is heated and heated; When the central working area of ​​the CVD tube furnace is heated to a predetermined decomposition temperature, a heater coated on the quartz tube of the tube furnace is started to heat the ferrocene therein to a predetermined sublimation temperature, wherein the predetermined decomposition temperature is 590°C to 610°C, and the predetermined sublimation temperature is 150°C to 200°C; When the central working area of ​​the CVD tube furnace continues to be heated to a CVD working temperature, a working gas is introduced into the CVD tube furnace to form CNTs on the lithium iron phosphate particles by CVD, wherein the CVD working temperature is 630° C. to 650° C.; and After the sublimation of ferrocene in the heater is completed or when the central working area of ​​the CVD tube furnace is heated to the CVD working temperature, the heater is turned off.

2. The preparation method according to claim 1, wherein the average particle size of the lithium iron phosphate particles is 5 to 15 μm.

3. The preparation method according to claim 1, wherein the mass ratio of lithium iron phosphate to ferrocene is 1.2 to 2.

4. The preparation method according to claim 1, wherein argon gas with a flow rate of 800-1200 sccm is continuously introduced into the CVD tube furnace before the central working area of ​​the CVD tube furnace is heated to the CVD working temperature.

5. The preparation method according to claim 1, wherein the working gas consists of ethylene, hydrogen, water vapor and argon.

6. A lithium battery positive electrode material prepared by the method according to any one of claims 1-5.