A composite environmentally friendly upper material and its production process
By using a composite material of modified montmorillonite and hyperbranched toughening agent in polylactic acid fiber, the problem of insufficient toughness of polylactic acid fiber is solved, its impact resistance and fracture strength are significantly improved, and high toughness and mechanical properties are achieved improvement.
Patent Information
- Application Number
- CN202410536502.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-30
AI Technical Summary
The insufficient toughness of polylactic acid fiber results in its low impact resistance and fracture strength in applications. Existing modification methods such as blending modification or inorganic toughening filler composite have problems of reduced strength and rigidity.
A composite material of polylactic acid resin, modified montmorillonite and hyperbranched toughening agent is used to improve the compatibility of montmorillonite and polylactic acid resin through amidation reaction and hydrogen bond formation, and through the hyperbranched toughening agent The urethane structure forms hydrogen bonds with the polylactic acid matrix resin to improve toughness and mechanical strength.
The impact resistance and fracture strength of the polylactic acid composite fiber are significantly improved, and its toughness and mechanical properties are enhanced, while maintaining the excellent performance of the original functions.
Smart Images

Figure BDA0004819755480000031 
Figure BDA0004819755480000032 
Figure BDA0004819755480000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of shoe upper materials, and in particular relates to a composite environmentally friendly shoe upper material and a production process thereof. Background Art
[0002] The materials of shoes are mainly natural fiber fabrics and leather. In modern times, there are more chemical synthetic materials. According to the structure of shoes, they can be divided into four categories: upper materials, lining materials, bottom materials and auxiliary materials. The existing upper materials are mainly woven fabrics and silicone leather.
[0003] Natural fibers were first used as raw materials for weaving materials. This type of fiber has the advantages of good air permeability, high comfort, good environmental protection, and high heat resistance. It is more suitable for spring and summer clothing and is conducive to heat dissipation and perspiration. However, natural fibers have poor durability and are prone to wear, which affects their service life. With the development of science and technology, artificially synthesized polymer compounds are used as raw materials. After preparing spinning solution, weaving and post-processing processes, fibers with textile functions are obtained. These fibers not only have similar functions to natural fibers, but also can make up for the poor durability of natural fibers. However, the plastics used in artificial synthetic fibers are difficult to degrade in the natural environment, which can easily pollute the environment and cannot meet the requirements of green development.
[0004] Silicone leather is a synthetic material composed of silicone rubber and coating materials. It has good wear resistance, UV resistance, waterproofness, and anti-fouling functions. At the same time, the surface of silicone rubber is soft, comfortable to the touch, and has good elasticity and plasticity. It is widely used in shoe upper materials, but silicone leather is also a synthetic polymer and is also difficult to degrade in the natural environment.
[0005] Polylactic acid fiber, also known as "corn fiber", has antibacterial, warmth-keeping, skin-friendly, breathable and other functions. At the same time, as a biodegradable polymer material, it can be degraded into carbon dioxide and water in nature after use. Due to its excellent performance and environmental protection characteristics, it is widely used in environmentally friendly shoe upper materials; but due to the poor crystallization ability of polylactic acid, the usual processing method leads to a very low degree of crystallinity of the material, so the generated crystal size is large, resulting in poor toughness of the polylactic acid material, thus limiting the wide application of polylactic acid fibers. In order to overcome the disadvantage of poor toughness of polylactic acid fibers, the commonly used practices are currently blending modification, inorganic toughening filler composite modification or chemical modification methods, etc., but these methods all have inevitable problems. For example, blending elastomers such as ethylene / octene copolymers and ethylene / vinyl acetate copolymers in polylactic acid can improve the toughness of polylactic acid, but will inevitably lead to a decrease in strength and rigidity; adding inorganic toughening fillers such as nano-calcium carbonate, modified rectorite particles, montmorillonite, etc., but these inorganic rigid particles are not well dispersed in the matrix, resulting in limited toughening effects; therefore, it is necessary to develop a polylactic acid material that can both improve the toughness of polylactic acid and not affect its performance. Summary of the invention
[0006] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a composite environmentally friendly upper material and a production process thereof;
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A composite environmentally friendly shoe upper material, comprising the following raw materials in parts by weight:
[0009] 100 parts of polylactic acid resin, 10-15 parts of hyperbranched toughening agent, 5-8 parts of modified montmorillonite, 2-3 parts of antioxidant and 1-2 parts of lubricant;
[0010] The modified montmorillonite is prepared by the following method:
[0011] Step A1: ricinoleic acid, DCC, DMAP and DMF are mixed and added into a reaction kettle, the stirring reaction rate is controlled to be 200-300 r / min, the temperature is raised to 50-65° C., and p-hydroxyaniline is added after being kept warm and stirred for 20 minutes. The mixture is kept warm and stirred for 5-6 hours, and then washed with water 2-3 times and dried to obtain intermediate 1;
[0012] Further, the usage ratio of ricinoleic acid, p-hydroxyaniline, DCC, DMAP and DMF is 0.1 mol: 0.1 mol: 10-15 g: 5-7 g: 100 mL;
[0013] In step A1, the carboxyl group in ricinoleic acid and the amino group in p-hydroxyaniline undergo an amidation reaction to form an amide intermediate with an unsaturated long chain and a hydroxyl group;
[0014]
[0015] Step A2: Mix the intermediate 1 and anhydrous aluminum chloride and add them to a reactor, control the stirring reaction rate to 200-300 r / min, raise the temperature to 140-150° C., then introduce hydrogen sulfide gas, and after the hydrogen sulfide gas is completely introduced, keep the temperature for 20 minutes to obtain the intermediate 2;
[0016] Further, the usage ratio of intermediate 1, hydrogen sulfide gas and anhydrous aluminum chloride is 0.1 mol: 2 mol: 0.3-0.5 g;
[0017] In step A2, the unsaturated double bond in the intermediate 1 undergoes an addition reaction with hydrogen sulfide gas to introduce a thiol group; its structural formula is shown below:
[0018]
[0019] Step A3: Disperse ultrafine montmorillonite in deionized water, control the stirring reaction rate to 150-200 r / min, heat to 30-35° C., stir for 10 min, add intermediate 2, continue to stir for 1-2 h, filter and dry to obtain modified montmorillonite;
[0020] Further, the dosage ratio of ultrafine montmorillonite, intermediate 2 and deionized water is 10 g: 3-5 g: 50 mL;
[0021] In step A3, the hydroxyl group and amide group contained in the intermediate 2 can form hydrogen bonds with the hydroxyl group contained on the surface of the ultrafine montmorillonite, so that the intermediate 2 is grafted onto the surface of the ultrafine montmorillonite;
[0022] The hyperbranched toughening agent is prepared by the following method:
[0023] Step B1: citric acid, EDC, NHS and THF were mixed and added into a reactor, the stirring reaction rate was controlled to be 100-200 r / min, the temperature was raised to 25-40°C, and p-methoxyaniline was added after stirring for 10 min. The reaction was stirred for 2-3 h and then vacuum rotary evaporation was performed to obtain intermediate 3;
[0024] Further, the usage ratio of citric acid, p-methoxyaniline, EDC, NHS and THF is 0.1 mol: 0.3 mol: 15-20 g: 8 g: 100 mL;
[0025] In step B1, the carboxyl group in citric acid and the amino group in p-methoxyaniline undergo condensation reaction to introduce a rigid benzene ring structure and a methoxy group; the structural formula is shown below:
[0026]
[0027] Step B2: Take intermediate 3, potassium carbonate and DMSO and mix them into a reactor, control the stirring reaction rate to 300-400r / min, heat to 90-100°C, keep stirring for 30 minutes, add propylene chloride under nitrogen atmosphere, continue to keep stirring for 4-5 hours, wash with water 2-3 times and dry, then transfer to dichloromethane and add boron tribromide, stand in an ice-water bath for 24 hours, then add water for quenching, then remove the solvent by vacuum rotary evaporation, and finally use Na 2 SO 4 Filtration, concentration and drying were performed to obtain intermediate 4;
[0028] Further, the usage ratio of intermediate 3, propylene chloride, potassium carbonate and DMSO is 0.1 mol: 0.1 mol: 5-8 g: 200 mL; the usage ratio of boron tribromide, dichloromethane and water is 3-5 g: 50 mL: 30 mL;
[0029] In step B2, the hydroxyl group in the intermediate 3 reacts with propylene chloride to graft an unsaturated double bond in the intermediate 3, and then demethylates under the catalytic action of boron tribromide to introduce polyhydroxyl groups; its structural formula is shown below:
[0030]
[0031] Step B3: intermediate 4, isophorone diisocyanate, dibutyltin dilaurate and DMF were mixed and added into a reactor, the stirring reaction rate was controlled to be 300-400 r / min, the temperature was raised to 70-80°C under a nitrogen atmosphere, the mixture was stirred and reacted for 3-4 hours, and then the mixture was washed with water 2-3 times and dried for 24 hours to obtain a hyperbranched toughening agent;
[0032] Further, the usage ratio of intermediate 4, isophorone diisocyanate, TBTDL and DMF is 0.2 mol: 0.3 mol: 0.5-1 g: 500 mL;
[0033] In step B3, the polyhydroxyl group in the intermediate 4 and isophorone diisocyanate undergo an addition reaction to form a hyperbranched toughening agent;
[0034] A production process of a composite environmentally friendly upper material comprises the following steps:
[0035] Step S1: adding polylactic acid resin, hyperbranched toughening agent and modified montmorillonite into a drying oven, and drying for 10 hours to obtain a mixture;
[0036] Further, the drying temperature was set to (60 ± 5) °C;
[0037] Step S2: Mix the mixture, antioxidant and lubricant and feed them into an extruder for melt extrusion, and then spin through a spinneret, cool and shape to obtain polylactic acid composite fiber; then weave it into cloth through a knitting machine to make a composite environmentally friendly shoe upper material;
[0038] Beneficial effects of the present invention:
[0039] The invention discloses a production process of a composite environmentally friendly shoe upper material, which takes polylactic acid resin as a matrix, adds modified montmorillonite and hyperbranched toughening agent to participate in blending, and has higher impact resistance and fracture strength than the existing polylactic acid resin; firstly, the polar hydroxyl group and amide group contained in the intermediate 1 can form hydrogen bonds with the hydroxyl group on the surface of ultrafine montmorillonite, and graft it onto the ultrafine montmorillonite; the flexible long chain contained in the intermediate 1 can be entangled with the polylactic acid resin, thereby improving the compatibility of the ultrafine montmorillonite and the polylactic acid resin matrix; when subjected to external forces, the montmorillonite can absorb energy and induce cracks, and the generation and growth of cracks will consume energy, thereby restraining the expansion of cracks and effectively improving the impact resistance of the matrix;
[0040] At the same time, the hyperbranched toughening agent contains a large amount of carbamate structure, which can form hydrogen bonds with the molecular chains of the polylactic acid matrix resin. On the one hand, it increases the distance between the polylactic acid molecular chains, weakens the intermolecular forces, and reduces the entanglement points between the polylactic acid matrix resin molecular chains, which is beneficial to the enhancement of the toughness of the polylactic acid matrix resin. On the other hand, the physical cross-linking structure formed by the hydrogen bonds can transform the chain structure between the polylactic acid matrix resins into a three-dimensional network structure, which can not only improve its mechanical strength, but also disperse the energy acting on the polylactic acid matrix, thereby playing a role in stress dispersion and further strengthening the toughness of the polylactic acid matrix.
[0041] Moreover, the unsaturated double bonds in the hyperbranched toughening agent and the thiol structure on the modified montmorillonite can undergo a click reaction to produce an interfacial bond of a certain strength, forming an organic-inorganic composite toughening system, and tightly combining with the polylactic acid matrix resin. Through its dispersed energy transfer and the energy consumption of crack generation and growth, the two work together to significantly improve the impact resistance of the polylactic acid matrix resin. DETAILED DESCRIPTION
[0042] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] 1) Preparation of modified montmorillonite
[0045] a1: Take ricinoleic acid, DCC, DMAP and DMF and add them into a reactor, control the stirring reaction rate to 200r / min, heat to 50℃, keep stirring for 20min, then add p-hydroxyaniline, continue to keep stirring for 5h, wash with water twice and dry to obtain intermediate 1; in the above reaction, the amount ratio of ricinoleic acid, p-hydroxyaniline, DCC, DMAP and DMF is 0.1mol:0.1mol:10g:5g:100mL;
[0046] a2: Mix the intermediate 1 and anhydrous aluminum chloride and feed them into a reactor, control the stirring reaction rate to 200r / min, raise the temperature to 140°C, then introduce hydrogen sulfide gas, and after it is completely introduced, keep the temperature for reaction for 20 minutes to obtain intermediate 2; in the above reaction, the amount ratio of intermediate 1, hydrogen sulfide gas and anhydrous aluminum chloride is 0.1mol:2mol:0.3g;
[0047] a3: Disperse ultrafine montmorillonite in deionized water, control the stirring reaction rate to 150r / min, heat to 30℃, keep stirring for 10min, add intermediate 2, then continue to keep stirring for 1h, filter and dry to obtain modified montmorillonite; the dosage ratio of ultrafine montmorillonite, intermediate 2 and deionized water is 10g:3g:50mL;
[0048] 2) Preparation of hyperbranched toughening agent
[0049] b1: Mix citric acid, EDC, NHS and THF into a reactor, control the stirring reaction rate to 100r / min, heat to 25°C, keep stirring for 10min, then add p-methoxyaniline, keep stirring for 2h, then evaporate under reduced pressure to obtain intermediate 3; in the above reaction, the dosage ratio of citric acid, p-methoxyaniline, EDC, NHS and THF is 0.1mol:0.3mol:15g:8g:100mL;
[0050] b2: Take intermediate 3, potassium carbonate and DMSO and mix them into a reactor, control the stirring reaction rate to 300r / min, heat to 90℃, keep stirring for 30min, add propylene chloride under nitrogen atmosphere, continue to keep stirring for 4h, wash twice with water and dry, then transfer to dichloromethane and add boron tribromide, let stand in an ice-water bath for 24h, then add water for quenching, then remove the solvent by vacuum rotary evaporation, and finally use Na 2 SO 4 Filtration, concentration and drying were performed to obtain intermediate 4; in the above reaction, the usage ratio of intermediate 3, propylene chloride, potassium carbonate and DMSO was 0.1 mol: 0.1 mol: 5 g: 200 mL; the usage ratio of boron tribromide, dichloromethane and water was 3 g: 50 mL: 30 mL;
[0051] b3: Take intermediate 4, isophorone diisocyanate, dibutyltin dilaurate and DMF, mix and feed into a reactor, control the stirring reaction rate to 300r / min, heat to 70°C under a nitrogen atmosphere, keep stirring and react for 3 hours, wash with water twice and dry for 24 hours to obtain a hyperbranched toughening agent; in the above reaction, the dosage ratio of intermediate 4, isophorone diisocyanate, TBTDL and DMF is 0.2mol:0.3mol:0.5g:500mL.
[0052] Example 2
[0053] 1) Preparation of modified montmorillonite
[0054] a1: Take ricinoleic acid, DCC, DMAP and DMF and mix them into a reactor, control the stirring reaction rate to 300r / min, heat to 60℃, keep stirring for 20min, then add p-hydroxyaniline, continue to keep stirring for 5h, wash with water 3 times and dry to obtain intermediate 1; in the above reaction, the amount ratio of ricinoleic acid, p-hydroxyaniline, DCC, DMAP and DMF is 0.1mol:0.1mol:15g:7g:100mL;
[0055] a2: Mix the intermediate 1 and anhydrous aluminum chloride and feed them into a reactor, control the stirring reaction rate to 250r / min, raise the temperature to 150°C, then introduce hydrogen sulfide gas, and after it is completely introduced, keep the temperature for reaction for 20 minutes to obtain intermediate 2; in the above reaction, the amount ratio of intermediate 1, hydrogen sulfide gas and anhydrous aluminum chloride is 0.1mol:2mol:0.4g;
[0056] a3: Disperse ultrafine montmorillonite in deionized water, control the stirring reaction rate to 150r / min, heat to 30°C, keep stirring for 10min, add intermediate 2, continue to keep stirring for 1h, filter and dry to obtain modified montmorillonite; the dosage ratio of ultrafine montmorillonite, intermediate 2 and deionized water is 10g:4g:50mL;
[0057] 2) Preparation of hyperbranched toughening agent
[0058] b1: Mix citric acid, EDC, NHS and THF into a reactor, control the stirring reaction rate to 200r / min, heat to 35°C, keep stirring for 10min, then add p-methoxyaniline, keep stirring for 2h, then evaporate under reduced pressure to obtain intermediate 3; in the above reaction, the dosage ratio of citric acid, p-methoxyaniline, EDC, NHS and THF is 0.1mol:0.3mol:20g:8g:100mL;
[0059] b2: Take intermediate 3, potassium carbonate and DMSO and mix them into a reactor, control the stirring reaction rate to 350r / min, heat to 95℃, keep stirring for 30min, add propylene chloride under nitrogen atmosphere, keep stirring for 4h, wash twice with water and dry, then transfer to dichloromethane and add boron tribromide, let stand in ice water bath for 24h, then add water for quenching, then remove the solvent by vacuum rotary evaporation, and finally use Na 2 SO 4 Filtration, concentration and drying were performed to obtain intermediate 4; in the above reaction, the usage ratio of intermediate 3, propylene chloride, potassium carbonate and DMSO was 0.1 mol: 0.1 mol: 8 g: 200 mL; the usage ratio of boron tribromide, dichloromethane and water was 4 g: 50 mL: 30 mL;
[0060] b3: Take intermediate 4, isophorone diisocyanate, dibutyltin dilaurate and DMF, mix and feed into a reactor, control the stirring reaction rate to 350r / min, heat to 75°C under a nitrogen atmosphere, keep stirring and react for 3 hours, wash with water twice and dry for 24 hours to obtain a hyperbranched toughening agent; in the above reaction, the dosage ratio of intermediate 4, isophorone diisocyanate, TBTDL and DMF is 0.2mol:0.3mol:1g:500mL.
[0061] Example 3
[0062] 1) Preparation of modified montmorillonite
[0063] a1: Take ricinoleic acid, DCC, DMAP and DMF and add them into a reactor, control the stirring reaction rate to 400r / min, heat to 65℃, keep stirring for 20min, then add p-hydroxyaniline, continue to keep stirring for 5h, wash with water 3 times and dry to obtain intermediate 1; in the above reaction, the amount ratio of ricinoleic acid, p-hydroxyaniline, DCC, DMAP and DMF is 0.1mol:0.1mol:15g:7g:100mL;
[0064] a2: Mix the intermediate 1 and anhydrous aluminum chloride and feed them into a reactor, control the stirring reaction rate to 300r / min, heat to 150°C, then introduce hydrogen sulfide gas, and after complete introduction, keep the temperature for reaction for 20 minutes to obtain intermediate 2; in the above reaction, the amount ratio of intermediate 1, hydrogen sulfide gas and anhydrous aluminum chloride is 0.1mol:2mol:0.5g;
[0065] a3: Disperse ultrafine montmorillonite in deionized water, control the stirring reaction rate to 200r / min, heat to 35°C, keep stirring for 10min, add intermediate 2, continue to keep stirring for 1h, filter and dry to obtain modified montmorillonite; the dosage ratio of ultrafine montmorillonite, intermediate 2 and deionized water is 10g:5g:50mL;
[0066] 2) Preparation of hyperbranched toughening agent
[0067] b1: Mix citric acid, EDC, NHS and THF into a reactor, control the stirring reaction rate to 200r / min, heat to 40°C, keep stirring for 10min, then add p-methoxyaniline, keep stirring for 2h, then evaporate under reduced pressure to obtain intermediate 3; in the above reaction, the dosage ratio of citric acid, p-methoxyaniline, EDC, NHS and THF is 0.1mol:0.3mol:15g:8g:100mL;
[0068] b2: Take intermediate 3, potassium carbonate and DMSO and mix them into a reactor, control the stirring reaction rate to 400r / min, heat to 100℃, keep stirring for 30min, add propylene chloride under nitrogen atmosphere, keep stirring for 4h, wash twice with water and dry, then transfer to dichloromethane and add boron tribromide, let stand in ice water bath for 24h, then add water for quenching, then remove the solvent by vacuum rotary evaporation, and finally use Na 2 SO 4 Filtration, concentration and drying were performed to obtain intermediate 4; in the above reaction, the usage ratio of intermediate 3, propylene chloride, potassium carbonate and DMSO was 0.1 mol: 0.1 mol: 6 g: 200 mL; the usage ratio of boron tribromide, dichloromethane and water was 5 g: 50 mL: 30 mL;
[0069] b3: Take intermediate 4, isophorone diisocyanate, dibutyltin dilaurate and DMF, mix and feed into a reactor, control the stirring reaction rate to 400r / min, heat to 80°C under a nitrogen atmosphere, keep stirring and react for 3 hours, wash with water twice and dry for 24 hours to obtain a hyperbranched toughening agent; in the above reaction, the dosage ratio of intermediate 4, isophorone diisocyanate, TBTDL and DMF is 0.2mol:0.3mol:1g:500mL.
[0070] The formula of raw materials used in this embodiment is as follows:
[0071] Polylactic acid resin: polylactic acid resin of Shanghai Aladdin Biochemical Technology Co., Ltd., model number P169115;
[0072] Anti-aging agent: Anti-aging agent 246BHT;
[0073] Lubricant: lauric acid;
[0074] Example 4
[0075] A production process of a composite environmentally friendly upper material comprises the following steps:
[0076] 100 parts of polylactic acid resin, 10 parts of hyperbranched toughening agent prepared in Example 1, 5 parts of modified montmorillonite prepared in Example 1, 1 part of antioxidant and 1 part of lubricant
[0077] s1: weighing raw materials according to weight, adding polylactic acid resin, hyperbranched toughening agent and modified montmorillonite into a drying oven at 60° C., and drying for 10 hours to obtain a mixture;
[0078] s2: The mixed material, antioxidant and lubricant are mixed and fed into an extruder for melt extrusion, and then spun through a spinneret, cooled and shaped to obtain polylactic acid composite fibers; and then woven into cloth through a knitting machine to make a composite environmentally friendly shoe upper material.
[0079] Example 5
[0080] A production process of a composite environmentally friendly upper material comprises the following steps:
[0081] 100 parts of polylactic acid resin, 15 parts of hyperbranched toughening agent prepared in Example 2, 8 parts of modified montmorillonite prepared in Example 2, 3 parts of antioxidant and 2 parts of lubricant
[0082] s1: weighing raw materials according to weight, adding polylactic acid resin, hyperbranched toughening agent and modified montmorillonite into a drying oven at 60° C., and drying for 10 hours to obtain a mixture;
[0083] s2: The mixed material, antioxidant and lubricant are mixed and fed into an extruder for melt extrusion, and then spun through a spinneret, cooled and shaped to obtain polylactic acid composite fibers; and then woven into cloth through a knitting machine to make a composite environmentally friendly shoe upper material.
[0084] Example 6
[0085] A production process of a composite environmentally friendly upper material comprises the following steps:
[0086] 100 parts of polylactic acid resin, 15 parts of the hyperbranched toughening agent prepared in Example 3, 8 parts of the modified montmorillonite prepared in Example 3, 3 parts of antioxidant and 2 parts of lubricant lauric acid
[0087] s1: weighing raw materials according to weight, adding polylactic acid resin, hyperbranched toughening agent and modified montmorillonite into a drying oven at 60° C., and drying for 10 hours to obtain a mixture;
[0088] s2: The mixed material, antioxidant and lubricant are mixed and fed into an extruder for melt extrusion, and then spun through a spinneret, cooled and shaped to obtain polylactic acid composite fibers; and then woven into cloth through a knitting machine to make a composite environmentally friendly shoe upper material.
[0089] Comparative Example 1
[0090] This comparative example prepares a composite environmentally friendly shoe upper material, which is different from Example 6 in that the added montmorillonite is KH-570 modified montmorillonite.
[0091] Comparative Example 2:
[0092] This comparative example prepares a composite environmentally friendly upper material, which is different from Example 6 in that the added hyperbranched toughening agent is the unsaturated hyperbranched polyurethane in patent CN104311783A.
[0093] Comparative Example 3:
[0094] This comparative example prepares a composite environmentally friendly upper material, which is different from Example 6 in that the added montmorillonite is KH-570 modified montmorillonite, and the hyperbranched toughening agent is the unsaturated hyperbranched polyurethane in patent CN104311783A.
[0095] Comparative Example 4:
[0096] A polylactic acid resin (in this comparative example, a commercially available PLA toughened grade, model L8600H I) , an antioxidant and a lubricant are mixed and fed into an extruder for melt extrusion, and then spun through a spinneret, cooled and shaped to obtain a polylactic acid composite fiber; and then woven into a cloth through a knitting machine to make a composite environmentally friendly shoe upper material.
[0097] The polylactic acid composite fibers prepared in Examples 4-6 and Comparative Examples 1-4 were tested by an XQ-1A yarn strength and elongation tester:
[0098] Toughening performance test:
[0099] The polylactic acid composite fibers prepared in Examples 4-6 and Comparative Examples 1-4 were subjected to impact resistance tests according to GB / T1451-2005. The test data are shown in Table 1:
[0100] Table 1
[0101]
[0102] From the data in Table 1, it can be seen that the composite environmentally friendly upper materials prepared in Examples 4-6 have a breaking strength of 4.7-5.1 CN / dtex, a breaking elongation of 26.5-27.6%, and an impact strength of 5.52-5.64 KJ / m 2 The breaking strength of the environmentally friendly composite upper material in comparative example 1-2 is not much different from that in examples 4-6, but the impact strength is significantly lower than that in examples 4-6. The breaking strength, breaking elongation and impact strength of the environmentally friendly composite upper material in comparative example 3 are significantly higher than those in comparative example 1-2, but still lower than those of the composite environmentally friendly upper material of the banknote in examples 4-6.
[0103] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0104] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A composite environmentally friendly upper material, characterized in that: The composition comprises, by weight, 100 parts of polylactic acid resin, 10-15 parts of hyperbranched toughening agent, 5-8 parts of modified montmorillonite, 2-3 parts of antioxidant and 1-2 parts of lubricant; The modified montmorillonite is prepared by the following method: Step A1: Mix ricinoleic acid, DCC, DMAP and DMF, heat to 50-65°C, stir for 20 minutes, add p-hydroxyaniline, continue to stir for 5-6 hours, wash with water 2-3 times and dry to obtain intermediate 1; Step A2: Mix the intermediate 1 and anhydrous aluminum chloride, raise the temperature to 140-150° C., then introduce hydrogen sulfide gas, and after the hydrogen sulfide gas is completely introduced, keep the temperature for reaction for 20 minutes to obtain the intermediate 2; Step A3: Disperse ultrafine montmorillonite in deionized water, heat to 30-35°C, keep warm and stir for 10 minutes, add intermediate 2, continue to keep warm and stir for 1-2 hours, filter and dry to obtain modified montmorillonite; The hyperbranched toughening agent is prepared by the following method: Step B1: Mix citric acid, EDC, NHS and THF, heat to 25-40°C, stir for 10 min, add p-methoxyaniline, stir for 2-3 h, and evaporate under reduced pressure to obtain intermediate 3; Step B2: Take intermediate 3, potassium carbonate and DMSO, mix and feed, heat to 90-100°C, keep warm and stir for 30 minutes, add propylene chloride under nitrogen atmosphere, continue to keep warm and stir for 4-5 hours, wash with water 2-3 times and dry, then transfer to dichloromethane and add boron tribromide, stand in an ice-water bath for 24 hours, then add water for quenching, then remove the solvent by vacuum rotary evaporation, finally filter with Na2SO4, concentrate and dry to obtain intermediate 4; Step B3: intermediate 4, isophorone diisocyanate, dibutyltin dilaurate and DMF were mixed and added, the temperature was raised to 70-80°C under a nitrogen atmosphere, the mixture was stirred and reacted for 3-4 hours, washed with water 2-3 times and dried for 24 hours to obtain a hyperbranched toughening agent.
2. The composite environmentally friendly upper material according to claim 1, characterized in that: In step A1, the usage ratio of ricinoleic acid, p-hydroxyaniline, DCC, DMAP and DMF is 0.1 mol: 0.1 mol: 10-15 g: 5-7 g: 100 mL; In step A2, the usage ratio of intermediate 1, hydrogen sulfide gas and anhydrous aluminum chloride is 0.1 mol: 2 mol: 0.3-0.5 g.
3. The composite environmentally friendly upper material according to claim 2, characterized in that: In step A3, the usage ratio of ultrafine montmorillonite, intermediate 2 and deionized water is 10 g: 3-5 g: 50 mL.
4. The environmentally friendly composite upper material according to claim 3, characterized in that: In step B1, the usage ratio of citric acid, p-methoxyaniline, EDC, NHS and THF is 0.1 mol: 0.3 mol: 15-20 g: 8g:100mL.
5. The environmentally friendly composite upper material according to claim 4, characterized in that: In step B2, the usage ratio of intermediate 3, propylene chloride, potassium carbonate and DMSO is 0.1 mol: 0.1 mol: 5-8 g: 200 mL; the usage ratio of boron tribromide, dichloromethane and water is 3-5 g: 50 mL: 30 mL.
6. The environmentally friendly composite upper material according to claim 5, characterized in that: In step B3, the usage ratio of intermediate 4, isophorone diisocyanate, TBTDL and DMF is 0.2 mol: 0.3 mol: 0.5-1 g: 500 mL.
7. The production process of a composite environmentally friendly upper material according to claim 6, characterized in that: The following steps are involved: Step S1: adding polylactic acid resin, hyperbranched toughening agent and modified montmorillonite into a drying oven, and drying for 10 hours to obtain a mixture; Step S2: Mix the mixture, antioxidant and lubricant and feed them into an extruder for melt extrusion, and then spin through a spinneret, cool and shape to obtain polylactic acid composite fiber; then use a knitting machine to weave it into cloth to make a composite environmentally friendly shoe upper material.
8. The production process of a composite environmentally friendly upper material according to claim 7, characterized in that: The antioxidant is antioxidant 246BHT.
9. The production process of a composite environmentally friendly upper material according to claim 8, characterized in that: The lubricant is lauric acid.