Preparation method and application method of asphalt pavement toughening agent with oil storage and slow release function

Through the shape-selective adsorption and skeleton-sustaining and slow-release function of silicon-aluminum molecular sieve, a toughener with oil storage and slow-release function was developed, which solved the problem of reducing bond strength caused by aging of asphalt pavements, extended the life of asphalt pavements and Reduces maintenance costs and significantly improves its durability and road performance.

CN118325351BActive Publication Date: 2024-12-06SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410459569.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-12-06
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

Asphalt pavement ages after long-term exposure to environmental factors, resulting in reduced bond strength and cracks and pits, shortening its service life, and affecting its durability and road performance.

Method used

Using the shape-selective adsorption and skeleton-sustaining and slow-release functions of silicon-aluminum molecular sieve, we develop asphalt pavement toughening agent with oil storage and slow-release function. Through desorption and desorption and channel activation treatment, we prepare asphalt mixture with toughening properties and fill it with asphalt. Pavement to solve the problem of oil lean aging.

Benefits of technology

It significantly improves the service toughness and life of asphalt pavement, delays the major and medium-sized repair years of highways, reduces the cost of road maintenance and maintenance, and improves the durability and road performance of asphalt pavement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118325351B_ABST
    Figure CN118325351B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method and application method of an asphalt pavement toughening agent with an oil storage and slow-release function. The preparation method comprises the following steps: S1: desorption and desorption treatment; S2: molecular sieve pore activation treatment; S3: obtaining a road toughening agent after absorbing oil, and the key materials used mainly include mesoporous molecular sieves, molecular sieve pore activation hydrolyzate and surfactants. The preparation method of the asphalt pavement toughening agent provided by the present invention takes the adsorption and mass transfer behavior of porous media as the theoretical basis, develops an asphalt pavement toughening agent with an oil storage and slow-release function, realizes the shape-selective adsorption of light components in asphalt, and has a simple preparation and production process and low cost of basic raw materials; by replacing mineral powder with a pavement toughening agent for filling asphalt pavement, the oil content in the asphalt pavement is autonomously regulated, and the problem of oil-poor aging of asphalt pavement is solved from the source, the major and medium repair period of highways is delayed, the road maintenance and repair costs are reduced, and the service performance and life of asphalt pavement are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of road surface materials, and in particular to a preparation method and an application method of an asphalt road surface toughening agent with oil storage and slow-release function. Background Art

[0002] As the national transportation demand continues to increase, the traffic volume continues to increase, and the proportion of multi-axle, high wheel pressure, and heavy axle load traffic is increasing. In addition, extreme environmental climates occur frequently, and early damage such as cracks, rutting, and water damage is more prominent, which puts higher requirements on road materials. Among them, asphalt pavement has the advantages of smooth surface, no joints, comfortable driving, low vibration, low noise, wear resistance, no dust and easy cleaning, and short construction period, and is widely used in high-grade highway paving construction. However, asphalt pavement is a high-molecular organic material. After being coupled with environmental factors such as temperature, oxygen, water vapor, and ultraviolet rays for a long time, a series of complex chemical reactions will occur, including oxidation, volatilization and absorption of light components, polymerization, agglomeration, and cracking of modifiers, causing changes in the internal structure and properties of asphalt, which is specifically manifested as a decrease in the penetration and ductility of asphalt, and an increase in viscosity and softening point. The deterioration of these physical indicators is called asphalt aging.

[0003] The bonding strength between asphalt and aggregate decreases after aging, causing the asphalt mixture to become loose, and eventually cracks, potholes and other defects will appear, thus shortening the service life of the asphalt pavement. At the same time, asphalt is a complex thermosensitive rheological organic material. Under different temperatures and stresses, asphalt exhibits different linear or nonlinear viscoelastic properties. Its mechanical response is not only related to the real-time load, but also affected by the loading history, and is continuously accompanied by fatigue damage. Aging will cause asphalt to harden and aggravate fatigue damage under the repeated action of vehicle loads, which will seriously affect the road performance and durability of the asphalt pavement.

[0004] The invention proposes a preparation method and an application method of an asphalt pavement toughening agent with oil storage and slow-release function, which can improve the durability of asphalt pavement and increase the service life of asphalt pavement, significantly reduce the frequency of road maintenance and road reconstruction, and conform to the development trend of building long-life pavement with Chinese characteristics. Summary of the invention

[0005] The present invention provides a preparation method and an application method of an asphalt pavement toughening agent with an oil storage and slow-release function. The asphalt pavement toughening agent with an oil storage and slow-release function is developed based on the shape-selective adsorption and skeleton slow-release functions of silicon-aluminum molecular sieves, and is filled with asphalt pavement mineral powder to obtain a new type of long-life toughened asphalt pavement material. The asphalt pavement toughening agent can effectively improve the service toughness and life of the asphalt pavement, solve the problem of oil-poor aging of the asphalt pavement from the source, delay the major and medium repair period of highways, and reduce the cost of road maintenance and repair.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing an asphalt pavement toughening agent with oil storage and slow-release function comprises the following steps:

[0008] S1: desorption treatment, placing the molecular sieve raw material in a high-temperature vacuum drying oven for heating, desorption and desorption of the molecular sieve raw material in a high-temperature environment, removing the adsorbed water and impurities on the surface of the molecular sieve raw material and in its pores, and preparing a pure molecular sieve, i.e., a molecular sieve master plate;

[0009] The drying and desorption temperature of the molecular sieve raw material in the high-temperature vacuum drying oven is set to 270°C-300°C, and the drying and desorption treatment time is not less than 6 hours;

[0010] S2: Molecular sieve pore activation treatment, preparing a molecular sieve pore activation hydrolyzate, soaking the molecular sieve master obtained in S1 in the molecular sieve pore activation hydrolyzate at room temperature and stirring it fully, then transferring the molecular sieve master after adsorbing the activation hydrolyzate to a high-temperature drying oven for heating and activation, and performing the following steps in the activation process:

[0011] S2.1: Periodically stir the molecular sieve master in the high temperature drying oven, and the stirring cycle is set to stir once every 30 minutes;

[0012] S2.2: Take out the molecular sieve master from the high temperature drying oven after activation, and grind the molecular sieve master using a rolling ball mill;

[0013] S2.3: Grinding the activated molecular sieve master to a desired particle size standard to obtain an activated molecular sieve;

[0014] The molecular sieve pore activation hydrolyzing solution is prepared from isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropanol. The isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropanol are mixed and stirred and then hydrolyzed for 30 minutes.

[0015] The configuration mass ratio of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropyl alcohol is isopropyl tri(dioctyl pyrophosphate acyloxy) titanate: isopropyl alcohol = 2-8: 92-98;

[0016] The immersion time of the molecular sieve master in the molecular sieve channel activation hydrolyzate is set to 12 hours, and the stirring rate is not less than 500r / min;

[0017] The heating activation time of the molecular sieve master is not less than 6 hours, and the heating activation temperature is set to 170°C-200°C;

[0018] The expected particle size standard of the molecular sieve master after grinding is less than 75μm;

[0019] S3: After absorbing the oil, a road toughening agent is obtained. The activated molecular sieve obtained in S2 is immersed in an oil-containing solution, and the oil-containing solution is kept at a high temperature. After the activated molecular sieve fully absorbs the oil-containing solution, it is placed in a normal temperature drying oven to drain. The oil-soaked activated molecular sieve after draining is in the form of granules with separated particles. The granular oil-soaked activated molecular sieve is the road toughening agent;

[0020] The oil-containing solution is one or a combination of two or more of asphalt, bio-oil and industrial oil; the oil content in the oil-containing solution is not less than 20%; the temperature of the oil-containing solution for soaking the activated molecular sieve is not less than 150°C, and the soaking time is not less than 24 hours.

[0021] Preferably, the molecular sieve raw material in S1 is a mesoporous molecular sieve.

[0022] Preferably, the mesoporous molecular sieve is a silicon-aluminum molecular sieve, and the specification parameters of the particle size o, silicon-aluminum ratio l and pore size d of the silicon-aluminum molecular sieve are as follows:

[0023] Particle size o<100μm;

[0024] Silicon-aluminum ratio l≥10;

[0025] 2nm≤pore size d≤50nm.

[0026] A method for applying a road toughening agent in an asphalt pavement comprises the following steps:

[0027] S1: mixing and stirring a road toughening agent and a surfactant at room temperature, wherein the surfactant used is set to be a water-based polyamide thixotropic agent, and the amount of the water-based polyamide thixotropic agent is 0.5%-2% of the road toughening agent, to obtain a toughened filler;

[0028] S2: The toughened filler obtained in S1 is mixed with asphalt and stirred, the stirring time is set to 30 minutes, and the stirring rate is not less than 500 r / min to obtain toughened asphalt mortar;

[0029] S3: The toughened asphalt mortar obtained in S2 is mixed with aggregates according to the optimal asphalt-stone ratio, and the temperature is set to 150-180°C during the mixing process, the stirring rate is not less than 300r / min, and the stirring time is not less than 5min, to obtain an asphalt mixture with toughening performance;

[0030] S4: The asphalt mixture obtained in S3 is laid and used in asphalt pavement construction.

[0031] Beneficial effects of the present invention:

[0032] 1. The preparation method of the asphalt pavement toughening agent provided by the present invention is based on the adsorption and mass transfer behavior of porous media, and develops an asphalt pavement toughening agent with oil storage and slow release function, so as to achieve shape-selective adsorption of light components in asphalt. The preparation and production process is simple, and the cost of basic raw materials is low. While reducing the production cost, the quality of the toughening agent is significantly improved;

[0033] 2. When the asphalt pavement toughening agent provided by the present invention is used, the pavement toughening agent is used to replace mineral powder for filling the asphalt pavement, thereby realizing autonomous regulation of the oil content in the asphalt pavement, solving the problem of oil-poor aging of the asphalt pavement from the source, delaying the major and medium repair years of highways, reducing road maintenance and repair costs, and improving the service performance and life of the asphalt pavement. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0035] Figure 1 A flow chart of the preparation method and application method of an asphalt pavement toughening agent with oil storage and slow-release function;

[0036] Figure 2 A CT scan of an asphalt pavement toughening agent prepared by the preparation method of the pavement toughening agent provided by the present invention;

[0037] Figure 3 The complex shear modulus display diagram of Examples 2-5 of the present invention;

[0038] Figure 4 The complex shear modulus display diagram of Comparative Example 1 of the present invention;

[0039] Figure 5 The creep recovery rate and irrecoverable compliance of Examples 2-5 of the present invention and Comparative Example 1 are displayed. DETAILED DESCRIPTION

[0040] In conjunction with the drawings in the embodiments of the present invention, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] like Figure 1 As shown, the preparation method of the asphalt pavement toughening agent with oil storage and slow release function comprises the following steps:

[0042] S1: desorption treatment, placing the molecular sieve raw material in a high-temperature vacuum drying oven for heating, desorption and desorption of the molecular sieve raw material in a high-temperature environment, removing the adsorbed water and impurities on the surface of the molecular sieve raw material and in its pores, and preparing a pure molecular sieve, i.e., a molecular sieve master plate;

[0043] The drying and desorption temperature of the molecular sieve raw material in the high-temperature vacuum drying oven is set to 270°C-300°C, and the drying and desorption treatment time is not less than 6 hours;

[0044] Preferably, the drying and desorption temperature of the molecular sieve raw material is 280° C. and the time is 8 h;

[0045] S2: Molecular sieve pore activation treatment, preparing a molecular sieve pore activation hydrolyzate, soaking the molecular sieve master obtained in S1 in the molecular sieve pore activation hydrolyzate at room temperature and stirring it fully, then transferring the molecular sieve master after adsorbing the activation hydrolyzate to a high-temperature drying oven for heating and activation, and performing the following steps in the activation process:

[0046] S2.1: Periodically stir the molecular sieve master in the high-temperature drying oven, and set the stirring cycle to stir once every 30 minutes to prevent the molecular sieve master from solidifying and hardening;

[0047] S2.2: Take out the molecular sieve master from the high temperature drying oven after activation, and grind the molecular sieve master using a rolling ball mill;

[0048] S2.3: Grinding the activated molecular sieve master to a desired particle size standard to obtain an activated molecular sieve;

[0049] The molecular sieve pore activation hydrolyzing solution is prepared from isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropanol. The isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropanol are mixed and stirred and then hydrolyzed for 30 minutes.

[0050] The configuration mass ratio of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropyl alcohol is isopropyl tri(dioctyl pyrophosphate acyloxy) titanate: isopropyl alcohol = 2-8: 92-98;

[0051] Preferably, the mass ratio of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate to isopropyl alcohol is isopropyl tri(dioctyl pyrophosphate acyloxy) titanate: isopropyl alcohol = 5:95;

[0052] The immersion time of the molecular sieve master in the molecular sieve channel activation hydrolyzate is set to 12 hours, and the stirring rate is not less than 500r / min;

[0053] The heating activation time of the molecular sieve master is not less than 6 hours, and the heating activation temperature is set to 170°C-200°C;

[0054] Preferably, the heating activation time of the activated molecular sieve is 8 hours and the temperature is 180°C;

[0055] The expected particle size standard of the molecular sieve master after grinding is less than 75μm;

[0056] S3: After absorbing the oil, a road toughening agent is obtained. The activated molecular sieve obtained in S2 is immersed in an oil-containing solution, and the oil-containing solution is kept at a high temperature. After the activated molecular sieve fully absorbs the oil-containing solution, it is placed in a normal temperature drying oven to drain. The oil-soaked activated molecular sieve after draining is in the form of granules with separated particles. The granular oil-soaked activated molecular sieve is the road toughening agent;

[0057] The oil-containing solution is set to be one or a combination of two or more of asphalt, bio-oil and industrial oil;

[0058] As a preferred embodiment, the oil-containing solution is 90# asphalt; the oil immersion temperature of the activated molecular sieve is 180°C;

[0059] The oil content in the oil-containing solution is not less than 20%; the temperature of the oil-containing solution for soaking the activated molecular sieve is not less than 150°C, and the soaking time is not less than 24h;

[0060] The molecular sieve raw material in S1 is a mesoporous molecular sieve;

[0061] The mesoporous molecular sieve is set as a silicon-aluminum molecular sieve, and the specification parameters of the particle size o, silicon-aluminum ratio l and pore size d of the silicon-aluminum molecular sieve are as follows:

[0062] Particle size o<100μm;

[0063] Silicon-aluminum ratio l≥10;

[0064] 2nm≤pore size d≤50nm.

[0065] Preferably, the silicon-aluminum molecular sieve uses 13X silicon-aluminum molecular sieve, which has a particle size o of 10 μm, a silicon-aluminum ratio l of 16, and an average pore size d of 13 nm.

[0066] A method for applying a road toughening agent in an asphalt pavement comprises the following steps:

[0067] S1: mixing and stirring a road toughening agent and a surfactant at room temperature, wherein the surfactant used is set to be a water-based polyamide thixotropic agent, and the amount of the water-based polyamide thixotropic agent is 0.5%-2% of the road toughening agent, to obtain a toughened filler;

[0068] Preferably, the amount of waterborne polyamide thixotropic agent is 1.3% of the road toughening agent;

[0069] S2: The toughened filler obtained in S1 is mixed with asphalt and stirred, the stirring time is set to 30 minutes, and the stirring rate is not less than 500 r / min to obtain toughened asphalt mortar;

[0070] Preferably, the mixing rate of the toughening filler and the asphalt is 600 r / min;

[0071] S3: The toughened asphalt mortar obtained in S2 is mixed with aggregates according to the optimal asphalt-stone ratio, and the temperature is set to 150-180°C during the mixing process, the stirring rate is not less than 300r / min, and the stirring time is not less than 5min, to obtain an asphalt mixture with toughening performance;

[0072] Preferably, the temperature during the mixing process is controlled at 170°C, the stirring rate is 300r / min, and the stirring time is 5min;

[0073] S4: The asphalt mixture obtained in S3 is laid and used in asphalt pavement construction.

[0074] According to the above content, multiple examples and comparative examples are carried out to compare and analyze the advantages and feasibility of preparing asphalt pavement toughening agent by this method; Example

[0075] The preparation method of the asphalt pavement toughening agent specifically comprises the following steps:

[0076] (1) placing the 13X silica-alumina molecular sieve in a high-temperature vacuum drying oven at 280° C. for 8 h to obtain a pure molecular sieve master;

[0077] (2) mixing isopropyl tri(dioctyl pyrophosphate) titanate and isopropanol and stirring them for hydrolysis for 30 minutes to prepare a molecular sieve pore activation hydrolyzate, wherein the mass ratio of isopropyl tri(dioctyl pyrophosphate) titanate to isopropanol is 5:95;

[0078] (3) After immersing the 13X silicon-alumina molecular sieve in the activated hydrolyzate and stirring for 12 hours, the sieve is placed in a high-temperature drying oven for heating and activation. The heating and activation time is 8 hours at a temperature of 180° C. To prevent solidification and hardening, the sieve is stirred every 30 minutes during the activation period. After 6 hours of activation, the sieve is ground with a rolling ball mill to obtain an activated molecular sieve.

[0079] (4) Soaking the activated molecular sieve in 90# asphalt melted at 180°C for 24 hours, and after being fully absorbed, placing it in a room temperature drying oven to drain and granulate, thereby obtaining a road toughening agent;

[0080] (5) The road toughening agent and the water-based polyamide thixotropic agent are mixed and stirred at room temperature for 30 minutes at a stirring rate of 600 r / min. The amount of the water-based polyamide thixotropic agent is 1.3% of the road toughening agent to obtain an asphalt pavement toughening filler. Example

[0081] A method for applying a road toughening agent in asphalt mortar specifically comprises the following steps:

[0082] (1) Weigh 100 g of asphalt, 25 g of toughening filler and 75 g of limestone powder;

[0083] (2) mixing the toughening filler and the limestone powder and stirring them uniformly, wherein the stirring time is 10 minutes and the stirring speed is 50 rad / min;

[0084] (3) The filler and asphalt are stirred to obtain asphalt mortar at a stirring temperature of 170° C., a stirring rate of 300 r / min, and a stirring time of 5 min. Example

[0085] A method for applying a road toughening agent in asphalt mortar specifically comprises the following steps:

[0086] (1) Weigh 100 g of asphalt, 50 g of toughening filler and 50 g of limestone powder;

[0087] (2) mixing the toughening filler and the limestone powder and stirring them uniformly, wherein the stirring time is 10 minutes and the stirring speed is 50 rad / min;

[0088] (3) The filler and asphalt are stirred to obtain asphalt mortar at a stirring temperature of 170° C., a stirring rate of 300 r / min, and a stirring time of 5 min. Example

[0089] A method for applying a road toughening agent in asphalt mortar specifically comprises the following steps:

[0090] (1) Weigh 100 g of asphalt, 75 g of toughening filler and 25 g of limestone powder;

[0091] (2) mixing the toughening filler and the limestone powder and stirring them uniformly, wherein the stirring time is 10 min and the stirring speed is 50 rad / min;

[0092] (3) The filler and asphalt are stirred to obtain asphalt mortar at a stirring temperature of 170° C., a stirring rate of 300 r / min, and a stirring time of 5 min. Example

[0093] A method for applying a road toughening agent in asphalt mortar specifically comprises the following steps:

[0094] (1) Weigh 100 g of asphalt and 100 g of toughening filler;

[0095] (2) The toughening filler and asphalt are stirred to obtain asphalt mortar at a stirring temperature of 170°C, a stirring rate of 300 r / min, and a stirring time of 5 min. Example

[0096] A method for applying a road toughening agent in an asphalt pavement comprises the following steps:

[0097] (1) Weigh 100 g of asphalt and 100 g of toughening filler;

[0098] (2) mixing the toughening filler and asphalt to obtain asphalt mortar at a stirring temperature of 170° C., a stirring rate of 300 r / min, and a stirring time of 5 min;

[0099] (3) The toughened asphalt mortar was mixed with 2000 g of stone at a stirring temperature of 170°C, a stirring rate of 300 r / min, and a stirring time of 5 min to obtain an asphalt mixture with toughening properties.

[0100] Comparative Example 1

[0101] A preparation method of conventional asphalt mortar specifically comprises the following steps:

[0102] (1) Weigh 100 g of asphalt and 100 g of limestone powder;

[0103] (2) The limestone powder and asphalt are stirred to obtain asphalt mortar at a stirring temperature of 170° C., a stirring rate of 300 r / min, and a stirring time of 5 min.

[0104] Comparative Example 2

[0105] A preparation method for a conventional asphalt pavement comprises the following steps:

[0106] (1) Weigh 100 g of asphalt and 100 g of limestone powder;

[0107] (2) mixing limestone powder and asphalt to obtain asphalt mortar, with the stirring temperature being 170° C., the stirring speed being 300 r / min, and the stirring time being 5 min;

[0108] (3) The asphalt mortar was mixed with 2000 g of stone at a stirring temperature of 170°C, a stirring rate of 300 r / min, and a stirring time of 5 min to obtain a conventional asphalt mixture.

[0109] In the above Example 1, the molecular sieve used is 13X silicon aluminum molecular sieve produced by Guangzhou Xinci Environmental Protection Materials Co., Ltd., with a particle size o of 10 μm, a silicon aluminum ratio l of 16, and an average pore size d of 13 nm. The light component content in the prepared asphalt pavement toughening agent is 37.8%, and the CT scan is as follows: Figure 2 shown.

[0110] The asphalt mortar materials prepared in the above-mentioned Examples 2-5 and Comparative Example 1 were subjected to performance testing. After high-temperature ultraviolet and low-temperature immersion treatments were performed on Examples 2-5 and Comparative Example 1 to simulate road aging, shear rheology tests were performed. The results are as follows: Figure 3 and Figure 4 shown.

[0111] Depend on Figure 3 and Figure 4 It can be seen that at 46°C, the complex shear modulus of Examples 2-5 and Comparative Example 1 is 100% toughened asphalt mortar> 75% toughened asphalt mortar> 50% toughened asphalt mortar> 25% toughened asphalt mortar> mineral powder asphalt mortar; among them, the highest complex shear modulus of the asphalt mortar using 100% toughening filler is 33.54 kPa, which is 28.05% higher than that of the mineral powder asphalt mortar; with the increase in the amount of toughening filler used, the complex shear modulus of the asphalt mortar increases significantly, and the toughening filler improves the elastic response of the asphalt mortar when resisting permanent deformation, increases the proportion of the elastic component of the asphalt mortar, and significantly improves the toughness of the asphalt;

[0112] The creep recovery rate and irrecoverable compliance of Examples 2-5 and Comparative Example 1 at 64°C were obtained by MSCR test, as shown in Figure 5 shown.

[0113] Depend on Figure 5 It can be seen that at the stress level of 0.1KPa, the creep recovery rate of asphalt mortar after adding toughening filler is greater than that of mineral powder asphalt mortar. The R values ​​of 25% toughening agent, 50% toughening agent, 75% toughening agent and 100% toughening agent are increased by 52.43%, 75.77%, 223.04% and 426.88% respectively compared with mineral powder asphalt mortar; at the stress level of 3.2KPa, its R value has the same change trend as that at the stress level of 0.1KPa; at the stress level of 0.1KPa, mineral powder asphalt mortar has the highest J value, and 100% toughening filler has the lowest J value, which is 166.28% lower than that of mineral powder asphalt mortar;

[0114] The above test results show that the elastic deformation of mineral powder asphalt mortar is difficult to recover, and its ability to resist deformation is low. The asphalt mortar with the addition of toughening fillers can significantly reduce the J value; it also shows that the asphalt mortar with the addition of toughening fillers has better resistance to irreversible deformation and can adapt to more severe traffic loads.

[0115] The asphalt pavement materials prepared in Example 6 and Comparative Example 2 were tested for performance: after dynamic water scouring and high-temperature ultraviolet aging simulation treatment were carried out on Example 6 and Comparative Example 2, uniaxial compression test, splitting tensile test and asphalt four-component test were carried out respectively. The results are shown in Tables 1-3. The contents of the charts and the derived conclusions are as follows:

[0116] Table 1 Uniaxial compression test data of Example 6 and Comparative Example 2

[0117] Compressive strength (MPa) Compression strain Compression failure modulus (MPa) Comparative Example 2 8.669 0.0181 483.704 Example 6 10.054 0.0204 496.392

[0118] It can be seen from the data in Table 1 that after aging treatment, the compressive strength and compression failure stiffness modulus of Example 6 are improved. The compressive strength of Example 6 is increased by 15.98% compared with 8.669 MPa of Comparative Example 2, while the compression failure stiffness modulus is increased by 2.62% compared with 483.704 MPa of Comparative Example 2.

[0119] Table 2 Splitting tensile test data of Example 6 and Comparative Example 2

[0120] Splitting tensile strength (MPa) Tensile strain at failure Destruction modulus (MPa) Comparative Example 2 1.426 0.01025 263.384 Example 6 1.815 0.01016 351.243

[0121] It can be seen from the data in Table 2 that after aging treatment, the splitting tensile strength of Example 6 reaches 1.815 MPa, which is 27.33% higher than that of Comparative Example 2, and the breaking stiffness modulus reaches 351.243 MPa, which is 33.36% higher than that of Comparative Example 2.

[0122] Table 3 Four-component test data of Example 6 and Comparative Example 2

[0123] Saturation Aroma Gel Asphaltene Comparative Example 2 4.281 43.742 21.23 30.747 Example 6 9.586 57.002 13.576 19.873

[0124] It can be seen from the data in Table 3 that after aging treatment, the proportion of saturated fraction and aromatic fraction in Example 6 is 66.588%, and the proportion of saturated fraction and aromatic fraction in Comparative Example 2 is 48.023. After aging, the light component in Example 6 is increased by 38.6% compared with Comparative Example 2, and the anti-aging performance of Example 6 is significant.

[0125] In summary, the preparation method of the asphalt pavement toughening agent with oil storage and slow-release function provided by the present invention can realize the shape-selective adsorption of light components in asphalt, and the preparation and production process is simple and the cost of basic raw materials is low. When the asphalt pavement toughening agent is used, by replacing mineral powder with the pavement toughening agent for filling the asphalt pavement, the oil content in the asphalt pavement can be autonomously regulated, and the problem of oil-poor aging of the asphalt pavement can be solved from the source, delaying the major and medium repair years of highways, reducing the cost of road maintenance and repair, and improving the service performance and life of the asphalt pavement. It has the characteristics of being green, inexpensive, toughening, and extending life.

[0126] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0127] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing an asphalt pavement toughening agent with oil storage and slow-release function, characterized in that: The following steps are involved: S1: desorption treatment, placing the molecular sieve raw material in a high-temperature vacuum drying oven for heating, desorption and desorption of the molecular sieve raw material in a high-temperature environment, removing the adsorbed water and impurities on the surface of the molecular sieve raw material and in its pores, and preparing a pure molecular sieve, i.e., a molecular sieve master plate; Among them, the molecular sieve raw material is mesoporous molecular sieve; The mesoporous molecular sieve is set as a silicon-aluminum molecular sieve, and the specification parameters of the particle size (o), silicon-aluminum ratio (l) and pore size (d) of the silicon-aluminum molecular sieve are as follows: Particle size (o) < 100 μm; Silicon-aluminum ratio (l) ≥ 10; 2nm≤pore diameter (d)≤50nm; S2: Molecular sieve pore activation treatment, preparing a molecular sieve pore activation hydrolyzate, soaking the molecular sieve master obtained in S1 in the molecular sieve pore activation hydrolyzate at room temperature and stirring it fully, then transferring the molecular sieve master after adsorbing the activation hydrolyzate to a high-temperature drying oven for heating and activation, and performing the following steps in the activation process: S2.1: Periodically stir the molecular sieve master in the high temperature drying oven, and the stirring cycle is set to stir once every 30 minutes; S2.2: Take out the molecular sieve master from the high temperature drying oven after activation, and grind the molecular sieve master using a rolling ball mill; S2.3: Grinding the activated molecular sieve master to a desired particle size standard to obtain an activated molecular sieve; The molecular sieve pore activation hydrolysis solution is prepared from isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropanol, and the isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropanol are mixed and stirred and then hydrolyzed for 30 minutes; The configuration mass ratio of isopropyl tri(dioctyl pyrophosphate acyloxy) titanate and isopropyl alcohol is isopropyl tri(dioctyl pyrophosphate acyloxy) titanate: isopropyl alcohol = 2-8: 92-98; S3: After absorbing the oil, a road toughening agent is obtained. The activated molecular sieve obtained in S2 is immersed in an oil-containing solution, and the oil-containing solution is kept at a high temperature. After the activated molecular sieve fully absorbs the oil-containing solution, it is placed in a normal temperature drying oven to drain. The oil-soaked activated molecular sieve after draining is in the form of granules with separated particles. The granular oil-soaked activated molecular sieve is the road toughening agent; Wherein, the oil-containing solution is set to be one or a combination of two or more of asphalt, bio-oil and industrial oil.

2. The method for preparing the asphalt pavement toughening agent with oil storage and slow-release function according to claim 1, characterized in that: The drying and desorption temperature of the molecular sieve raw material in S1 in the high-temperature vacuum drying oven is set to 270°C-300°C, and the drying and desorption treatment time is not less than 6 hours.

3. The method for preparing the asphalt pavement toughening agent with oil storage and slow-release function according to claim 1, characterized in that: The immersion time of the molecular sieve master in the molecular sieve pore activation hydrolyzate in S2 is set to 12 h, and the stirring rate is not less than 500 r / min; The heating activation time of the molecular sieve master is not less than 6 hours, and the heating activation temperature is set to 170°C-200°C; The expected particle size standard of the molecular sieve master after grinding is less than 75 μm.

4. The method for preparing the asphalt pavement toughening agent with oil storage and slow-release function according to claim 1, characterized in that: The oil content of the oil-containing solution in S3 is not less than 20%; The temperature of the oil-containing solution for soaking the activated molecular sieve is not less than 150°C, and the soaking time is not less than 24 hours.

5. A method for using the road toughening agent prepared by the method for preparing an asphalt pavement toughening agent according to any one of claims 1 to 4 in an asphalt pavement, characterized in that: The following steps are involved: S1: mixing and stirring a road toughening agent and a surfactant at room temperature to obtain a toughening filler; S2: The toughened filler obtained in S1 is mixed with asphalt and stirred, the stirring time is set to 30 minutes, and the stirring rate is not less than 500 r / min to obtain toughened asphalt mortar; S3: The toughened asphalt mortar obtained in S2 is mixed with aggregates according to the optimal asphalt-stone ratio, and the temperature is set to 150-180°C during the mixing process, the stirring rate is not less than 300r / min, and the stirring time is not less than 5min, to obtain an asphalt mixture with toughening performance; S4: The asphalt mixture obtained in S3 is laid and used in asphalt pavement construction.