A road joint repair method
By using a bonding material of emulsified asphalt and modifier at the road joints after milling, and using the slow-release effect of temperature-regulating microcapsules, an oil film with strong crack resistance is formed, which solves the problem of joints during milling and re-paving. Water infiltration and crack problems improve the waterproof and crack-resistant performance of the road and extend the service life of the pavement.
Patent Information
- Application Number
- CN202410375722.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-03-29
AI Technical Summary
During the process of road milling and re-paving, improper joint treatment leads to water infiltration, softening of the roadbed, reduced strength, slurry diseases and cracks, affecting the pavement structure and service life.
Using modified binding materials, including emulsified asphalt, modifiers and temperature-adjusting microcapsules, sodium hydroxide and calcium oxide are slowly released through the mitigating effects of gelatin and polylactic acid, and the pH value and temperature of the emulsified asphalt are adjusted to promote its rapid Demulsification, forming a strong adhesive oil film, combined with water-stable paving and compaction, improves the anti-peeling performance and waterproof performance of the pavement.
It effectively prevents moisture infiltration at joints, enhances the crack resistance of pavement, extends service life, reduces maintenance frequency, reduces noise and dust pollution, and improves urban environmental sanitation.
Smart Images

Figure BDA0004766998640000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of road maintenance, and more specifically, to a method for repairing road joints. Background Art
[0002] With the continuous development of urban construction, more and more roads need constant maintenance and renewal. For damaged or aged roads that need to be repaved, asphalt pavement milling and paving technology has become one of the most commonly used methods. It is an effective solution to completely mill the old pavement to a certain depth and then repave the new pavement.
[0003] In the process of milling and resurfacing, the joint treatment of the new and old pavement is the key. If the joint treatment is not done properly, it is easy to cause water to penetrate from the joint, and then the water will penetrate into the roadbed through the cracks, causing the roadbed material to soften and reduce its strength. Then, under the action of vehicle load, slurry-like substances will be squeezed out of the road surface, causing slurry pumping. In addition, if the joint treatment is not done properly, cracks are likely to appear around the pits formed by milling in the subsequent resurfacing process. The cracks in the base layer will be reflected to the surface layer, causing cracks in the asphalt pavement. The cracks in the pavement not only affect the appearance of the road and driving comfort, but are also more likely to expand and cause structural damage to the pavement, shortening the service life of the pavement. In addition, rainwater and other debris will enter the surface structure and roadbed along the cracks, causing the pavement to have a reduced bearing capacity and accelerating local or large-scale damage to the pavement.
[0004] Therefore, in the process of planing, milling and resurfacing construction, the treatment of joints after milling plays a vital role in the quality of road maintenance. Summary of the invention
[0005] In order to improve the waterproofness and crack resistance of joints during road milling and resurfacing, reduce subsequent cracking and water seepage, and improve road quality, the present application provides a road joint repair method.
[0006] In the first aspect, the present application provides a road joint repair method, which adopts the following technical solution:
[0007] A road joint repair method comprises the following steps:
[0008] The modified bonding material is spread on the groove wall and groove bottom formed after the road is milled in layers, and water-stabilized paving and compaction are carried out in the groove after 5-10 minutes. The modified bonding material is obtained by mixing a modifier and emulsified asphalt in a volume ratio of 1: (2.5-3.5); the modifier includes the following raw materials in parts by weight: 50-70 parts of hydrotalcite, 15-25 parts of anti-cracking fiber, 10-20 parts of fluorocarbon resin and 5-10 parts of temperature-regulating microcapsules;
[0009] The temperature regulating microcapsule comprises a core material and a wall material. The core material comprises a mixture of sodium hydroxide and calcium oxide, and the wall material is made of a mixture of polylactic acid, polyurea and gelatin.
[0010] By adopting the above technical scheme, in the present application, after milling, a bonding material containing emulsified asphalt and a modifier is first spread on the wall of the pit formed, and temperature-regulating microcapsules are added to the bonding material. After the gelatin of the wall material meets the emulsified asphalt, the gelatin dissolves due to the water content in the emulsified asphalt, and the polylactic acid is also slowly corroded and decomposed by water molecules in the water, so that the sodium hydroxide and calcium oxide in the capsule are slowly released. Both of them are soluble in water and release heat, which promotes the evaporation of water. In addition, sodium hydroxide has strong water absorption, so that sodium hydroxide can absorb water molecules in the emulsified asphalt, and the addition of the two regulates the emulsified asphalt body. The pH value of the system causes the emulsified asphalt to quickly demulsify within 5-10 minutes due to the changes in pH value and temperature of the bonding material system. After demulsification, a highly adhesive oil film is formed on the wall of the pit formed by milling, and then the water-stabilized concrete is spread and compacted in the pit. The emulsified asphalt is combined with the mineral materials in the spread water-stabilized concrete to form a uniform bonding layer, forming an overall pavement structure, improving the pavement's anti-stripping performance, and preventing the pavement from cracking. In addition, the emulsified asphalt eventually forms an asphalt film, which effectively prevents surface water from seeping into the joints and ground water from rising, prevents water from eroding and damaging the pavement, and eliminates road pumping diseases.
[0011] The temperature regulating microcapsules in the modifier in the present application can adjust the demulsification time of the emulsified asphalt, and the asphalt can be spread after rapid demulsification, so that the combination with the water-stabilizing layer is more firm and the bonding strength is high. The addition of fluorocarbon resin further improves the waterproof performance of the emulsified asphalt and the water resistance of the joints. Polyurea can also play a good waterproof role. On the one hand, it improves the waterproof performance of the bonding material, and on the other hand, it plays a slow-release role in the release of the core material in the temperature regulating microcapsules. Combined with the effect of polylactic acid, the modifier and the emulsified asphalt are mixed for sufficient time, and there is sufficient time to mix and spread the two. After the core material is slowly released, the temperature is increased and the pH value is adjusted, so that the emulsification is quickly broken after spreading; the addition of anti-cracking fiber further improves the crack resistance of the joint, and is more conducive to the emulsified asphalt and the water-stabilizing bonding to form a stable layer, improve the quality of joint treatment, improve the quality of maintenance projects, reduce the maintenance frequency, avoid traffic jams and hidden dangers of traffic accidents, improve the image of the city and environmental sanitation, reduce the noise and dust generated during construction, and avoid interference and pollution to surrounding residents.
[0012] Optionally, the hydrotalcite is added after being modified by the following method:
[0013] The hydrotalcite and ethylene glycol are stirred to obtain a primary mixture, sodium terephthalate is dissolved in water, and then the primary mixture is added, stirred at 80-100° C. for 1-2 hours, filtered and washed with water, and then a silane coupling agent is added to obtain a modified hydrotalcite.
[0014] By adopting the above technical solution, the strength and heat resistance of the bonding material are improved after the hydrotalcite is modified and added, and the bonding material is prevented from softening and failing due to the heat release of the temperature-regulating microcapsules, so that the bonding material can be demulsified quickly without affecting its viscosity and forming.
[0015] In the present application, the hydrotalcite is first modified with sodium terephthalate, and the terephthalate anions realize the anion exchange between the hydrotalcite layers, and the intercalation modification of the hydrotalcite is realized by introducing terephthalate ions. The introduction of rigid groups is beneficial to improving the thermal stability of the hydrotalcite. Then, through the modification of the silane coupling agent, the coupling of the hydrotalcite surface with the polymer emulsion and the capsule and other substances is realized, which is not only beneficial to the dispersion of the hydrotalcite in the modifier system, but also enables the bonding material to form a macromolecular network structure under the action of the silane coupling agent, thereby further improving its crack resistance and waterproof performance.
[0016] Optionally, the mass ratio of the hydrotalcite to ethylene glycol is 1:(0.4-0.6), the mass ratio of the sodium terephthalate to the hydrotalcite is 1:(2-3), the mass ratio of the sodium terephthalate to water is 1:(3-5), and the mass ratio of the silane coupling agent to the hydrotalcite is 1:(3-4).
[0017] By adopting the above technical solution and selecting the above ratio to obtain the modified hydrotalcite, the comprehensive performance of the road at the joint of the final bonding material is better.
[0018] Optionally, the modifier further comprises 15-30 parts by weight of versatate vinyl carbonate, 8-15 parts by weight of EVA emulsion and 3-5 parts by weight of vinyl triethoxy silane.
[0019] By adopting the above technical solution, the addition of tert-butyl vinyl carbonate helps to further improve the waterproof performance of the bonding material, thereby further improving the waterproof performance of the joint. The addition of EVA emulsion further improves the bonding strength of the emulsified asphalt, and EVA emulsion has a certain hydrophilicity, which is conducive to improving the compatibility of the modifier and emulsified asphalt, and the addition of vinyl triethoxysilane as a silane additive can achieve cross-linking of EVA emulsion and tert-butyl vinyl carbonate, thereby improving the water resistance of EVA emulsion, and at the same time, the tert-butyl vinyl carbonate in the modifier, EVA emulsion and polymers such as polycarboxylic acid on the surface of the phase change capsule form a macromolecular network structure, further improving its water resistance.
[0020] Optionally, the added mass ratio of sodium hydroxide to calcium oxide is 1:(0.3-0.5);
[0021] The added mass ratio of the polylactic acid, polyurea and gelatin is 1:(0.3-0.5):(0.6-0.8).
[0022] By adopting the above technical scheme and controlling the raw materials in the wall material, polylactic acid is corroded and decomposed in water molecules, gelatin is soluble in water, and polyurea is insoluble in water. By adjusting the mass ratio of the three, the core material can be slowly released, thereby achieving the control of the demulsification time of the emulsified asphalt, ensuring that it has sufficient operating time, and can also quickly demulsify and bond with the water-stabilizing layer to improve the maintenance quality of the joints.
[0023] Optionally, the added mass ratio of the core material to the wall material is 1:(0.8-1.2).
[0024] Optionally, the temperature-regulating microcapsules are prepared by the following method:
[0025] Dry granulating sodium hydroxide and calcium oxide to obtain core material particles;
[0026] Polylactic acid, polyurea and gelatin are dissolved in methanol to prepare a coating solution, which is then sprayed on the surface of the core particles and dried to obtain temperature-adjusting microcapsules. The amount of methanol added is 3-5 times the mass of the sum of the amounts of polylactic acid, polyurea and gelatin added.
[0027] Optionally, the anti-cracking fiber is one or more of steel fiber or basalt fiber.
[0028] Optionally, the emulsified asphalt is an emulsified asphalt prepared using a cationic emulsifier.
[0029] By adopting the above technical scheme, when the emulsified asphalt is prepared by using a cationic emulsifier, the emulsified asphalt is acidic and reacts with the alkaline phase after the core material in the temperature regulating microcapsule is released, thereby accelerating the demulsification speed and realizing the regulation of the demulsification speed.
[0030] Optionally, the modified bonding material is spread at the bottom of the pit at a rate of 0.8-1.2 kg / m 2 , the spreading amount on the side wall of the pit is 0.3-0.5kg / m 2 .
[0031] In summary, this application has the following beneficial effects:
[0032] 1. In the present application, a bonding material containing emulsified asphalt and a modifier is first spread on the wall of the pit formed after milling. The emulsified asphalt is quickly demulsified within 5-10 minutes. After demulsification, a highly adhesive oil film is formed on the wall of the pit formed by milling. Then, water-stabilized paving and compaction are carried out in the pit. The emulsified asphalt is combined with the mineral material in the water-stabilized paving to form a uniform bonding layer, forming an overall pavement structure, improving the anti-stripping performance of the pavement, and preventing the pavement from cracking. In addition, the emulsified asphalt eventually forms an asphalt film, which effectively prevents the infiltration of surface water and the upwelling of ground water at the joints, prevents the erosion and damage of the pavement by water, and eliminates the road pumping disease.
[0033] 2. The temperature-regulating microcapsules in the modifier of the present application can adjust the demulsification time of the emulsified asphalt, and the emulsified asphalt can be spread after rapid demulsification, so that the combination with the water-stabilizing layer is more firm and the bonding strength is high. The addition of fluorocarbon resin further improves the waterproof performance of the emulsified asphalt and the water resistance of the joints. Polyurea can also play a good waterproof role. On the one hand, it improves the waterproof performance of the bonding material, and on the other hand, it plays a slow-release role in the release of the core material in the temperature-regulating microcapsule. Combined with the effect of polylactic acid, the modifier and the emulsified asphalt have sufficient mixing time, and there is sufficient time to mix and spread the two. After the core material is slowly released, the temperature is increased and the pH value is adjusted, so that the emulsification is quickly broken after spreading;
[0034] 3. The temperature-regulating microcapsules are added to the adhesive material of the present application. When the gelatin of the wall material meets the emulsified asphalt, the gelatin dissolves due to the water content in the emulsified asphalt, and the polylactic acid is also slowly eroded and decomposed by water molecules in the water, so that the sodium hydroxide and calcium oxide in the capsule are slowly released. Both are soluble in water and release heat, which promotes the evaporation of water. In addition, sodium hydroxide has strong water absorption, so that sodium hydroxide can absorb water molecules in the emulsified asphalt. The addition of the two regulates the pH value of the emulsified asphalt system, so that the adhesive material system can achieve the regulation of the emulsified asphalt demulsification time due to the changes in pH value and temperature;
[0035] 4. In the present application, the hydrotalcite is first modified with sodium terephthalate, and the terephthalate anions realize the anion exchange between the hydrotalcite layers, and the intercalation modification of the hydrotalcite is introduced into the terephthalate ions. The introduction of the rigid group is beneficial to improve the thermal stability of the hydrotalcite. Then, the surface of the hydrotalcite is modified by the silane coupling agent to realize the coupling with the EVA emulsion and the capsule and other materials, which is not only beneficial to the dispersion of the hydrotalcite in the modifier system, but also enables the bonding material to form a macromolecular network structure under the action of the silane coupling agent, thereby further improving its crack resistance and waterproof performance;
[0036] 5. The addition of EVA emulsion further improves the bonding strength of emulsified asphalt, and EVA emulsion has a certain hydrophilicity, which is beneficial to improve the compatibility between the modifier and emulsified asphalt. The addition of vinyl triethoxysilane as a silane additive can achieve the cross-linking of EVA emulsion and versatate, thereby improving the water resistance of EVA emulsion. At the same time, the versatate in the modifier, EVA emulsion and polymers such as polycarboxylic acid on the surface of the phase change capsule form a macromolecular network structure, further improving its water resistance. DETAILED DESCRIPTION
[0037] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.
[0038] The fluorocarbon resin in the following embodiments is the fluorocarbon resin of model CX-803 produced by Shanghai Deyude Trade Co., Ltd.; the EVA emulsion in the following embodiments is the EVA emulsion of model EP706K produced by Guangdong Hualitai Chemical Co., Ltd.
[0039] The emulsified asphalt in the present application is an emulsified asphalt made with a cationic emulsifier. In the following examples, the emulsified asphalt model BC-1 from Xinxiang Tantu Road and Bridge Engineering Co., Ltd. is used.
[0040] The following preparation example is an example of the preparation of temperature-regulating microcapsules
[0041] Preparation Example 1
[0042] A method for preparing temperature-regulating microcapsules comprises the following steps:
[0043] Sodium hydroxide and calcium oxide are mixed in a mass ratio of 1:0.4, and dry granulation is performed to obtain core particles with a particle size of 0.1-0.2 mm; polylactic acid, polyurea and gelatin are dissolved in methanol to obtain a coating solution, and then the coating solution is sprayed on the surface of the core particles, and dried to obtain temperature-regulating microcapsules, the added mass ratio of polylactic acid, polyurea and gelatin is 1:0.4:0.7, and the added mass ratio of core material and wall material is 1:1, that is, the mass ratio of the sum of the added amounts of sodium hydroxide and calcium oxide to the sum of the added amounts of polylactic acid, polyurea and gelatin is 1:1, and the added amount of methanol is 4 times the mass of the sum of the added amounts of polylactic acid, polyurea and gelatin.
[0044] Preparation Example 2
[0045] A method for preparing temperature-regulating microcapsules comprises the following steps:
[0046] Sodium hydroxide and calcium oxide are mixed in a mass ratio of 1:0.3, and dry granulation is performed to obtain core particles with a particle size of 0.1-0.2 mm; polylactic acid, polyurea and gelatin are dissolved in methanol to obtain a coating solution, and then the coating solution is sprayed on the surface of the core particles, and dried to obtain temperature-regulating microcapsules, the added mass ratio of polylactic acid, polyurea and gelatin is 1:0.3:0.6, and the added mass ratio of core material and wall material is 1:0.8, that is, the mass ratio of the sum of the added amounts of sodium hydroxide and calcium oxide to the sum of the added amounts of polylactic acid, polyurea and gelatin is 1:0.8, and the added amount of methanol is 3 times the mass of the sum of the added amounts of polylactic acid, polyurea and gelatin.
[0047] Preparation Example 3
[0048] A method for preparing temperature-regulating microcapsules comprises the following steps:
[0049] Sodium hydroxide and calcium oxide are mixed in a mass ratio of 1:0.5, and dry granulation is performed to obtain core particles with a particle size of 0.1-0.2 mm; polylactic acid, polyurea and gelatin are dissolved in methanol to obtain a coating solution, and then the coating solution is sprayed on the surface of the core particles, and dried to obtain temperature-regulating microcapsules, the added mass ratio of polylactic acid, polyurea and gelatin is 1:0.5:0.8, and the added mass ratio of core material and wall material is 1:1.2, that is, the mass ratio of the sum of the added amounts of sodium hydroxide and calcium oxide to the sum of the added amounts of polylactic acid, polyurea and gelatin is 1:1.2, and the added amount of methanol is 5 times the mass of the sum of the added amounts of polylactic acid, polyurea and gelatin.
[0050] Comparative Preparation Example 1
[0051] A method for preparing temperature-regulating microcapsules is carried out according to the method in Preparation Example 1, except that polyurea is replaced by polylactic acid and gelatin in equal amounts at a mass ratio of 1:0.7.
[0052] Comparative Preparation Example 2
[0053] A method for preparing temperature-regulating microcapsules is carried out according to the method in Preparation Example 1, except that polylactic acid is replaced by polyurea and gelatin in equal amounts at a mass ratio of 0.4:0.7.
[0054] Example 1
[0055] A road joint repair method comprises the following steps:
[0056] S1. Prepare a modifier: mix 20 kg of anti-cracking fiber and 60 kg of hydrotalcite, then add 15 kg of fluorocarbon resin, and finally add 8 kg of the temperature-regulating microcapsules prepared in Preparation Example 1, mix and stir for 15 minutes to prepare a modifier; wherein the anti-cracking fiber is steel fiber;
[0057] S2, preparing a modified bonding material: mixing the modifier prepared in step S1 with the emulsified asphalt in a volume ratio of 1:3, and stirring to prepare a modified bonding material;
[0058] S3. The road is milled in layers to the water-stable base to form a T-shaped pit. Then, the modified bonding material is spread on the wall and bottom of the T-shaped pit formed after the road milling. After 8 minutes, the emulsified asphalt in the modified bonding material is demulsified. After demulsification, the water-stable layer is spread and compacted in the pit to fill the water-stable layer. The amount of modified bonding material spread on the bottom of the pit is 1.0 kg / m 2 The amount of modified bonding material spread on the side wall of the pit is 0.4kg / m 2 .
[0059] Example 2
[0060] A road joint repair method comprises the following steps:
[0061] S1. Prepare a modifier: mix 15 kg of anti-cracking fiber and 50 kg of hydrotalcite, then add 10 kg of fluorocarbon resin, and finally add 5 kg of the temperature-regulating microcapsules prepared in Preparation Example 2, mix and stir for 10 minutes to prepare a modifier; wherein the anti-cracking fiber is steel fiber;
[0062] S2, preparing a modified bonding material: mixing the modifier prepared in step S1 with the emulsified asphalt in a volume ratio of 1:2.5, and stirring to prepare a modified bonding material;
[0063] S3. The road is milled in layers to the water-stable base to form a T-shaped pit. Then, the modified bonding material is spread on the wall and bottom of the T-shaped pit formed after the road milling. After 5 minutes, the emulsified asphalt in the modified bonding material is demulsified. After demulsification, the water-stable layer is spread and compacted in the pit to fill the water-stable layer. The amount of modified bonding material spread on the bottom of the groove is 0.8kg / m 2 The amount of modified bonding material spread on the side wall of the pit is 0.3kg / m 2 .
[0064] Example 3
[0065] A road joint repair method comprises the following steps:
[0066] S1. Prepare a modifier: mix 25 kg of anti-cracking fiber and 70 kg of hydrotalcite, then add 20 kg of fluorocarbon resin, and finally add 10 kg of the temperature-regulating microcapsules prepared in Preparation Example 3, mix and stir for 20 minutes to prepare a modifier; wherein the anti-cracking fiber is steel fiber;
[0067] S2, preparing a modified bonding material: mixing the modifier prepared in step S1 with the emulsified asphalt in a volume ratio of 1:3.5, and stirring to prepare a modified bonding material;
[0068] S3. The road is milled in layers to the water-stable base to form a T-shaped pit. Then, the modified bonding material is spread on the wall and bottom of the T-shaped pit formed after the road milling. After 10 minutes, the emulsified asphalt in the modified bonding material is demulsified. After demulsification, the water-stable layer is spread and compacted in the pit to fill the water-stable layer. The amount of modified bonding material spread on the bottom of the groove is 1.2kg / m 2 The amount of modified bonding material spread on the side wall of the pit is 0.5kg / m 2 .
[0069] Example 4
[0070] A road joint repair treatment method is carried out according to the method in Example 1, except that in step S1, the hydrotalcite is modified by the following method and then added:
[0071] The hydrotalcite and ethylene glycol are stirred in a mass ratio of 1:0.5 to obtain a primary mixture, sodium terephthalate is dissolved in water, the mass ratio of sodium terephthalate to hydrotalcite is 1:2.5, and the mass ratio of sodium terephthalate to water is 1:4, then the primary mixture is added to the terephthalic acid solution dissolved in water, stirred at 90°C for 1.5h, filtered and washed with water, and then silane coupling agent KH-560 is added to obtain modified hydrotalcite, and the mass ratio of silane coupling agent to hydrotalcite is 1:3.5.
[0072] Example 5
[0073] A road joint repair treatment method is carried out according to the method in Example 1, except that in step S1, the hydrotalcite is modified by the following method and then added:
[0074] The hydrotalcite and ethylene glycol are stirred in a mass ratio of 1:0.4 to obtain a primary mixture, sodium terephthalate is dissolved in water, the mass ratio of sodium terephthalate to hydrotalcite is 1:2, and the mass ratio of sodium terephthalate to water is 1:3, then the primary mixture is added to the terephthalic acid solution dissolved in water, stirred at 80°C for 2h, filtered and washed with water, and then silane coupling agent KH-560 is added to obtain modified hydrotalcite, and the mass ratio of silane coupling agent to hydrotalcite is 1:3.
[0075] Example 6
[0076] A road joint repair treatment method is carried out according to the method in Example 1, except that in step S1, the hydrotalcite is modified by the following method and then added:
[0077] The hydrotalcite and ethylene glycol are stirred in a mass ratio of 1:0.6 to obtain a primary mixture, sodium terephthalate is dissolved in water, the mass ratio of sodium terephthalate to hydrotalcite is 1:3, and the mass ratio of sodium terephthalate to water is 1:5, then the primary mixture is added to the terephthalic acid solution dissolved in water, stirred at 100°C for 1h, filtered and washed with water, and then silane coupling agent KH-560 is added to obtain modified hydrotalcite, and the mass ratio of silane coupling agent to hydrotalcite is 1:4.
[0078] Example 7
[0079] A road joint repair treatment method is carried out according to the method in Example 4, except that when the hydrotalcite is modified, no silane coupling agent is added for modification after filtration and water washing, and the hydrotalcite modified with sodium terephthalate is directly added to the modifier for use.
[0080] Example 8
[0081] A road joint repair treatment method is carried out according to the method in Example 4, except that when the hydrotalcite is modified, the hydrotalcite is not modified by sodium phthalate, and the hydrotalcite is directly mixed with a silane coupling agent to obtain the modified hydrotalcite.
[0082] Example 9
[0083] A road joint repair method is carried out according to the method in Example 1, except that in step S1, after adding the fluorocarbon resin, 20 kg of versatate, 12 kg of EVA emulsion and 4 kg of vinyl triethoxysilane are also added, and then the temperature regulating microcapsules are added after mixing.
[0084] Example 10
[0085] A road joint repair method is carried out according to the method in Example 1, except that in step S1, after adding the fluorocarbon resin, 15 kg of versatate, 8 kg of EVA emulsion and 3 kg of vinyl triethoxysilane are also added, and then the temperature regulating microcapsules are added after mixing.
[0086] Embodiment 11
[0087] A road joint repair method is carried out according to the method in Example 1, except that in step S1, after adding the fluorocarbon resin, 30 kg of versatate, 15 kg of EVA emulsion and 5 kg of vinyl triethoxysilane are also added, and then the temperature regulating microcapsules are added after mixing.
[0088] Example 12
[0089] A road joint repair treatment method is carried out according to the method in Example 9, except that vinyl triethoxysilane is not added.
[0090] Comparative Example 1
[0091] A road joint repair method is carried out according to the method in Example 1, except that steps S1 and S2 are not performed, and emulsified asphalt is directly spread in step S3.
[0092] Comparative Example 2
[0093] A road joint repair method is carried out according to the method in Example 1, except that no temperature-regulating microcapsules are added in step S1, and 40 minutes are required to demulsify the emulsified asphalt in the modified bonding material in step S3.
[0094] Comparative Example 3
[0095] A road joint repair method is carried out according to the method in Example 1, except that no fluorocarbon resin is added in step S1.
[0096] Comparative Example 4
[0097] A road joint repair method is carried out according to the method in Example 1, except that the temperature-regulating microcapsules in step S1 are the temperature-regulating microcapsules prepared in Comparative Preparation Example 1.
[0098] Comparative Example 5
[0099] A road joint repair method is carried out according to the method in Example 1, except that the temperature-regulating microcapsules in step S1 are the temperature-regulating microcapsules prepared in Comparative Preparation Example 2.
[0100] Comparative Example 6
[0101] A road joint repair method is carried out according to the method in Example 1, except that in step S1, an equal amount of temperature regulating microcapsules is replaced by polyurea.
[0102] Performance Testing
[0103] According to the methods in the above embodiments and comparative examples, the road is milled and the joints are treated and the water-stabilizing layer is backfilled. After backfilling and maintenance, the waterproof performance and crack resistance of the repaired water-stabilizing layer are tested, so as to examine the waterproof performance and crack resistance of the joint repair treatment method of the present application. The test of waterproof performance is mainly to simulate rainwater on the surface of the water-stabilizing layer for 3 hours and then let it stand for 3 hours to test the penetration depth. In addition, the water-stabilizing layer that has not been milled and re-paved is taken for penetration depth detection as a control group. The crack resistance is tested by the ring method. In addition, the compressive strength of the water-stabilizing layer after backfilling is tested for 7 days. The test results are shown in Table 1 below.
[0104] Table 1:
[0105]
[0106] The penetration depth of the control group was 25 mm, and the cracking time was 50 h. Referring to the test results of Examples 1-3 of the present application, it can be seen that after the joint treatment of the present application, the water-stabilizing layer is backfilled with water-stabilizing layer, and the water-stabilizing layer has excellent waterproof and anti-seepage performance, and excellent crack resistance, which helps to improve the service life of the road. Referring to the test results of Example 1 and Examples 4-6, it can be seen that after the hydrotalcite is modified with sodium terephthalate and a silane coupling agent, the water resistance and strength of the water-stabilizing layer obtained after the joint repair treatment are better, because the hydrotalcite, as an inorganic material, has good waterproof properties, and can effectively fill the tiny gaps at the contact point between the new and old pavements, prevent water penetration, and improve the waterproof performance of the joints. Moreover, the modified hydrotalcite can form a macromolecular network structure with other raw materials in the bonding material, and can also improve its crack resistance. Combined with the test results of Example 7 and Example 8, in Example 7, the hydrotalcite is only modified with sodium terephthalate, and it can be seen that its waterproof performance and crack resistance are improved compared with Example 1, but weaker than the test results of Example 4. This is because although the modification of sodium terephthalate can introduce rigid groups, the dispersion in the bonding material system is still insufficient, and in Example 8, only the modification of the silane coupling agent is helpful for its dispersion in the system, thereby improving the waterproof performance, but its crack resistance is reduced compared with Example 4.
[0107] Referring to the test results of Examples 1 and 9-11, it can be seen that when tert-butyl vinyl carbonate, EVA emulsion and vinyl triethoxysilane are added to the modifier after fluorocarbon resin, the crack resistance and waterproof performance are significantly improved. Combined with the test results of Example 12, when vinyl triethoxysilane is not added in Example 12, its waterproof performance and crack resistance are significantly reduced compared with Example 9. On the one hand, the introduction of silane groups helps to improve its waterproof performance. On the other hand, vinyl triethoxysilane as a cross-linking agent helps the polymer molecules in the bonding material to form a macromolecular network cross-linking structure, thereby improving its crack resistance.
[0108] Combined with the test results of Example 1 and Comparative Example 1, it can be seen that when the emulsified asphalt is directly spread without modification in Comparative Example 1, the waterproof performance and crack resistance of the replenished water-stabilizing layer are significantly reduced. Referring to Comparative Example 2, when the temperature-regulating microcapsules are not added, the demulsification time is longer, and the final crack resistance is significantly reduced. The longer demulsification time is not conducive to combining with the water-stabilizing filler, resulting in a decrease in its crack resistance; combined with the test results of Comparative Example 3, when the fluorocarbon resin is not added in step S1, the waterproof performance and crack resistance are reduced, especially the waterproof performance is reduced more, and the addition of fluorocarbon resin helps to improve its waterproof performance; referring to the test results of Comparative Examples 4 and 5, when the temperature-regulating microcapsules are prepared, when polyurea or polylactic acid is not added to the wall material, when polyurea is not added to the wall material in Comparative Example 4, demulsification occurs when the modifier and emulsified asphalt are stirred and mixed, which is not conducive to the improvement of subsequent performance, and when polylactic acid is not added in Comparative Example 5, the demulsification time requires 20 minutes, but the subsequent performance improvement is still small. Referring to the test results of Comparative Example 6, when no temperature-regulating microcapsules are added to the modifier but only polyurea is added, it can be seen that the subsequent demulsification time requires more than 30 minutes, and the waterproof performance and crack resistance of the replenished water-stabilizing layer are still poor.
[0109] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A road joint repair method, characterized in that: The following steps are involved: The modified bonding material is spread on the groove wall and groove bottom formed after the road is milled in layers, and water-stable paving and compaction are carried out in the groove after 5-10 minutes. The modified bonding material is obtained by mixing a modifier and emulsified asphalt in a volume ratio of 1: (2.5-3.5); The modifier comprises the following raw materials in parts by weight: 50-70 parts of hydrotalcite, 15-25 parts of anti-cracking fiber, 10-20 parts of fluorocarbon resin and 5-10 parts of temperature-regulating microcapsules; The temperature-regulating microcapsule comprises a core material and a wall material, wherein the core material comprises a mixture of sodium hydroxide and calcium oxide, and the wall material is made of a mixture of polylactic acid, polyurea and gelatin; The temperature-regulating microcapsules are prepared by the following method: Dry granulating sodium hydroxide and calcium oxide to obtain core material particles; Dissolving polylactic acid, polyurea and gelatin in methanol to prepare a coating solution, then spraying the coating solution on the surface of the core material particles, and drying to obtain temperature-adjusting microcapsules, wherein the amount of methanol added is 3-5 times the sum of the amounts of polylactic acid, polyurea and gelatin added; The added mass ratio of sodium hydroxide and calcium oxide is 1: (0.3-0.5); The added mass ratio of polylactic acid, polyurea and gelatin is 1: (0.3-0.5): (0.6-0.8); The added mass ratio of the core material to the wall material is 1:(0.8-1.2).
2. A road joint repair method according to claim 1, characterized in that: The hydrotalcite is added after modification by the following method: The hydrotalcite and ethylene glycol are stirred to obtain a primary mixture, sodium terephthalate is dissolved in water, and then the primary mixture is added, stirred at 80-100° C. for 1-2 hours, filtered and washed with water, and then a silane coupling agent is added to obtain a modified hydrotalcite.
3. A road joint repair method according to claim 2, characterized in that: The mass ratio of the hydrotalcite to ethylene glycol is 1:(0.4-0.6), the mass ratio of the sodium terephthalate to the hydrotalcite is 1:(2-3), the mass ratio of the sodium terephthalate to water is 1:(3-5), and the mass ratio of the silane coupling agent to the hydrotalcite is 1:(3-4).
4. A road joint repair method according to claim 1, characterized in that: The modifier further comprises 15-30 parts by weight of versatate vinyl carbonate, 8-15 parts by weight of EVA emulsion and 3-5 parts by weight of vinyl triethoxy silane.
5. A road joint repair method according to claim 1, characterized in that: The anti-cracking fiber is selected from one or more of steel fiber and basalt fiber.
6. A road joint repair method according to claim 1, characterized in that: The emulsified asphalt is an emulsified asphalt prepared by using a cationic emulsifier.
7. A road joint repair method according to claim 1, characterized in that: The amount of modified bonding material spread on the bottom of the pit is 0.8-1.2kg / m 2 , the spreading amount on the side wall of the pit is 0.3-0.5kg / m 2 .