A silver paste containing a conductive additive on the back of a TOPCon battery and its preparation and application

By using specific formula silver paste on the back of the N-type TOPCon battery, including silver powder, glass powder, conductive additives and organic carriers, combined with high temperature sintering process, the problem of high contact resistance between the silver electrode and the silicon surface is solved, and the efficiency of the battery is improved .

CN118335379BActive Publication Date: 2024-12-06JIANGSU RIYU PHOTOVOLTAIC NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410059260.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2024-12-06
Estimated Expiration
2044-01-16

AI Technical Summary

Technical Problem

The silver electrode on the back of the N-type TOPCon battery has a high contact resistance between the silicon surface and the surface of the silicon, and the ETA efficiency of conductive silver paste in the prior art still needs to be improved.

Method used

Silver paste containing 85% to 90% silver powder, 1.5% to 3.5% glass powder, 0.01% to 1.00% conductive additive and 6% to 13% organic carrier, is prepared by melting, grinding and rolling, combined with screen printing Technology and sintering process reduce the contact resistance between the silver electrode and the silicon surface.

Benefits of technology

The contact resistance between the silver electrode and the silicon surface is significantly reduced, the ETA efficiency is improved, and the design purpose is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a silver paste containing a conductive additive on the back of a TOPCon cell and its preparation and application, belonging to the technical field of crystalline silicon solar cells. The silver paste on the back of the N-type TOPCon cell comprises, by mass fraction, 85% to 90% silver powder, 1.5% to 3.5% glass powder, 0.01% to 1.00% conductive additive, and 6% to 13% organic carrier; the glass powder contains the following components by weight: 17% to 30% bismuth oxide, 25% to 38% lead oxide, 29% to 43% glass former, 4% to 5% alkali metal oxide and alkaline earth metal oxide, and 9% to 12% other oxides. The back silver paste designed by the invention can effectively reduce the contact resistance between the silver electrode and the silicon surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of crystalline silicon solar cells, and in particular to a silver paste containing a conductive additive on the back of a TOPCon cell, and preparation and application thereof. Background Art

[0002] TOPCon (Tunnel Oxide Passivated Contact) is a tunnel oxide passivated contact solar cell technology based on the principle of selective carriers; the back side uses a 1-2nm ultra-thin tunnel oxide and an N+ highly doped polysilicon (Poly-Si) stacked structure deposited on its surface, and the outer layer is further stacked with Al2O3 and a-SiNx:H passivation layer to reduce surface recombination and metal contact recombination, and comprehensively improve the performance of the battery. TOPCon cells have conductive pastes coated on the front and back sides; currently, the silver paste used for the fine grid on the back side of N-type TOPCon crystalline silicon solar cells is mainly composed of silver powder, glass powder, and organic carriers; the glass powder used in the silver paste on the back side plays a key role in corroding the silicon nitride layer, forming an electrode, and building an electron transport bridge. During the metallization process of the battery, the high-temperature sintering of the silver paste can etch the silicon nitride layer on the back side and form contact with the Poly-Si layer.

[0003] The back of the N-type TOPCon and the front of the traditional P-type PERC cell are both N+ doped and use conductive silver paste. However, the front of the P-type PERC monocrystalline cell has a pyramid structure after texturing. This microstructure is conducive to the growth of silver grains under the silver grid line and on the surface of the silicon cell, which helps to reduce the contact resistance between the silver electrode and the silicon surface. The back of the N-type TOPCon usually adopts an alkaline polishing structure, which has no pyramid structure and is a mirror-like polishing surface. This smooth polishing surface is not conducive to the growth of silver grains on the surface of the silicon cell under the silver grid line, so the contact resistance between the silver electrode and the silicon surface is high.

[0004] In the related prior art, patent CN116598043A discloses a conductive silver paste for N-type TOPCon back side grid, but the final result shows that its resistance is still 0.5Ω, and the ETA efficiency is only 25.24%, which still needs to be improved. Patent CN116313213A discloses a conductive silver aluminum paste, and its final data shows that the lowest resistance is 0.422Ω, and the ETA efficiency is 25.10%, which also needs to be further improved. Summary of the invention

[0005] In order to solve the problem of too high contact resistance between the TOPCon back electrode and the silicon surface, the present invention proposes a silver paste for the back of an N-type TOPCon battery and a preparation method and application thereof, which can effectively reduce the contact resistance between the silver electrode and the silicon surface.

[0006] The invention provides an N-type TOPCon battery back silver paste, which comprises, by mass fraction, 85% to 90% of silver powder, 1.5% to 3.5% of glass powder, 0.01% to 1.00% of a conductive auxiliary agent, and 6% to 13% of an organic carrier.

[0007] Preferably, the silver paste on the back side of the N-type TOPCon battery comprises, by mass fraction, 88% to 90% silver powder, 2.1% to 2.5% glass powder, 0.3% to 0.5% conductive additive, and 8% to 9% organic carrier.

[0008] More preferably, the silver paste on the back side of the N-type TOPCon battery comprises, by mass fraction, 88.8% silver powder, 2.3% glass powder, 0.4% conductive additive, and 8.5% organic carrier.

[0009] Furthermore, the glass powder contains the following components by weight: 17% to 30% bismuth oxide, 25% to 38% lead oxide, 29% to 43% glass formers, 4% to 5% alkali metal oxides and alkaline earth metal oxides, and 9% to 12% other oxides.

[0010] Preferably, the glass powder contains the following components by weight: 18% to 29% bismuth oxide, 27% to 37% lead oxide, 29% to 36% glass formers, 4.3% to 4.8% alkali metal oxides and alkaline earth metal oxides, and 9% to 11% other oxides.

[0011] Furthermore, the composition of the glass former includes two or more of silicon oxide, tellurium oxide, boron oxide, and aluminum oxide.

[0012] Preferably, the glass former consists of silicon oxide and tellurium oxide.

[0013] Furthermore, the alkali metal oxide includes one or more of lithium oxide, sodium oxide, and potassium oxide.

[0014] Preferably, the alkali metal oxide is lithium oxide or sodium oxide.

[0015] Furthermore, the alkaline earth metal oxide includes one or more of magnesium oxide, calcium oxide, and strontium oxide.

[0016] Preferably, the alkaline earth metal oxide is magnesium oxide.

[0017] Furthermore, other oxides include one or more of zinc oxide, molybdenum oxide, and tungsten oxide.

[0018] Furthermore, the other oxides are a combination of tungsten oxide and any one or more of zinc oxide, molybdenum oxide and tungsten oxide.

[0019] Preferably, the other oxides are tungsten oxide and zinc oxide.

[0020] Preferably, in the silver paste on the back of the N-type TOPCon battery, the glass powder has a composition by mass fraction of Bi2O3 18.94%, PbO 30.24%, SiO2 7.33%, TeO2 28.11%, Li2O 3.04%, Na2O 1.05%, MgO0.68%, WO3 7.85%, and ZnO 2.76%;

[0021] Or, Bi2O3 28.79%, PbO 27.58%, SiO2 5.94%, TeO2 23.67%, Li2O 2.77%, Na2O0.96%, MgO 0.62%, WO3 7.16%, ZnO 2.51%;

[0022] Or, Bi2O3 18.30%, PbO 36.52%, SiO2 6.29%, TeO2 24.03%, Li2O 2.93%, Na2O1.01%, MgO 0.66%, WO3 7.59%, ZnO 2.66%.

[0023] More preferably, in the silver paste on the back of the N-type TOPCon battery, the glass powder has a composition containing Bi2O3 18.30%, PbO 36.52%, SiO2 6.29%, TeO2 24.03%, Li2O 2.93%, Na2O 1.01%, MgO 0.66%, WO3 7.59%, and ZnO 2.66% by mass.

[0024] Furthermore, the conductive additive is a conductive additive that can reduce the contact resistance between the silver electrode and the silicon wafer after the battery is metallized and sintered.

[0025] Furthermore, the conductive aid includes lead acetate, lead salicylate, lead citrate, lead acetylacetonate, lead isooctanoate, lead neodecanoate, bismuth acetate, bismuth salicylate, bismuth citrate, bismuth acetylacetonate, bismuth isooctanoate, bismuth neodecanoate, and one or more of other lead organic compounds, hydrated lead organic compounds, bismuth organic compounds, and hydrated bismuth organic compounds.

[0026] Preferably, the conductive aid is bismuth acetate or a combination of bismuth acetate and lead acetate.

[0027] More preferably, the conductive aid is a combination of bismuth acetate and lead acetate in a mass ratio of 1:1.

[0028] Furthermore, the organic carrier is composed of a solvent, a resin, a thixotropic agent, and other additives.

[0029] Furthermore, the solvent includes at least three of dibutyl phthalate, pineol, butyl carbitol, butyl carbitol acetate, benzyl alcohol, diethylene glycol dibutyl ether, diethylene glycol butyl ether, and alcohol ester twelve; the resin includes at least two of ethyl cellulose, CAB, PVB, acrylic resin, and rosin resin; other additives include silicone oil, dispersant, and leveling agent.

[0030] Furthermore, the organic carrier is prepared by mixing 5-10% of acrylic resin, 1-5% of ethyl cellulose, and 80-90% of pinene alcohol, diethylene glycol monobutyl ether, and diethylene glycol butyl ether acetate.

[0031] The present invention also provides a method for preparing the silver paste on the back side of the N-type TOPCon battery, comprising the following steps:

[0032] The glass powder components are mixed and melted at 900-1300°C, then quenched to 20-30°C, ground and pulverized, and dried to obtain glass powder; the glass powder, conductive additive, and silver powder are then added to an organic carrier, stirred to obtain a mixture, and then the mixture is rolled and ground to obtain silver paste on the back of an N-type TOPCon battery.

[0033] Furthermore, the particle size of the pulverized glass powder is 1 μm to 3 μm.

[0034] Furthermore, the rolling and grinding time is 10 to 120 minutes; the rolling and grinding time can be determined according to the quality of the mixture. The larger the amount of the mixture, the longer the grinding time, and the smaller the amount of the mixture, the shorter the grinding time.

[0035] Application of the silver paste on the back side of an N-type TOPCon battery provided by the present invention in the battery field.

[0036] The present invention also provides a glass powder, comprising the following components by weight: 17% to 30% bismuth oxide, 25% to 38% lead oxide, 29% to 43% glass formers, 4% to 5% alkali metal oxides and alkaline earth metal oxides, and 9% to 12% other oxides.

[0037] Furthermore, the composition of the glass former includes two or more of silicon oxide, tellurium oxide, boron oxide, and aluminum oxide.

[0038] Furthermore, the alkali metal oxide includes one or more of lithium oxide, sodium oxide, and potassium oxide.

[0039] Furthermore, the alkaline earth metal oxide includes one or more of magnesium oxide, calcium oxide, and strontium oxide.

[0040] Furthermore, other oxides include one or more of zinc oxide, molybdenum oxide, and tungsten oxide.

[0041] The glass powder provided by the invention is used in the field of preparing conductive silver paste.

[0042] The present invention also provides a method for preparing a TOPCon battery, comprising the following steps:

[0043] The silver paste on the back of the N-type TOPCon battery is printed onto a silicon wafer substrate by screen printing technology, and then dried, and then sintered at 750-850° C. and cooled after sintering to obtain a TOPCon battery.

[0044] The present invention provides a TOPCon battery prepared according to the method.

[0045] Beneficial Effects

[0046] Due to the special pyramid-free surface structure on the back of TOPCon, which is similar to a mirror, it is difficult to establish a low contact resistance. Therefore, after matching the glass and the lead and bismuth organic compounds, the contact resistance between the silver electrode and the silicon wafer is significantly reduced, and the efficiency is improved. The design purpose is achieved. DETAILED DESCRIPTION

[0047] Test Method

[0048] The battery efficiency of the prepared battery was tested using a HALM IV tester, and the contact resistance was tested using a TLM contact resistance tester.

[0049] Example 1

[0050] The mixture was mixed according to the formula in Tables 1 and 2, melted at 900-1300°C, and then quenched to about 25°C. The obtained material was then crushed to a particle size of 1 μm to 3 μm using a planetary grinder and dried to obtain a uniform glass powder.

[0051] If the conductive agent (ie, lead organic compound, bismuth organic compound) is solid, it should be crushed by planetary mill to obtain a conductive agent with a particle size of 0.5 to 2 μm. If the conductive agent is liquid, it can be directly poured in.

[0052] The organic carrier is a mixture of 7% acrylic resin, 3% ethyl cellulose, 90% pineol, diethylene glycol monobutyl ether and diethylene glycol butyl ether acetate.

[0053] Add glass powder, conductive additive and silver powder to the organic carrier and stir thoroughly to form a mixture. Use a three-roll grinder to repeatedly roll the paste composition and grind it into a conductive paste. Then use screen printing technology to print the conductive paste on the silicon wafer substrate. Dry the cell in an infrared drying oven, then pass it through a belt sintering furnace, sinter it at 800°C, and cool it after sintering to form a battery.

[0054] Table 1 Detailed formula of glass (weight %)

[0055]

[0056] Table 2 Glass composition by functional oxide (weight %)

[0057]

[0058]

[0059] Example 2

[0060] Table 3 Test results of glass formulations G1 to G4

[0061] Element P1 P2 P3 P4 P5 P6 P7 P8 G1 2.3% 2.3% G2 2.3% 2.3% G3 2.3% 2.3% G4 2.3% 2.3% Bismuth acetate 0.4% 0.4% 0.4% 0.4% organic 8.5% 8.5% 8.5% 8.5% 8.5% 8.5% 8.5% 8.5% Silver powder 89.2% 89.2% 89.2% 89.2% 88.8% 88.8% 88.8% 88.8% total 100.0% 100.0% 100.0% 100.0% 100.0% 100.0% 100.0% 100.0% Contact resistance(Ω) 1.12 0.48 0.42 0.53 0.55 0.32 0.36 0.65 Eta(%) 23.43 25.23 25.41 25.10 25.08 25.64 25.52 24.88

[0062] P1 to P4 do not have conductive additives, while P5 to P8 have conductive additives. The corresponding slurries after adding conductive additives to P1, P2, P3, and P4 are P5, P6, P7, and P8. It can be seen that after adding additives to G1, G2, and G3, the contact resistance decreases and the efficiency increases. However, after adding conductive additives to G4, the contact resistance deteriorates and the efficiency decreases.

[0063] Example 3

[0064] Table 4 Test results of G5-G6 glass formula

[0065] Element P9 P10 P11 P12 G5 2.3% 2.3% G6 2.3% 2.3% Lead acetate 0.4% 0.4% organic 8.5% 8.5% 8.5% 8.5% Silver powder 89.2% 89.2% 88.8% 88.8% total 100.0% 100.0% 100.0% 100.0% Contact resistance(Ω) 0.53 0.46 0.45 0.34 Eta(%) 25.06 25.34 25.39 25.59

[0066] P9-P10 has no conductive additive, while P11-P12 has conductive additive. The corresponding slurries after adding conductive additive to P9 and P10 are P11 and P12. It can be seen that after adding additive to G5 and G6, the resistance is reduced and the efficiency is increased.

[0067] Example 4

[0068] Table 5 Test results of G6 glass formula

[0069] Element P10 P12 P13 P14 G6 2.3% 2.3% 2.3% 2.3% Bismuth acetate 0.20% Lead acetate 0.4% 0.20% 0.1% organic 8.5% 8.5% 8.5% 8.5% Silver powder 89.2% 89.0% 88.8% 89.1% total 100.0% 100.2% 100.0% 100.0% Contact resistance(Ω) 0.46 0.34 0.30 0.41 Eta(%) 25.34 25.59 25.77 25.44

[0070] G6 added different conductive additives, the contact resistance was reduced, and the efficiency was increased. P13 added two additives, and the efficiency gain was the largest. P14 added 0.1 conductive additives, and the efficiency gain was also obvious.

[0071] Example 5

[0072] Table 6 Test results of G7-G8 glass formulations

[0073] Element P15 P16 P17 P18 G7 2.3% 2.3% G8 2.3% 2.3% Bismuth acetate 0.4% 0.4% organic 8.5% 8.5% 8.5% 8.5% Silver powder 89.2% 89.2% 88.8% 88.8% total 100.0% 100.0% 100.0% 100.0% Contact resistance(Ω) 0.56 0.52 0.60 0.39 Eta(%) 25.03 25.14 24.97 25.47

[0074] After adding conductive additives to G7 (P15) (P17), the contact resistance became worse and the efficiency decreased, indicating that the glass must contain tungsten oxide. After adding conductive additives to G8 (P16) (P18), the contact resistance became lower and the efficiency increased, indicating that ZnO is not a necessary oxide.

[0075] Table 7 Test results of G9-G10 glass formula

[0076]

[0077]

[0078] The efficiencies of G9 and G10 are relatively low, indicating that CuO and TiO2 are not suitable for this glass system.

[0079] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. A silver paste for the back side of an N-type TOPCon battery, characterized in that: Its composition includes 85% to 90% silver powder, 1.5% to 3.5% glass powder, 0.01% to 1.00% conductive additive, and 6% to 13% organic carrier by mass fraction; The composition of the glass powder is as follows: Bi2O3 18.94%, PbO30.24%, SiO2 7.33%, TeO2 28.11%, Li2O3.04%, Na2O1.05%, MgO0.68%, WO3 7.85%, ZnO2.76% by mass fraction; or, Bi2O328.79%, PbO27.58%, SiO25.94%, TeO223.67%, Li2O2.77%, Na2O0.96%, MgO0.62%, WO37.16%, ZnO2.51%; or, Bi2O318.30%, PbO36.52%, SiO26.29%, TeO224.03%, Li2O2.93%, Na2O1.01%, MgO0.66%, WO37.59%, ZnO2.66%; The conductive auxiliary agent is bismuth acetate or a combination of bismuth acetate and lead acetate.

2. The silver paste on the back side of the N-type TOPCon battery according to claim 1, characterized in that: The composition of the silver paste on the back of the N-type TOPCon battery includes, by mass fraction, 88% to 90% silver powder, 2.1% to 2.5% glass powder, 0.3% to 0.5% conductive additive, and 8% to 9% organic carrier.

3. The silver paste on the back side of the N-type TOPCon battery according to claim 1, characterized in that: The organic carrier is composed of solvent, resin, thixotropic agent and other additives; the solvent includes at least three of dibutyl phthalate, pineol, butyl carbitol, butyl carbitol acetate, benzyl alcohol, diethylene glycol dibutyl ether, diethylene glycol butyl ether and alcohol ester; the resin includes at least two of ethyl cellulose, CAB, PVB, acrylic resin and rosin resin; other additives include silicone oil, dispersant and leveling agent.

4. Application of the silver paste on the back side of an N-type TOPCon battery according to any one of claims 1 to 3 in the battery field.

5. The method for preparing the silver paste on the back side of an N-type TOPCon battery according to any one of claims 1 to 3, characterized in that: The following steps are involved: The glass powder components are mixed and melted at 900~1300℃, then suddenly cooled to 20~30℃, then ground and crushed, and dried to obtain glass powder; then the glass powder, conductive additive, and silver powder are added to an organic carrier, stirred to obtain a mixture, and then the mixture is rolled and ground to obtain the silver paste on the back of the N-type TOPCon battery.

6. A method for preparing a TOPCon battery, characterized in that: The following steps are involved: The silver paste on the back of the N-type TOPCon battery as claimed in any one of claims 1 to 3 is printed onto a silicon wafer substrate by screen printing technology, and then dried, and then sintered at 750 to 850° C. and cooled after sintering to obtain a TOPCon battery.