A biomass liquefied resin adhesive and preparation method thereof
Through the multi-component copolymerization of peanut shell phenol liquefied products, corn cob alkaline pulp and formaldehyde, combined with Lewis acid catalysis, the problem of poor cold pressing effect of biomass liquefied resin adhesive in plywood production was solved, and the cold pressing efficiency and gluing were improved. performance, enabling more efficient biomass material utilization and environmental protection.
Patent Information
- Application Number
- CN202410475490.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-18
AI Technical Summary
Biomass liquefied resin adhesive easily forms a semi-dry film during the plywood production process, which affects the wettability, resulting in poor cold pressing effect. The cold pressing pressure is high and the time is long, which affects production efficiency.
The biomass liquefied resin adhesive is prepared by multi-component copolymerization of peanut shell phenol liquefied products, corn cob alkaline pulp and formaldehyde. Lewis acid zinc chloride and concentrated hydrochloric acid are used as catalysts to promote the production of high ortho polymers and reduce the curing reaction. temperature, improve the curing speed and production efficiency, and avoid surface drying through the toughening, modification and moisturizing effects of corncob alkaline pulp.
It improves the cold pressing efficiency and cold pressing effect of plywood, enhances the gluing performance, improves the applicability and environmental protection of the adhesive, reduces the use of fossil-based raw materials, and increases the utilization value of biomass materials.
Smart Images

Figure CN118325539B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a biomass liquefied resin adhesive and a preparation method thereof. Background Art
[0002] Adhesives are single-component or multi-component materials that can bond the bonded materials tightly together through surface adhesion under certain conditions. They are synthetic or naturally renewable polymer materials with sufficient bonding strength after curing. They are currently widely used in the fields of medicine, paper, automobiles, aircraft, ships, and wood processing. Wood adhesives are indispensable materials for wood-based panels. The quality of the adhesives directly determines the final performance of wood-based panels. The most commonly used adhesives in the wood industry are traditional "trialdehyde glues", namely urea-formaldehyde, phenolic formaldehyde and melamine formaldehyde resin glues. These glues are based on formaldehyde and will release formaldehyde during use. Since formaldehyde is a carcinogen and has a damaging effect on the eyes and respiratory tract of the human body, it is extremely harmful to human health. Most trialdehyde resins are synthesized using non-renewable resources as raw materials. Among them, phenolic resin is a widely used adhesive in the board industry. Phenolic resin gives wood products excellent bonding strength, thermal stability, anti-delamination and moisture resistance. Phenol and other phenolic compounds can undergo polymerization with formaldehyde and other aldehyde compounds under certain conditions to generate highly water-resistant phenolic resin adhesives. However, phenol comes from fossil resources, and its price fluctuates greatly due to the reserves of fossil resources and regional political fluctuations. Therefore, in recent years, in order to meet the current requirements of environmental protection and resource renewable, plywood prepared with biomass adhesives has been widely used.
[0003] Agricultural and forestry biomass is the most abundant natural resource on land, with the characteristics of carbon storage, renewable and recyclable. The efficient use of agricultural and forestry biomass can not only improve the utilization value of materials and delay carbon emission footprint, but also reduce the consumption of petrochemical raw materials and energy materials. Among them, catalytic liquefaction is an important technical means to achieve the conversion and utilization of agricultural and forestry biomass, and it is also one of the hot spots of extensive research around the world. The choice of liquefier determines the fundamental properties of the liquefied product; the type and dosage of the catalyst and the liquefaction process have a very important influence on the liquefaction efficiency; different biomass materials have huge differences in their basic units, degree of polymerization, and proportion, which significantly affects the liquefaction efficiency and the reaction activity of the liquefied product. However, there are two common problems with biomass liquefied resin adhesives in the plywood production process: first, a semi-dry film is easily formed on the surface of the glue layer of the coated veneer, which affects the wettability of the adhesive to the adjacent uncoated veneer, resulting in poor cold pressing effect. This phenomenon is particularly obvious in the high temperature environment of summer and autumn; second, compared with urea-formaldehyde resin adhesives and phenolic resin adhesives, the cold pressing pressure and time required for plywood slabs are large, which affects production efficiency.
[0004] The patent with authorization announcement number CN114369435A discloses a method for preparing a biomass-based adhesive and an adhesive, wherein a biomass raw material is hydrolyzed in an acidic solution and filtered to obtain a biomass hydrolyzate rich in aldehydes; then a biomass raw material rich in lignin and a lignin activation additive are added to an alkaline solution for activation to obtain activated lignin; finally, the biomass hydrolyzate and the activated lignin are reacted in an alkaline solution to obtain a biomass-based adhesive. This invention uses biomass hydrolyzate and activated lignin to replace formaldehyde and phenol respectively to prepare a biomass-based wood adhesive, which not only reduces the health hazards and cost issues caused by the use of fossil-based raw materials to produce synthetic resin adhesives, but also significantly enhances the bonding properties of the wood adhesive. However, during the production of plywood, a semi-dry film is easily formed on the surface of the adhesive layer of the glued veneer, which affects the wettability of the adhesive to the adjacent layers of uncoated veneer, resulting in poor cold pressing effects. Therefore, the cold pressing pressure required for the plywood blank is large and the cold pressing time is long, which affects production efficiency. Summary of the invention
[0005] The present invention aims to provide a biomass liquefied resin adhesive and a preparation method thereof. The present invention utilizes a multi-polymerization reaction of peanut shell phenol liquefaction, corn cob alkaline pulp and formaldehyde solution to prepare a biomass liquefied resin adhesive, which not only improves the cold pressing efficiency and cold pressing effect of the adhesive, but also improves the utilization value of the biomass material, and further improves the applicability and environmental protection of the adhesive.
[0006] To achieve the above object, the present invention provides a method for preparing a biomass liquefied resin adhesive, comprising:
[0007] Remove impurities from peanut shells and corn cobs respectively, dry them, and then grind them into powder;
[0008] Phenol is melted and injected into a reactor, a strong acid catalyst is added, and the mixture is stirred for 5 minutes. Peanut shell powder is added into the reactor, and the mixture is stirred fully. The mixture is reacted at 120 to 140° C. for 40 to 80 minutes, and the mixture is cooled to 70 to 90° C., and a caustic soda solution with a concentration of 30 to 40% is injected to increase the pH value to between 8.0 and 9.0. The addition of the materials is stopped, and the mixture is cooled to below 45° C. to obtain a peanut shell phenol liquefied product.
[0009] Put purified water and corncob powder into a reaction kettle, stir thoroughly, add solid caustic soda, stir until the solid caustic soda is completely dissolved, stir and react at 60-95° C. for 20-60 minutes, cool to below 40° C., and obtain corncob alkaline pulp;
[0010] Peanut shell phenol liquefact and formaldehyde solution are injected into the reactor in sequence, stirred evenly, reacted at 40-50°C for 30-50min, heated to 75-90°C, stirred and reacted for 30-40min, corn cob alkaline pulp was added, reacted at 80-85°C for 20-40min, cooled and cooled to below 35°C to obtain a novel biomass liquefied resin adhesive.
[0011] Preferably, the peanut shells are dried to a moisture content of 3-10%, and crushed to a fineness of 40-60 meshes.
[0012] Preferably, the corn cob is dried to a moisture content of 6-12%, and crushed to a fineness of 160 mesh or more.
[0013] Preferably, the strong acid catalyst is a mixture of Lewis acid zinc chloride and concentrated hydrochloric acid with a concentration of 30-34%; based on the mass of pure HCl, the mass ratio of Lewis acid zinc chloride to concentrated hydrochloric acid with a concentration of 30-34% is (5-25): (75-95).
[0014] Preferably, the mass ratio of the phenol, the strong acid catalyst and the peanut shell powder is 100:(15-25):(70-120).
[0015] Preferably, the mass ratio of the purified water, corncob powder and solid caustic soda is 100:(10-20):(20-45).
[0016] Preferably, the concentration of the formaldehyde solution is 36.8-37.5%.
[0017] Preferably, the mass ratio of the peanut shell phenol liquefied product, the formaldehyde solution, and the corn cob alkaline pulp is 100:(60-90):(30-50).
[0018] The present invention also provides a biomass liquefied resin adhesive, which is prepared by the above-mentioned preparation method.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0020] 1. The present invention uses Lewis acid zinc chloride and concentrated hydrochloric acid as catalysts, which, on the one hand, reduce the pressure of condensation reflux and tail gas treatment, and on the other hand, the Lewis acid, as a cosolvent for cellulose, can accelerate the degradation reaction of peanut shell cellulose; in the resinification stage, the divalent zinc ions of the Lewis acid play an ortho-para activation effect on the benzene ring structure, promote the generation of high ortho-position polymers, and help to reduce the curing reaction temperature of the synthetic resin; in the hot pressing stage of the glue-coated slab, the divalent zinc ions of the Lewis acid play a curing accelerator role, which helps to improve the curing speed and production efficiency.
[0021] 2. Corncobs contain 12-16% lignin, 32-37% hemicellulose and 35-42% easily degradable cellulose. The present invention firstly performs alkaline degradation on the corncobs. Under strong alkaline environmental conditions, the lyophilic phenolic hydroxyl groups are easily ionized, so that the lignin in the corncobs is dissolved to form alkaline lignin, wherein the phenolic structural units exist in the form of phenol anions. Through the induction effect, the ether bonds on the α-carbon atoms of the side chains are easily broken to form a methylene quinone structure with high reaction activity. At the same time, the cellulose and hemicellulose removed from the lignin are prone to peeling reaction and hydrolysis reaction, the glycosidic bonds are broken and more reducing end groups are generated, and the acetyl groups in the polysaccharide molecules fall off. As the temperature rises, the reaction rate is accelerated, and finally sugar acid groups are formed to obtain corncob alkaline pulp mainly composed of carboxyl sugars.
[0022] 3. The present invention adopts a multi-polymer system of peanut shell phenol liquefaction, corn cob alkaline pulp and formaldehyde to prepare a biomass liquefied resin adhesive. The active phenolic compounds of the peanut shell phenol liquefaction react with formaldehyde under alkaline conditions, and the hydroxymethylated products or the hydroxymethylated products and phenolic compounds undergo condensation dehydration to form polymers of various lengths connected by methylene or methylene ether bonds. On the other hand, corn cob alkaline pulp mainly composed of carboxyl sugar is added, and the carbon cations on the carboxyl group can attack the active sites on the phenolic compounds to undergo addition reactions and further polycondensation reactions to form longer chain polymers, further increasing the molecular weight; at the same time, hydration can occur between the carboxylic acid group and the water molecules, and by forming hydrogen bonds and ionic bonds with the water molecules, it can absorb and store moisture, and play a good moisturizing role. Corn cob alkaline pulp plays a good toughening modification and moisturizing role. On the one hand, it avoids the phenomenon that the surface of the glued veneer is easy to dry and form a film, improves the cold pressing strength and cold pressing efficiency of the plywood blank, and on the other hand, further improves the dimensional stability and aging resistance of the plywood. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 FTIR spectra of the corncob powder, corncob alkaline pulp and the reaction products thereof with peanut shell phenol liquefied product in Example 1;
[0024] Figure 2 The DSC spectra of the adhesives prepared in Example 1 and Comparative Example 4 are shown. DETAILED DESCRIPTION
[0025] The following embodiments are only used to more clearly illustrate the technical solutions of the present invention, and are not intended to limit the protection scope of the present invention.
[0026] The sources of the products used in the examples and comparative examples are shown in Table 1 below:
[0027] Table 1 Sources of products used in Examples and Comparative Examples
[0028]
[0029] Example 1
[0030] A method for preparing a biomass liquefied resin adhesive comprises the following steps:
[0031] (1) Remove impurities from peanut shells and corn cobs, dry them, and then grind them into powder.
[0032] (2) 1000 g of phenol is melted and injected into a reactor. During the stirring process, 10 g of zinc chloride and 550 g of hydrochloric acid with a concentration of 31% are sequentially injected and stirred for 5 minutes. 800 g of peanut shell powder (water content 8%, fineness 40 mesh) is added into the reactor. After the reactor is closed, it is rapidly stirred for 20 minutes, and the temperature is rapidly raised to 135° C. in the reactor, and the reaction is stirred for 60 minutes. The temperature is rapidly lowered to 85° C. in the reactor, and a caustic soda solution with a concentration of 40% is slowly injected while the temperature is continuously lowered. When the pH value of the reaction liquid is increased to 9.0±0.2, the feeding is stopped, and the temperature is continuously lowered to below 45° C. to obtain a peanut shell phenol liquefied product.
[0033] (3) 1000 g of 30% caustic soda solution was injected into a reactor, and 150 g of corn cob powder (water content 10%, fineness 200 mesh) was added, stirred evenly, heated to 90° C., and stirred and reacted for 30 minutes to obtain corn cob alkaline pulp.
[0034] (4) 500 g of peanut shell phenol liquefact, 200 g of corn cob alkaline pulp, and 400 g of formaldehyde solution (concentration of 37.5%) were injected into the reactor in sequence, stirred evenly, heated to 45±2° C., and stirred for reaction for 40 min; then quickly heated to 85° C., stirred for reaction for 40 min, and cooled to below 35° C. to obtain a novel biomass liquefied resin adhesive I.
[0035] Figure 1 FTIR spectra of the corncob powder, corncob alkaline pulp and their reaction products with peanut shell phenol liquefact in Example 1. Figure 1 It is shown that corncob alkaline pulp is at 3230cm -1 、1637cm -1 、1387cm -1 The absorption peaks at 1300-1600cm-1 are mainly the absorption vibration peaks of basic hydroxyl, lignin aromatic ring skeleton, carbonyl, carbon-hydrogen bond, etc., indicating that under strong alkalinity, the alkaline lignin is dissolved, the ether bond on the α-carbon atom of the side chain is broken, and a methylene quinone structure with high reaction activity is formed; in addition, at 1300-1600cm-1 -1 The characteristic peaks of cellulose and hemicellulose weakened, indicating that some degradation of cellulose and hemicellulose occurred.-1 The phenolic hydroxyl absorption vibration peak is the phenolic structure in the peanut shell liquefied product, 1444cm -1 Nearby and 700-800cm -1 The absorption peak of benzene ring is shown, indicating that corncob alkaline pulp and peanut shell phenol liquefied product have undergone cross-linking reaction.
[0036] Example 2
[0037] A method for preparing a biomass liquefied resin adhesive comprises the following steps:
[0038] (1) Remove impurities from peanut shells and corn cobs, dry them, and then grind them into powder.
[0039] (2) 1000 g of phenol is melted and injected into a reactor. During the stirring process, 24 g of zinc chloride and 700 g of hydrochloric acid with a concentration of 31% are injected in sequence, and the mixture is stirred for 5 min. 1000 g of peanut shell powder (water content 6%, fineness 60 mesh) is injected into the reactor. After the reactor is closed, the mixture is rapidly stirred for 30 min, the temperature is rapidly raised to 130° C. in the reactor, and the mixture is stirred for reaction for 70 min. The temperature is rapidly lowered to 90° C. in the reactor, the temperature is continuously lowered and a caustic soda solution with a concentration of 40% is slowly injected. When the pH value of the reaction liquid is increased to 9.0±0.2, the feeding is stopped, and the temperature is continuously lowered to below 45° C. to obtain a peanut shell phenol liquefied product.
[0040] (3) 1000 g of 17.5% caustic soda solution was injected into a reactor, and 100 g of corn cob powder (water content 8%, fineness 250 mesh) was added. The mixture was stirred evenly, and the temperature was raised to 80° C. The mixture was stirred and reacted for 50 min to obtain corn cob alkaline pulp.
[0041] (4) 500 g of peanut shell phenol liquefact, 200 g of corn cob alkaline pulp, and 350 g of formaldehyde solution (concentration of 37.5%) were injected into the reactor in sequence, stirred evenly, heated to 50±2°C, and stirred for reaction for 30 minutes; then quickly heated to 80°C, stirred for reaction for 50 minutes, and cooled to below 35°C to obtain a new biomass liquefied resin adhesive II.
[0042] Example 3
[0043] A method for preparing a biomass liquefied resin adhesive comprises the following steps:
[0044] (1) Remove impurities from peanut shells and corn cobs, dry them, and then grind them into powder.
[0045] (2) 1000 g of phenol is melted and injected into a reactor. During the stirring process, 8 g of zinc chloride and 500 g of hydrochloric acid with a concentration of 31% are injected in sequence, and the mixture is stirred for 5 min. 700 g of peanut shell powder (water content 10% and fineness 60 mesh) is put into the reactor, and the reactor is sealed and rapidly stirred for 30 min. The temperature is rapidly raised to 125° C. in the reactor, and the mixture is stirred for reaction for 80 min. The temperature is rapidly lowered to 90° C. in the reactor, and a caustic soda solution with a concentration of 30% is slowly injected while the temperature is continuously lowered. When the pH value of the reaction solution is increased to 8.5±0.2, the feeding is stopped, and the temperature is continuously lowered to below 45° C. to obtain a peanut shell phenol liquefied product.
[0046] (3) 1000 g of 40% caustic soda solution was injected into a reactor, and 150 g of corn cob powder (water content 12%, fineness 160 mesh) was added, stirred evenly, heated to 70° C., and stirred and reacted for 40 minutes to obtain corn cob alkaline pulp.
[0047] (4) 500 g of peanut shell phenol liquefact, 180 g of corn cob alkaline pulp, and 360 g of formaldehyde solution (concentration of 37.5%) were injected into the reactor in sequence, stirred evenly, heated to 50±2° C., and stirred for reaction for 30 min; then quickly heated to 83° C., stirred for reaction for 40 min, and cooled to below 35° C. to obtain a novel biomass liquefied resin adhesive III.
[0048] Comparative Example 1
[0049] A method for preparing a peanut shell phenol liquefied resin adhesive comprises the following steps:
[0050] Add 200 g of molten phenol to a reactor, heat it to 50°C, add 180 g of peanut shell powder, stir evenly, add 120 g of 31% hydrochloric acid, heat it to 130°C, react for 1 hour, cool it to below 80°C, slowly add 280 g of caustic soda solution (concentration 40%), stir and continue to cool it to 50°C, add 400 g of formaldehyde solution (concentration 37%), react for 40 minutes, then heat it to 85°C, react for 60 minutes, cool it to below 40°C, discharge the material, and make a peanut shell phenol liquefied resin adhesive.
[0051] The adhesive prepared under the above conditions is a brown viscous opaque liquid with a solid content of 43.4%, a pH value of 11.4, and a storage period of not less than 20 days.
[0052] Comparative Example 2
[0053] A method for preparing a urea-modified peanut phenol liquefied resin adhesive comprises the following steps:
[0054] Add 200 g of molten phenol to a reactor, heat to 50°C, add 180 g of peanut shell powder, stir evenly, add 120 g of 31% hydrochloric acid, heat to 130°C, react for 1 hour, cool to below 80°C, slowly add 280 g of caustic soda solution (concentration 40%), stir and continue to cool to 50°C to make peanut shell phenol liquefied product.
[0055] 300g of 37% formaldehyde by mass was put into the reactor, stirring was started and the temperature was set to 85°C, 100g of urea was added, and 30% NaOH by mass was added dropwise to adjust the pH to 8.0, and the temperature was kept at 85°C for 45min. After the heat preservation, the temperature was lowered to 50°C, 300g of peanut shell liquefied material, 15g of 10% PVA solution by mass, and 30g of water were added, and the temperature was kept at 50°C for 40min. After the heat preservation, the temperature was raised to 85-90°C for reaction for 70min, and the viscosity reached 300mPa / s, and the temperature was lowered to below 40°C and discharged to prepare a urea-modified peanut phenol liquefied resin adhesive.
[0056] The adhesive prepared under the above conditions is a brown viscous opaque liquid with a solid content of 45.1%, a pH value of 11.1, and a storage period of not less than 30 days.
[0057] Comparative Example 3
[0058] Melamine modified urea-formaldehyde resin adhesive (abbreviated as E0 glue) is provided by Jiangsu Fuqing Wood Industry Co., Ltd. The main technical indicators are as follows: pH value: 7.0-8.0, solid content: ≥52%, viscosity: 150-200mPas, free formaldehyde content: ≤0.1%, storage period: ≥20 days.
[0059] Comparative Example 4
[0060] Phenolic resin adhesive (PF glue for short) is provided by Jiangsu Fuqing Wood Industry Co., Ltd. The main technical indicators are as follows: pH value: 10.0-11.0, solid content: ≥46%, viscosity: 250-400mPas, free formaldehyde content: ≤0.1%, free phenol content ≤0.5%, storage period: ≥30 days.
[0061] Figure 2 The DSC spectra of the adhesives prepared in Example 1 and Comparative Example 4 are shown in Figure 1. A is the heat exotherm of the thermal curing reaction of the novel biomass liquefied resin adhesive I prepared in Example 1, and B is the heat exotherm of the thermal curing reaction of the PF adhesive prepared in Comparative Example 4. Figure 2 It can be seen that the curing temperature of curve A is lower and the heat of curing reaction is higher, so the bond formed by the curing reaction is stronger.
[0062] Performance Testing
[0063] (1) Weigh 500 g of each of the three biomass liquefied resin adhesives prepared in Examples 1 to 3, and 500 g of each of the peanut shell phenol liquefied resin adhesive, urea-modified peanut phenol liquefied resin adhesive, EO and PF adhesive provided in Comparative Examples 1 to 4; add 50 g of flour to each adhesive, and add 10 g of ammonium chloride as a curing agent to the melamine-modified urea-formaldehyde resin adhesive, stir well, and prepare an adhesive for plywood;
[0064] (2) Select birch veneer with a size of 600 mm × 600 mm × 1.7 mm and a moisture content of 10% as the surface and bottom panels, and select eucalyptus veneer with a size of 600 mm × 600 mm × 1.8 mm and a moisture content of 10% as the core panel;
[0065] (3) The 1st, 3rd, 5th, 7th and 9th layers of the core board are double-sided coated with glue, with a coating amount of 320g / m 2 , according to the principle of assembling adjacent veneers perpendicular to each other, an 11-layer plywood slab with a symmetrical structure is prepared;
[0066] (4) Place the assembled slab into a cold press, cold press for 30 min at a unit pressure of 1.2 MPa, take it out and place it for 2 h, and check the cold pressing effect;
[0067] (5) The cold pressed slab was loaded into a hot press and hot pressed for 20 min at a hot press plate temperature of 132±2°C (the hot pressing temperature of the slab with melamine-modified urea-formaldehyde resin adhesive was set to 105±2°C) and a unit pressure of 1.3 MPa. The pressure was then reduced to a unit pressure of 0.5 MPa and continued to be pressed for 5 min. The slab was unloaded, taken out and stacked for 24 h, and the edges were aligned vertically and horizontally, and the plywood was sanded on both sides to form a finished plywood with a thickness of 18±0.2 mm. The physical and mechanical properties of the plywood were tested in accordance with GB17657 "Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels". The relevant test data are shown in Table 2.
[0068] Table 2 Performance test results of plywood made of adhesives in the examples and comparative examples
[0069]
[0070]
[0071] The test data in Table 2 above show that: the cold pressing effect of the slabs prepared by the adhesive made by the embodiment of the present invention is significantly better than that of Comparative Example 1 (peanut shell phenol liquefied resin adhesive) and Comparative Example 2 (urea modified peanut shell liquefied resin adhesive), and it also has a greater advantage over Comparative Example 3 (E0 glue) and Comparative Example 4 (PF glue); the static bending strength and elastic modulus of the plywood are higher than the response index values of the comparative examples, in addition, its bonding strength, bonding water resistance and aging resistance are better than E0 glue and PF glue; the plywood made of E0 glue can only be used in indoor environments and cannot be used as an outdoor structural adhesive. The dimensional stability of the plywood made by the embodiment of the present invention is better than that of the comparative example E0 glue, and it also has certain advantages over PF glue, especially the thickness change rate, which is mainly attributed to the addition of corn cob alkaline pulp in the adhesive prepared by the present invention, which plays a good toughening modification and moisturizing effect, so the prepared adhesive has high water resistance and high toughness, thereby weakening the dimensional change caused by the release of internal stress caused by temperature and humidity changes.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a biomass liquefied resin adhesive, characterized in that: include: Remove impurities from peanut shells and corn cobs respectively, dry them, and then grind them into powder; Phenol is melted and injected into a reactor, a strong acid catalyst is added, and the mixture is stirred for 5 minutes. Peanut shell powder is added into the reactor, and the mixture is stirred fully. The mixture is reacted at 120 to 140° C. for 40 to 80 minutes, and the mixture is cooled to 70 to 90° C., and a caustic soda solution with a concentration of 30 to 40% is injected to increase the pH value to between 8.0 and 9.
0. The addition of the materials is stopped, and the mixture is cooled to below 45° C. to obtain a peanut shell phenol liquefied product. Put purified water and corncob powder into a reaction kettle, stir thoroughly, add solid caustic soda, stir until the solid caustic soda is completely dissolved, stir and react at 60-95° C. for 20-60 minutes, cool to below 40° C., and obtain corncob alkaline pulp; Peanut shell phenol liquefact and formaldehyde solution are injected into the reactor in sequence, stirred evenly, reacted at 40-50°C for 30-50min, heated to 75-90°C, stirred and reacted for 30-40min, corn cob alkaline pulp was added, reacted at 80-85°C for 20-40min, cooled and cooled to below 35°C to obtain a novel biomass liquefied resin adhesive.
2. The method for preparing a biomass liquefied resin adhesive according to claim 1, characterized in that: The peanut shells are dried to a moisture content of 3-10%, and crushed to a fineness of 40-60 meshes.
3. The method for preparing a biomass liquefied resin adhesive according to claim 1, characterized in that: The corn cob is dried to a moisture content of 6-12%, and crushed to a fineness of more than 160 meshes.
4. The method for preparing a biomass liquefied resin adhesive according to claim 1, characterized in that: The strong acid catalyst is a mixture of Lewis acid zinc chloride and concentrated hydrochloric acid with a concentration of 30-34%. The mass ratio of the Lewis acid zinc chloride to the concentrated hydrochloric acid with a concentration of 30-34% is (5-25): (75-95) based on the mass of pure HCI.
5. The method for preparing a biomass liquefied resin adhesive according to claim 1, characterized in that: The mass ratio of the phenol, the strong acid catalyst and the peanut shell powder is 100:(15-25):(70-120).
6. The method for preparing a biomass liquefied resin adhesive according to claim 1, characterized in that: The mass ratio of the purified water, corncob powder and solid caustic soda is 100:(10-20):(20-45).
7. The method for preparing a biomass liquefied resin adhesive according to claim 1, characterized in that: The concentration of the formaldehyde solution is 36.8-37.5%.
8. The method for preparing a biomass liquefied resin adhesive according to claim 1, characterized in that: The mass ratio of the peanut shell phenol liquefied product, the formaldehyde solution and the corncob alkaline pulp is 100: (60-90): (30-50).
9. A biomass liquefied resin adhesive, characterized in that: The preparation method is described in any one of claims 1 to 8.
Citation Information
Patent Citations
Peanut hull liquefaction and method for preparing adhesive thereof
CN101157834A
Preparation method of biomass-based adhesive and adhesive
CN114369435A