A green and low-carbon mining method for ion-type rare earth ore leaching, smelting and leaching

By mixing the leaching tail water, hydrosmelting supernatant and leaching agent to form a leaching solution, and applying step-by-step leaching and membrane concentration technology, the problems of high carbon emissions, low rare earth recovery rates and leaching problems in rare earth mines are solved. The difficult problem of tail washing water treatment has been achieved, and low carbonization and efficient recycling of rare earth mines have been achieved.

CN118326182BActive Publication Date: 2024-10-11BEIJING MINING & METALLURGICAL TECH GRP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410645819.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-11
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

The leaching process in existing rare earth mines results in high carbon emissions, low rare earth recovery rates, high leaching tailwater treatment costs, and difficulty in stable operation.

Method used

An ionic rare earth ore leaching, smelting and leaching integrated green and low-carbon mining method is used to form a leaching liquid by mixing the leaching tail water, hydrosmelting supernatant and leaching agent to perform leaching and step-by-step leaching. Membrane concentration technology recovers rare earths and leaching agents, reduces the use of carbonates, and achieves reduction in carbon emissions and efficient recovery of rare earths.

Benefits of technology

It has achieved low-carbon production processes, increased rare earth recovery rates, reduced the amount of leaching agent and leaching tail water treatment costs, simplified the process flow, and reduced the risk of acidification pollution of the water and soil environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326182B_ABST
    Figure CN118326182B_ABST
Patent Text Reader

Abstract

The present application provides a green and low-carbon mining method for leaching, smelting and leaching of ionic rare earth ores, which relates to the technical field of rare earth mining. The method comprises: mixing leaching tail water, water smelting supernatant membrane concentrate and leaching agent, and then injecting the leaching site through the injection hole for leaching, collecting the leaching mother liquor; removing aluminum from the leaching mother liquor with an aluminum removal agent to obtain an aluminum concentrate and a dealuminized liquid; reacting the dealuminized liquid with a precipitant to obtain a rare earth product and a supernatant; membrane concentrating the supernatant to obtain a concentrate and fresh water; injecting the fresh water through the injection hole into the leaching site after leaching for the first leaching, using a mixed solution of fresh water and a regulator for the second leaching, using a mineralizer solution for the third leaching, and collecting the tail water to obtain the leaching tail water. The method provided by the present application does not use carbonate to reduce carbon emissions, and the leaching tail water is used for leaching to save the amount of leaching agent and acid. The step-by-step leaching restores the mining site to the acid-base environment before leaching, reduces the risk of acidification pollution of the ore soil in the leaching site, and realizes the green and low-carbon mining of rare earth ores.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of rare earth mining technology, and in particular to a green and low-carbon mining method for ionic rare earth ores that integrates leaching, smelting and leaching. Background Art

[0002] The only process allowed for ionic rare earth ores is the in-situ leaching process, which uses ammonium sulfate or magnesium sulfate as a leaching agent. The production process of the leaching field is that the leaching agent is used to prepare the leaching solution, which is injected into the leaching field through the injection hole, and the mother liquor is collected through the liquid collection system; the production process of the hydrometallurgical workshop is that the mother liquor enters the impurity removal tank, adds ammonium bicarbonate or sodium bicarbonate, and precipitates to obtain impurity-removed slag and impurity-removed liquid, and the impurity-removed liquid is added with ammonium bicarbonate or sodium bicarbonate and stirred and precipitated to obtain rare earth products and supernatant, and the supernatant enters the liquid preparation tank. The existing rare earth mine production process leaching field mainly considers leaching and liquid collection, and the hydrometallurgical workshop mainly considers mother liquor impurity removal and precipitation to obtain rare earth products. The mine production process is a leaching-hydrometallurgical process of "leaching solution leaching-mother liquor collection-mother liquor impurity removal-rare earth precipitation-supernatant preparation of leaching solution". The mother liquor impurity removal and precipitation uses carbonate to adjust the mother liquor pH from about 4.5 to about 7.0, which generates a large amount of carbon emissions; the carbonate rare earth product produces a large amount of carbon emissions in the subsequent acid dissolution process of separation and smelting. When the supernatant is prepared for leaching, sulfuric acid needs to be added to adjust the supernatant pH from about 7.0 to about 4.8, consuming a large amount of acid. In the in-situ leaching process, when the rare earth content in the collected mother liquor is less than 100 mg / L, the mine generally stops collecting the mother liquor, and the low-concentration rare earth leaching mother liquor is not recovered, resulting in a low rare earth recovery rate in the mine.

[0003] The in-situ leaching process of ammonium salt of ionic rare earth ore requires the addition of 6-12 tons of ammonium sulfate for every ton of rare earth produced, resulting in a large amount of ammonium sulfate accumulated in the leaching field; the in-situ leaching process of magnesium ammonium salt requires the addition of 8-15 tons of magnesium sulfate for every ton of rare earth produced, resulting in a large amount of magnesium sulfate accumulated in the leaching field. After the leaching is completed, a large amount of ammonium sulfate or magnesium sulfate is accumulated in the in-situ leaching field. Forced leaching is an effective environmental protection measure to reduce the residual leaching agent. However, due to the long leaching time of the residual leaching agent, the difficulty and high cost of leaching tail water treatment, the mines are reluctant to leach.

[0004] NH4 in the initial leaching tail water of ammonium salt leaching process + Concentration of about 1200mg / L, SO4 2- Concentration of about 3500mg / L, Re 3+ Concentration is about 100mg / L; NH4 in the tail water of the later stage + Concentration of about 100mg / L, SO4 2- Concentration is about 450mg / L, Re 3+The concentration is about 15 mg / L. If the tail water of ammonium salt leaching process is treated by biological method, due to the low carbon / nitrogen ratio of ammonia nitrogen wastewater, a carbon source needs to be added, which increases the COD in the wastewater, increases the treatment cost, causes secondary pollution, and the water quality of the tail water fluctuates greatly, which has an impact on the biological method and is difficult to operate stably. In addition, the rare earth and leaching agent ammonium sulfate in the tail water are not recovered.

[0005] The initial leaching tail water Mg of magnesium salt leaching process 2+ Concentration of about 1000mg / L, SO4 2- Concentration of about 4500mg / L, Re 3+ Concentration is about 100mg / L; Mg in the tail water of the later stage 2+ Concentration is about 120mg / L, SO4 2- Concentration is about 750mg / L, Re 3+ The concentration is about 20 mg / L. In short, the tail water contains Re 3+ 、SO4 2- Mg 2+ NH4 + The tail water of leaching has the characteristics of complex water quality and large fluctuations, which makes the treatment of tail water of leaching difficult. The treatment of magnesium and sulfate in the tail water of leaching of magnesium salt leaching process, such as the treatment by calcium sulfonate method, requires the addition of a large amount of lime, produces a large amount of sludge, and the pH chemical adjustment and control is difficult and the cost is very high. In addition, the rare earth and leaching agent magnesium sulfate in the tail water of leaching are not recovered.

[0006] If the tail water from ammonium salt leaching and magnesium salt leaching is treated with reverse osmosis membrane, the water quality of the tail water will fluctuate greatly, and Al 3+ 、Re 3+ 、SO4 2- High ion concentration can easily cause membrane scaling, which will affect the membrane life. The tail water needs to be pre-treated to remove Al 3 + 、Re 3+ The treatment is to below a certain concentration, and at the same time, the membrane operation control requirements are very strict and the cost is very high.

[0007] The water quality of leaching tail water is complex and fluctuates greatly. Regardless of whether chemical, biological or membrane treatment methods are used, there are problems such as high cost and difficulty in stable operation. Leaching and leaching tail water treatment as environmental protection measures are difficult to promote in mines, and the risk of pollution of the water and soil environment by residual leaching agents in the leaching field is difficult to solve. Summary of the invention

[0008] The purpose of this application is to provide a green and low-carbon mining method for ionic rare earth ore leaching, smelting and leaching to solve the above problems.

[0009] To achieve the above objectives, this application adopts the following technical solutions:

[0010] A green and low-carbon mining method for ion-type rare earth ore leaching, smelting and leaching, comprising:

[0011] The tail water of leaching, the membrane concentrate of the supernatant of water smelting and the leaching agent are mixed to obtain the leaching solution, which is then injected into the leaching field through the injection hole for leaching, and the leaching mother liquor is collected by the liquid collection system;

[0012] The leaching mother liquor is dealuminized by using a dealuminizing agent to obtain an aluminum-enriched product and a dealuminized liquid; the dealuminized liquid is reacted with a precipitant to separate the solid and the liquid to obtain a rare earth product and a water-metallurgical supernatant; the water-metallurgical supernatant is membrane concentrated to obtain the water-metallurgical supernatant membrane concentrated liquid and water-metallurgical supernatant membrane concentrated fresh water;

[0013] The fresh water concentrated by membrane from the supernatant of the water smelting is injected into the leaching field after the leaching through the injection hole for the first leaching, and after the first leaching, a mixed solution of the fresh water concentrated by membrane from the supernatant of the water smelting and a regulator is used for the second leaching, and after the second leaching, a mineralizer solution is used for the third leaching, and the tail water of the first leaching, the second leaching and the third leaching is collected to obtain the leaching tail water;

[0014] After the third elution is completed, the injection hole is backfilled to restore vegetation;

[0015] The leaching agent is magnesium sulfate and / or ammonium sulfate; the aluminum removal agent, the precipitant and the regulator are all sodium hydroxide; and the mineralizer solution is obtained by dissolving the aluminum enrichment by sulfuric acid.

[0016] Preferably, the pH of the leaching solution is 4.8-5.0.

[0017] Preferably, the rare earth ion concentration in the leaching mother solution is not less than 100 mg / L.

[0018] Preferably, after the leaching mother solution is mixed with the aluminum removal agent, the pH of the system is 5.2-5.4.

[0019] Preferably, the pH of the system of the aluminum-removed liquid and the precipitant is 6.7-7.2.

[0020] Preferably, the membrane concentration is performed using a reverse osmosis membrane.

[0021] Preferably, the pH of the mineralizer solution is 4.2-4.5.

[0022] Preferably, the end point of the first elution is: elution to the tail water SO4 2+ Concentration less than or equal to 700 mg / L, NH4 + The concentration is less than or equal to 15mg / L.

[0023] Preferably, the end point of the second elution is: elution until the pH of the tail water is 7.5-8.0.

[0024] Preferably, the endpoint of the third elution is: elution until the pH of the tail water is 5.5-6.0.

[0025] Compared with the prior art, the beneficial effects of this application include:

[0026] The present application provides an integrated green and low-carbon mining method for leaching, smelting and leaching of ionic rare earth ores. The aluminum removal agent, precipitant and regulator used in water smelting and leaching are sodium hydroxide (caustic soda flakes). No carbonate is used in the production process. The product is a rare earth hydroxide concentrate, which avoids carbon emissions caused by the addition of carbonates. The carbon emissions in the production process are zero, thereby achieving a low-carbon production process.

[0027] The green and low-carbon mining method of in-situ integrated leaching, smelting and leaching realizes the coordination of mine leaching, water smelting and leaching, and the production process is simpler. Leaching is an integral part of the solution mining process. The leaching tail water is used to prepare the leaching solution for leaching, and the acid and leaching agent in the leaching tail water are recovered. This avoids the acid adjustment step of the existing process in which the leaching solution is prepared by using the supernatant of the mother liquor precipitation, reduces the use of sulfuric acid and leaching agent by about 30% to 40%, and reduces the risk of acidification pollution of the water and soil environment in the leaching site.

[0028] The in-situ integrated leaching, smelting and leaching green and low-carbon mining method eliminates the treatment of leaching tail water and utilizes the leaching tail water as leaching liquid. The leaching agent in the leaching tail water is utilized, which reduces the amount of leaching agent. The rare earths in the leaching tail water are recovered with the mother liquor in the leaching field, which increases the rare earth concentration in the mother liquor, increases the rare earth recovery rate of the mine by about 15%, and makes leaching easier to implement.

[0029] In-situ leaching, smelting and leaching integrated green and low-carbon mining method, the supernatant of the water smelting is concentrated by membrane to obtain membrane concentrate and fresh water, the water quality of the supernatant of the water smelting is stable, Al 3+ ,RE 3+ The ion concentration is low, the risk of membrane scaling is small and the life is long; the membrane concentrate is used as leaching liquid, and the leaching agent in the mother liquor is recycled; the supernatant membrane concentrated fresh water is used for leaching, avoiding the use of new water for leaching.

[0030] After leaching, the mine adopts step-by-step leaching, which not only washes the residual leaching agent to a level that meets environmental protection requirements, but also adjusts the acidity and alkalinity of the mine soil to the level before leaching, reducing the risk of acidification pollution of the mine soil after leaching. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0032] Figure 1 A schematic diagram of an integrated green and low-carbon mining method for ionic rare earth ore leaching, smelting and leaching provided in an embodiment. DETAILED DESCRIPTION

[0033] In order to better explain the technical solution provided by this application, before the embodiments, the technical solution is first described as a whole, as follows:

[0034] A green and low-carbon mining method for ion-type rare earth ore leaching, smelting and leaching, comprising:

[0035] The tail water of leaching, the membrane concentrate of the supernatant of water smelting and the leaching agent are mixed to obtain the leaching solution, which is then injected into the leaching field through the injection hole for leaching, and the leaching mother liquor is collected by the liquid collection system;

[0036] The leaching mother liquor is dealuminized by using a dealuminizing agent to obtain an aluminum-enriched product and a dealuminized liquid; the dealuminized liquid is reacted with a precipitant to separate the solid and the liquid to obtain a rare earth product and a water-metallurgical supernatant; the water-metallurgical supernatant is membrane concentrated to obtain the water-metallurgical supernatant membrane concentrated liquid and water-metallurgical supernatant membrane concentrated fresh water;

[0037] The fresh water concentrated by membrane from the supernatant of the water smelting is injected into the leaching field after the leaching through the injection hole for the first leaching, and after the first leaching, a mixed solution of the fresh water concentrated by membrane from the supernatant of the water smelting and a regulator is used for the second leaching, and after the second leaching, a mineralizer solution is used for the third leaching, and the tail water of the first leaching, the second leaching and the third leaching is collected to obtain the leaching tail water;

[0038] After the third elution is completed, the injection hole is backfilled to restore vegetation;

[0039] The leaching agent is magnesium sulfate and / or ammonium sulfate; the aluminum removal agent, the precipitant and the regulator are all sodium hydroxide; and the mineralizer solution is obtained by dissolving the aluminum enrichment by sulfuric acid.

[0040] In an optional embodiment, the pH of the leaching solution is 4.8-5.0.

[0041] Leaching ore is leached in an acidic environment.

[0042] Optionally, the pH of the leaching solution may be 4.8, 4.9, 5.0 or any value between 4.8 and 5.0.

[0043] In an optional embodiment, the rare earth ion concentration in the leaching mother solution is not less than 100 mg / L.

[0044] The above concentration is the optimal rare earth recovery concentration considering the cost of recovering rare earths by removing aluminum from mother liquor and precipitating.

[0045] In an optional embodiment, after the leaching mother solution is mixed with the aluminum removal agent, the pH of the system is 5.2-5.4.

[0046] The above pH is the optimal pH for aluminum ions to form aluminum hydroxide precipitation.

[0047] Optionally, after the leaching mother solution is mixed with the aluminum removal agent, the pH of the system can be 5.2, 5.3, 5.4 or any value between 5.2 and 5.4.

[0048] In an optional embodiment, the pH value of the system of the aluminum-removed liquid and the precipitant is 6.7-7.2.

[0049] The above pH is the optimal pH for rare earth ions to form rare earth hydroxide precipitates.

[0050] Optionally, the pH of the system of the aluminum-removed liquid and the precipitant can be 6.7, 6.8, 6.9, 7.0, 7.1, 7.2 or any value between 6.7 and 7.2.

[0051] In an optional embodiment, the membrane concentration is performed using a reverse osmosis membrane.

[0052] In an optional embodiment, the pH of the mineralizer solution is 4.2-4.5.

[0053] The above pH is a preferred pH of the aluminum sulfate solution.

[0054] Optionally, the pH of the mineralizer solution may be 4.2, 4.3, 4.4, 4.5 or any value between 4.2 and 4.5.

[0055] In an optional embodiment, the end point of the first elution is: elution to the tail water SO4 2+ Concentration less than or equal to 700 mg / L, NH4 + The concentration is less than or equal to 15 mg / L, meeting the emission standards.

[0056] In an optional embodiment, the endpoint of the second elution is: eluting until the pH of the tail water is 7.5-8.0.

[0057] The mineral soil is eluted to alkalinity so that aluminum hydroxide precipitation is formed in the third elution.

[0058] In an optional embodiment, the endpoint of the third elution is: eluting until the pH of the tail water is 5.5-6.0.

[0059] The soil in rare earth mines is mostly weakly acidic before leaching, which is the end point of leaching.

[0060] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0061] like Figure 1 As shown, this embodiment provides an integrated green and low-carbon mining method for ion-type rare earth ore leaching, smelting and leaching, including the following steps:

[0062] The production process of a rare earth mine is "leaching tail water leaching - leaching mother liquor hydrometallurgy - step-by-step leaching and closure". The leaching agent is ammonium sulfate, the aluminum removal agent, precipitant and regulator are sodium hydroxide, and the mineralization liquid is obtained by dissolving aluminum enrichment with sulfuric acid. There is one leaching site and one leaching site. The liquid collection system consists of a liquid collection tunnel, diversion holes, liquid collection trenches, and seepage liquid recovery wells. The recovery rate of leaching mother liquor and leaching tail water is 80%, and the leaching intensity and leaching intensity are 3000m 3 / d, mother liquor collection time is 150 days, leaching tail water collection time is 150 days, leaching time is 150 days, and the leaching liquid volume is about 450,000 m 3 , the amount of leaching water is about 450,000 m 3 The average rare earth content in the leaching mother liquor is about 350 mg / L, ammonia nitrogen is about 1200 mg / L, and aluminum is about 60 mg / L; the rare earth content in the leaching tail water is about 50 mg / L, the average ammonia nitrogen is about 300 mg / L, the sulfate is about 1200 mg / L, and the aluminum is about 40 mg / L.

[0063] The details are as follows:

[0064] (a) Leaching tailings water

[0065] The leaching solution is prepared by adding ammonium sulfate and sulfuric acid to the tail water of leaching and the supernatant liquid of water smelting, and consuming about 290t of ammonium sulfate and about 29t of sulfuric acid.

[0066] (b) Leaching mother liquor water treatment

[0067] The mother liquor enters the aluminum removal tank, sodium hydroxide is added to adjust the pH to 5.2, and the aluminum concentrate and the aluminum removal liquid are obtained by stirring and precipitation. The aluminum removal liquid enters the rare earth precipitation tank, sodium hydroxide is added to adjust the pH to 7.0, and the rare earth product (rare earth hydroxide) and supernatant are obtained by precipitation and filtration. The supernatant enters the reverse osmosis membrane for treatment to obtain membrane concentrate and fresh water. The membrane concentrate is used for leaching, and the fresh water is used for leaching. The aluminum concentrate is about 90t and the rare earth product is about 300t.

[0068] (c) Step-by-step leaching and closure

[0069] After leaching, the mine is washed with fresh water to the tail water of SO42+ Concentration not more than 700 mg / L, NH4 + The concentration is not more than 15mg / L. The second-step regulator is eluted to a pH of 7.5 for the elution tail water, and the third-step mineralization liquid is eluted to a pH of 5.5 for the elution tail water. The elution tail water is collected by the liquid collection system and used for leaching in the leaching field. The injection hole is backfilled with the abandoned soil, compacted to about 50cm from the hole mouth, and then the topsoil is backfilled in the injection hole to plant plants.

[0070] No carbonate is used in the production process, thus reducing carbon emissions. The leaching tail water is used for leaching in the leaching field, eliminating the treatment of the leaching tail water. The rare earths and leaching agents in the leaching tail water enter the mother liquor for recycling. The aluminum-enriched solution is reinjected for leaching, thus realizing the utilization of the aluminum-enriched material. The acidity and alkalinity of the mine soil are adjusted to the level before leaching by step-by-step leaching, thus reducing the risk of acidification pollution of the mine soil after leaching.

[0071] Example 2

[0072] This embodiment provides a green and low-carbon mining method for ion-type rare earth ore leaching, smelting and leaching, including the following steps:

[0073] The production process of a rare earth mine is "leaching tail water leaching - leaching mother liquor hydrometallurgy - step-by-step leaching and closure". The leaching agent is magnesium sulfate, and the aluminum removal agent, precipitant and regulator are sodium hydroxide. The mineralization liquid is obtained by dissolving aluminum enrichment with sulfuric acid. There is one leaching site and one leaching site. The liquid collection system consists of a liquid collection tunnel, diversion holes, liquid collection trenches, and seepage liquid recovery wells. The recovery rate of leaching mother liquor and leaching tail water is 80%, and the leaching intensity and leaching intensity are 3000m 3 / d, mother liquor collection time is 180 days, leaching tail water collection time is 180 days, leaching time is 180 days, and the leaching liquid volume is about 540,000 m 3 , the amount of leaching water is about 540,000 m 3 The average rare earth content in the leaching mother liquor is about 300 mg / L, aluminum is about 80 mg / L, and magnesium is about 1000 mg / L; the average rare earth content in the leaching tail water is about 60 mg / L, magnesium is about 350 mg / L, sulfate is about 1000 mg / L, and aluminum is about 50 mg / L.

[0074] The details are as follows:

[0075] (a) Leaching tailings water

[0076] The leaching solution is prepared by adding magnesium sulfate and sulfuric acid to the membrane concentrate of the leaching tail water and the supernatant of the water smelting, with 330 tons of magnesium sulfate and 33 tons of sulfuric acid added.

[0077] (b) Leaching mother liquor water treatment

[0078] The mother liquor from the mother liquor pool enters the aluminum removal pool, and sodium hydroxide is added to adjust the pH to 5.4. The aluminum concentrate and the aluminum removal liquid are precipitated. The aluminum removal liquid enters the rare earth precipitation tank, and sodium hydroxide is added to adjust the pH to 7.0. The rare earth product (rare earth hydroxide) and supernatant are obtained by precipitation and filtration. The supernatant enters the reverse osmosis equipment to obtain membrane concentrate and fresh water. The membrane concentrate is used for leaching, and the fresh water is used for leaching. The hydrometallurgy obtains about 140t of aluminum concentrate and about 300t of rare earth products.

[0079] (d) Step-by-step leaching and closure

[0080] After leaching, the mine is washed with fresh water to the tail water of SO4 2+ The concentration is less than 700 mg / L. The second-step regulator is eluted to a pH of 8.0 for the elution tail water, and the third-step mineralization liquid is eluted to a pH of 5.8 for the elution tail water. The elution tail water is collected by the liquid collection system and used for leaching in the leaching field. The injection hole is backfilled with the abandoned soil, compacted to about 50 cm from the hole mouth, and then the topsoil is backfilled in the injection hole to plant plants.

[0081] The production process does not use carbonates, reducing carbon emissions; the leaching tail water is used for leaching in the leaching field, eliminating the leaching tail water treatment, and the rare earths and leaching agents in the leaching tail water enter the mother liquor for recycling; the aluminum enrichment solution is used for leaching, realizing the utilization of the aluminum enrichment; the step-by-step leaching adjusts the acid-base environment of the mine soil to the level before leaching, reducing the risk of acidification pollution of the mine soil after leaching.

[0082] Comparative Example 1

[0083] This comparative example is the ammonium sulfate leaching process of an ionic rare earth mine. The production process is "leaching with leaching solution-collecting mother liquor-removing impurities and settling mother liquor-rinsing with clean water-treating leaching tail water". The leaching agent is ammonium sulfate, and ammonium bicarbonate is used for aluminum removal and precipitation of the mother liquor. After leaching, the mining area is rinsed with clean water, and the leaching tail water is treated by biological methods. A rare earth mine adopts ammonium salt in-situ leaching mining, with one leaching mining area and one leaching mining area. The liquid collection system consists of a liquid collection tunnel, diversion holes, liquid collection trenches, seepage liquid recovery wells, etc. The recovery rate of leaching mother liquor and leaching tail water is 80%, and the leaching intensity and leaching intensity are 3000m 3 / d, mother liquor collection time is 150 days, leaching tail water collection time is 150 days, leaching time is 150 days, and the leaching liquid volume is about 450,000 m 3 , the amount of leaching water is about 450,000 m 3 The average rare earth content in the leaching mother liquor is about 300 mg / L, aluminum is about 50 mg / L, and ammonia nitrogen is about 1100 mg / L; the average rare earth content in the leaching tail water is about 50 mg / L, ammonia nitrogen is about 300 mg / L, sulfate is about 1200 mg / L, and aluminum is about 40 mg / L.

[0084] (a) Leaching liquid

[0085] The leaching solution is prepared by adding ammonium sulfate and sulfuric acid to the supernatant of water smelting, consuming about 450t of ammonium sulfate and about 45t of sulfuric acid.

[0086] (b) Leaching mother liquor water treatment

[0087] The mother liquor from the mother liquor pool enters the aluminum removal pool, and ammonium bicarbonate is added to adjust the pH to 5.4. The aluminum enriched product and the aluminum removal liquid are precipitated. The aluminum removal liquid enters the rare earth precipitation tank, and ammonium bicarbonate is added to adjust the pH to 7.0. The rare earth carbonate product is precipitated. The aluminum enriched product is about 75t, the rare earth carbonate product is about 260t, and about 300t of ammonium bicarbonate is added.

[0088] (c) Clean water washing and washing tail water treatment

[0089] After leaching, the mine is cleaned with water to collect the tail water, which is then treated by biological methods. The cost of treating the tail water is about RMB 10 / m 3 The cost of treating the leaching tail water is about 4.5 million yuan.

[0090] (d) Backfill and closure

[0091] The abandoned soil from the injection hole is backfilled into the injection hole and compacted to 50 cm from the hole mouth. Then the topsoil is backfilled into the injection hole and plants are planted.

[0092] This comparative example is leaching with ammonium sulfate, precipitation of impurities with ammonium bicarbonate, elution with clean water, and biological treatment of ammonia nitrogen in the elution tail water, while Example 1 is an integrated process of leaching-water metallurgy-elution, in which the elution tail water is used for leaching, and no elution tail water treatment is required, and no carbonate is used. Compared with Example 1, the process of this comparative example is more complicated, with an additional consumption of about 160 tons of ammonium sulfate, an additional consumption of about 16 tons of sulfuric acid, a reduced amount of rare earth recovery of about 40 tons, an additional treatment fee of about 4.5 million yuan for elution tail water, an consumption of about 300 tons of ammonium bicarbonate, and an estimated additional carbon emission of about 170 tons; the rare earth and leaching agent in the elution tail water are not recycled; 75 tons of aluminum concentrate need to be stored and disposed of; no conditioning agent elution is performed, and the site is directly backfilled and sealed, and the risk of acidification pollution of the mine soil in the mining area is not eliminated after elution.

[0093] Comparative Example 2

[0094] This comparative example is the magnesium sulfate leaching process of ionic rare earth mines. The production process is the leaching water metallurgy leaching process of "leaching solution leaching-mother liquor collection-mother liquor aluminum removal-rare earth precipitation-clean water leaching-tail water calcium sulfonate treatment". The leaching agent is magnesium sulfate, the aluminum removal agent and precipitant are sodium bicarbonate, and the leaching tail water is treated by calcium sulfonate method. A rare earth mine adopts magnesium salt in-situ leaching mining, with one leaching mining site and one leaching mining site. The liquid collection system consists of a liquid collection tunnel, diversion holes, liquid collection trenches, seepage liquid recovery wells, etc. The recovery rate of leaching mother liquor and leaching tail water is 80%, and the leaching intensity and leaching intensity are 3000m 3 / d, mother liquor collection time is 180 days, leaching tail water collection time is 180 days, leaching time is 180 days, and the leaching liquid volume is about 540,000 m 3 , the amount of leaching water is about 540,000 m 3 The average rare earth content in the leaching mother liquor is about 250 mg / L, and the aluminum content is about 70 mg / L; the rare earth content in the leaching tail water is about 60 mg / L, the average magnesium content is about 350 mg / L, the sulfate content is about 1000 mg / L, the sodium content is about 300 mg / L, and the aluminum content is about 50 mg / L.

[0095] (a) Leaching liquid

[0096] The leaching solution is prepared by adding magnesium sulfate and sulfuric acid to the supernatant of water smelting, consuming about 500t of magnesium sulfate and about 50t of sulfuric acid.

[0097] (b) Leaching mother liquor water treatment

[0098] The mother liquor from the mother liquor pool enters the aluminum removal pool, and sodium bicarbonate is added to adjust the pH to 5.4. The aluminum concentrate and the aluminum removal liquid are precipitated. The aluminum removal liquid enters the rare earth precipitation tank, and sodium bicarbonate is added to adjust the pH to 7.0. The rare earth product (rare earth carbonate) is precipitated and filtered. The aluminum concentrate is about 125t and the rare earth product is about 255t.

[0099] (a) Clean water washing and washing tail water treatment

[0100] Clean water is used to wash the mining area after leaching, and the washing tail water is collected. Lime and aluminum sulfate are added to the washing tail water to adjust the pH to 11.5, and the sludge volume is about 1100t after stirring and precipitation.

[0101] (b) Backfill and seal the site

[0102] The abandoned soil from the injection hole is backfilled into the injection hole and compacted to 50 cm from the hole mouth. Then the topsoil is backfilled into the injection hole and plants are planted.

[0103] This comparative example is leaching with magnesium sulfate, precipitation for aluminum removal with sodium bicarbonate, elution with clean water, and treatment of elution tail water with calcium sulfonate method, while Example 1 is an integrated process of leaching-water metallurgy-elution, and elution tail water is used for leaching, and no elution tail water treatment is required, and carbonate is not used in production. Compared with Example 1, the process of this comparative example is more complicated, with an additional consumption of about 170 tons of magnesium sulfate, an additional consumption of about 17 tons of sulfuric acid, a reduced amount of rare earth recovery of about 45 tons, an additional treatment fee of about 5 million yuan for elution tail water, an additional consumption of about 320 tons of sodium bicarbonate, and an estimated additional carbon emission of about 180 tons; rare earths and leaching agents in the elution tail water are not recycled; aluminum concentrate is about 75 tons, and the amount of sludge treated by the calcium sulfonate method is about 1,100 tons, which needs to be stored and disposed of; no conditioning agent elution is performed, and the site is directly backfilled and sealed, and the risk of acidification pollution of the mine soil in the mining area is not eliminated after elution.

[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A green and low-carbon mining method for ion-type rare earth ore leaching, smelting and leaching, characterized in that: include: The tail water of leaching, the membrane concentrate of the supernatant of the water smelting and the leaching agent are mixed to obtain the leaching solution, which is then injected into the leaching field through the injection hole for leaching, and the leaching mother liquor is collected by the liquid collection system; the pH of the leaching solution is 4.8-5.0; the rare earth ion concentration in the leaching mother liquor is not less than 100 mg / L; The leaching mother liquor is subjected to aluminum removal by using an aluminum removal agent to obtain an aluminum concentrate and an aluminum removal liquid; the aluminum removal liquid is reacted with a precipitant to separate the solid and liquid to obtain a rare earth product and a hydrometallurgical supernatant; the hydrometallurgical supernatant is subjected to membrane concentration to obtain the hydrometallurgical supernatant membrane concentrate and hydrometallurgical supernatant membrane concentrated fresh water; after the leaching mother liquor is mixed with the aluminum removal agent, the system pH is 5.2-5.4; after the aluminum removal liquid is mixed with the precipitant, the system pH is 6.7-7.2; The fresh water concentrated by membrane from the supernatant of the water smelting is injected into the leaching field after the leaching through the injection hole for the first leaching. After the first leaching, the mixed solution of the fresh water concentrated by membrane from the supernatant of the water smelting and the regulator is used for the second leaching. After the second leaching, the mineralizer solution is used for the third leaching. The tail water of the first leaching, the second leaching and the third leaching is collected to obtain the leached tail water. The end point of the first leaching is: SO4 2+ Concentration less than or equal to 700mg / L, NH4 + The concentration is less than or equal to 15 mg / L; the end point of the second elution is: the pH of the tail water is 7.5-8.0; the end point of the third elution is: the pH of the tail water is 5.5-6.0; the pH of the mineralizer solution is 4.2-4.5; After the third elution is completed, the injection hole is backfilled to restore vegetation; The leaching agent is magnesium sulfate and / or ammonium sulfate; the aluminum removal agent, the precipitant and the regulator are all sodium hydroxide; and the mineralizer solution is obtained by dissolving the aluminum enrichment by sulfuric acid.

2. The green and low-carbon mining method of ionic rare earth ore leaching, smelting and leaching integration according to claim 1 is characterized in that: The membrane concentration is carried out using a reverse osmosis membrane.

Citation Information

Patent Citations

  • Ion adsorption type rare earth ore in-situ leaching field drip washing and sealing method and application

    CN113265531A

  • Method for leaching and stabilizing closure of ion adsorption type rare earth ore magnesium salt in-situ leaching ore field

    CN115927886A

  • In-situ leaching, leaching and sealing integrated green mining method for ion type rare earth ore

    CN116926353A

  • Green mining method for ionic rare earth ore

    CN117821783A