A photosensitive resin composition and its preparation method and application
By using components such as multifunctional polyurethane acrylate and aliphatic urethane in the photosensitive resin, combined with reactive diluents and fillers, the problem of excessive viscosity of the photosensitive resin is solved, and the accuracy and mechanical properties of the dental model are improved. Efficient 3D printing effects are achieved.
Patent Information
- Application Number
- CN202410761264.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2044-06-13
AI Technical Summary
The viscosity of existing photosensitive resins for 3D printing is too high, which affects the printing efficiency and the accuracy and mechanical properties of dental models.
Using components such as multifunctional polyurethane acrylate and aliphatic urethane dimethacrylate, combined with reactive diluents, fillers, initiators and antioxidants, the viscosity and mechanical properties of the photosensitive resin are adjusted to form a suitable form for 3D printing photosensitive resin composition.
It improves the accuracy and mechanical properties of the dental model, reduces the viscosity, enhances the printing efficiency and the strength and hardness of the product, and is suitable for making dental models.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of 3D printing, and in particular to a photosensitive resin composition and a preparation method and application thereof. Background Art
[0002] In recent years, digital technology has developed rapidly, among which 3D printing digital light processing technology (Digital Light Processing, DLP) has been increasingly used in the field of oral implant restoration, such as 3D printing implant guides, casting models, dental restoration working models, temporary crowns, bridges, veneers, etc. With the development of 3D printing and polymer material technology, the technology of DLP printing to directly produce permanent restorations has also been improved to a certain extent. Due to the complex shape of prosthesis, it is a typical personalized customized product, which is particularly suitable for direct printing and molding with 3D printing technology. For traditional denture, crown and bridge cutting and processing technology, the CAD / CAM cutting system wastes raw materials seriously, and there are disadvantages such as tool wear and dust pollution. 3D printing has the advantages of high molding accuracy, high material utilization, low cost, short production cycle, and environmental protection, and is increasingly attracting attention in the field of oral restoration. Many manufacturers have successively launched photosensitive resins for 3D printing, which are used to directly print and produce permanent crowns and bridges.
[0003] The main disadvantages of photosensitive resins for 3D printing are: in order to achieve strength and hardness comparable to ceramic crowns, excessive inorganic fillers and high-viscosity oligomers are added to the resin, resulting in excessive resin viscosity. Excessive viscosity affects the leveling rate of the resin, thereby reducing printing efficiency. In addition, excessive viscosity makes it difficult to clean the printed crowns, and excessive inorganic fillers are also precipitated during the printing and cleaning process due to dispersion problems, affecting the accuracy of the crowns. How to reduce the viscosity of photosensitive resins while ensuring that the dental models produced have good mechanical properties is an urgent problem to be solved. Summary of the invention
[0004] The main purpose of the present invention is to provide a photosensitive resin composition and a preparation method and application thereof, so as to solve the problem in the prior art that the photosensitive resin has high viscosity and cannot balance the processing performance, precision and mechanical properties of the dental model.
[0005] In order to achieve the above object, according to a first aspect of the present invention, a photosensitive resin composition is provided, which comprises the following components in parts by weight: 5-20 parts of multifunctional polyurethane acrylate, 30-60 parts of aliphatic urethane dimethacrylate, 1-40 parts of reactive diluent, 5-30 parts of filler, 1-5 parts of initiator, 0.05-1 parts of antioxidant, and 0.01-1 parts of ultraviolet absorber; the functionality of the multifunctional polyurethane acrylate is ≥3, and the functionality of the aliphatic urethane dimethacrylate is ≤2.
[0006] Multifunctional polyurethane acrylate can greatly improve the mechanical properties of the photosensitive resin composition; aliphatic carbamate dimethacrylate can control the viscosity of the system while improving the mechanical properties, which is beneficial for subsequent processing; reactive diluents can reduce the viscosity of the photosensitive resin composition and help improve the cross-linking performance; fillers are of great help in improving the strength and hardness of products printed from the photosensitive resin composition; initiators can promote the cross-linking polymerization reaction; antioxidants and ultraviolet absorbers can effectively improve the anti-aging properties of the photosensitive resin composition and improve its stability. By limiting the components of the photosensitive resin composition and the amount of each component, the photosensitive resin composition can have good processing properties, is suitable for 3D printing, and can produce high-precision products. In addition, the strength and hardness of the products printed from the photosensitive resin composition are high, and are suitable for making dental models.
[0007] Furthermore, the functionality of the multifunctional polyurethane acrylate is 3-6.
[0008] Furthermore, the multifunctional polyurethane acrylate includes at least one of CN8898 NS, CN9245, CN929, CN989 NS, CN8007 NS, CN8000 NS, CN9110 NS, and CN8885 NS; the aliphatic urethane dimethacrylate includes at least one of GENOMER 4297, GENOMER 4256, GENOMER 4205, CN1963CG, CN1993CG, and CN2254NS.
[0009] Further, the active diluent includes at least one of cyclotrimethylolpropane formal acrylate, isobornyl methacrylate, isobornyl acrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, ethoxylated bisphenol A dimethacrylate, tricyclodecane dimethanol diacrylate, trimethylolpropane triacrylate, and ethoxylated trimethylolpropane triacrylate.
[0010] Using the above ingredients as active diluents can improve the dispersion uniformity of each component, promote the cross-linking reaction, and improve the comprehensive performance of the product.
[0011] Furthermore, the filler includes at least one of silicon dioxide, zirconium oxide, aluminum oxide, halloysite nanotubes, and carbon nanotubes.
[0012] Furthermore, the initiator includes at least one of (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide, (2,4,6-trimethylbenzoyl)-phenylphosphonic acid ethyl ester, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, camphorquinone, and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.
[0013] Furthermore, the antioxidant includes at least one of an amine antioxidant and a phenolic antioxidant; and the ultraviolet absorber includes at least one of a benzophenone ultraviolet absorber and a triazine ultraviolet absorber.
[0014] Furthermore, the components of the photosensitive resin composition also include 0.01-3 parts of a coloring additive, and the coloring additive is titanium dioxide.
[0015] Furthermore, among the components of the photosensitive resin composition, the weight parts of multifunctional polyurethane acrylate are 5-10, the weight parts of aliphatic urethane dimethacrylate are 40-55, the weight parts of reactive diluent are 20-25, the weight parts of filler are 10-20, and the weight parts of initiator are 1.5-2.
[0016] According to the second aspect of the present invention, there is provided a method for preparing the photosensitive resin composition of the first aspect of the present invention, the preparation method comprising: mixing the components according to a proportion, stirring to obtain a photosensitive resin composition; the stirring speed is 500-2000 rpm, the time is 2-6h, and the temperature is 40-70°C.
[0017] According to a third aspect of the present invention, there is provided an application of the photosensitive resin composition of the first aspect of the present invention in the field of 3D printing of dental restoration models, such as 3D printing to prepare crowns.
[0018] By applying the technical solution of the present invention, the addition of aliphatic urethane dimethacrylate and multifunctional polyurethane acrylate can improve the strength and hardness of the dental model 3D printed by the photosensitive resin composition, and make it have good toughness, and the dispersion uniformity and viscosity of the photosensitive resin composition can be improved by adding a reactive diluent, and the strength and hardness of the 3D printed dental model can be further improved by adding fillers. The present invention limits the components of the photosensitive resin composition and the weight of each component to make it have good comprehensive performance, and the dental model prepared by the photosensitive resin composition has high precision and mechanical properties. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0020] As described in the background technology of the present invention, DLP builds models by stacking photosensitive resin materials layer by layer, which can be used for tooth restoration, implantation, orthodontic treatment, custom dentures, dental education, etc. Dentures, crowns and bridges, and veneers made by 3D printing can adapt to the patient's oral environment with high precision and high efficiency, which is convenient for dentists to make more accurate diagnosis and treatment; compared with traditional CAD / CAM cutting processes, 3D printing technology has higher precision, shorter production cycle and lower material waste. However, the current 3D printed dentures, crowns and bridges, and veneer resin materials have problems with viscosity, hardness and toughness that are difficult to balance. In order to solve the above technical problems, in a typical embodiment of the present invention, a photosensitive resin composition is provided, which comprises the following components in parts by weight: 5-30 parts of multifunctional polyurethane acrylate, 10-60 parts of aliphatic carbamate dimethacrylate, 1-60 parts of active monomers, 1-70 parts of fillers, 1-5 parts of initiators, 0.05-1 parts of antioxidants, and 0.01-2 parts of ultraviolet absorbers; the functionality of the multifunctional polyurethane acrylate is ≥3, and the functionality of the aliphatic carbamate dimethacrylate is ≤2.
[0021] Multifunctional polyurethane acrylate has excellent weather resistance, yellowing resistance, and wear resistance, and has high bending strength. It can react with photoinitiators to achieve rapid photocuring. Aliphatic carbamate dimethacrylate has high mechanical strength and high elongation at break, and it can be rapidly photocured. It has strong adhesion to the tooth surface and can improve the bonding strength and durability of the restorative material. The compounding of multifunctional polyurethane acrylate and aliphatic carbamate dimethacrylate can synergistically improve the mechanical properties of the dental model made from the photosensitive resin composition. Reactive diluents can be used to adjust the viscosity, fluidity and curing speed of the photosensitive resin composition to improve the printing quality; fillers can further improve the strength and hardness of the dental model; initiators can decompose under light conditions to produce active intermediates, prompting the start of the photocuring reaction; antioxidants and ultraviolet absorbers can improve the anti-aging properties of the photosensitive resin composition. By limiting the components of the photosensitive resin composition and the weight of each component as above, the photosensitive resin composition can have a suitable viscosity, and the models of dentures, crown bridges, veneers, etc. made from the photosensitive resin composition have high mechanical properties and good precision.
[0022] In a preferred embodiment of the present invention, the functionality of the multifunctional polyurethane acrylate is 3-6.
[0023] In a preferred embodiment of the present invention, the multifunctional polyurethane acrylate includes at least one of CN8898 NS, CN9245, CN929, CN989 NS, CN8007 NS, CN8000 NS, CN9110 NS, and CN8885 NS of Sartomer; the aliphatic urethane dimethacrylate includes at least one of GENOMER 4297, GENOMER 4256, GENOMER 4205 of Ruian Company and CN1963CG, CN1993CG, and CN2254NS of Sartomer.
[0024] The compound of the multifunctional polyurethane acrylate and aliphatic urethane dimethacrylate has better mechanical properties, which helps to further improve the comprehensive performance of the dental model.
[0025] In a preferred embodiment of the present invention, the number average molecular weight of the multifunctional polyurethane acrylate is 100-5000, and the number average molecular weight of the aliphatic urethane dimethacrylate is 200-5000.
[0026] The above-mentioned limitation on the number average molecular weight of the multifunctional polyurethane acrylate can reduce the viscosity of the photosensitive resin composition while ensuring that the product has good mechanical properties. The resin composition has a fast leveling speed, good processing performance, and the obtained dental model has high precision.
[0027] In a preferred embodiment of the present invention, the active diluent includes at least one of cyclotrimethylolpropane formal acrylate, isobornyl methacrylate, isobornyl acrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, ethoxylated bisphenol A dimethacrylate, tricyclodecane dimethanol diacrylate, trimethylolpropane triacrylate, and ethoxylated trimethylolpropane triacrylate.
[0028] The above-mentioned active diluent improves the viscosity of the photosensitive resin composition without having a significant impact on the mechanical properties of the product, and helps to improve the crosslinking performance of the photosensitive resin composition, increase the crosslinking reaction rate, and also helps to improve the flexibility of the dental model printed by the photosensitive resin composition.
[0029] Typically, but not limiting, the filler includes at least one of silica, zirconia, alumina, halloysite nanotubes, and carbon nanotubes.
[0030] Silicon dioxide has good stability, high hardness, wear resistance and compressive strength, and is suitable for use as a filler to improve the mechanical properties of resins. Zirconium oxide has the characteristics of high melting point (about 2700°C), high hardness, high wear resistance, good thermal stability, chemical stability and biocompatibility, and is suitable for preparing dental models. Aluminum oxide has high hardness, which is of great help in improving the wear resistance of products prepared from photosensitive resin compositions. Halloysite nanotubes have good biocompatibility, and their surface carries a negative charge, which can form a good interaction with polymers, and at the same time can improve the mechanical properties and thermal stability of the material. Carbon nanotubes have extremely high strength and modulus, and can significantly improve the mechanical properties of composite materials, such as tensile strength, flexural strength and fracture toughness. The above fillers are all commonly used materials to improve the mechanical properties of resin materials and are easy to obtain.
[0031] In a preferred embodiment of the present invention, the D50 particle size of silicon dioxide, zirconium oxide and aluminum oxide is 5-500 nm, the diameter of halloysite nanotubes and carbon nanotubes is 1-100 nm, and the aspect ratio is 1000-20000.
[0032] By optimizing the performance parameters of the filler, the strength and hardness of the dental model prepared from the photosensitive resin composition can be increased while improving its toughness.
[0033] Typically, but not limiting, the initiator includes at least one of (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide, (2,4,6-trimethylbenzoyl)-phenylphosphonic acid ethyl ester, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, camphorquinone, and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.
[0034] The above-mentioned initiator has good photo-initiating performance, can promote the rapid photocuring reaction and improve production efficiency.
[0035] Typically, but not limiting, the antioxidant includes at least one of an amine antioxidant and a phenolic antioxidant; wherein the amine antioxidant is at least one of octylated diphenylamine, N-isopropyl-N′-phenyl-p-phenylenediamine, N,N′-bis(1,4-dimethylpentyl)-p-phenylenediamine, N-(p-toluenesulfonyl)-N′-phenyl-p-phenylenediamine, 2,2,6,6-tetramethylpiperidine, etc. and derivatives thereof; the phenolic antioxidant is at least one of antioxidant 1076, antioxidant 1010, antioxidant 264, antioxidant 545, antioxidant 590, etc. and derivatives thereof.
[0036] Amine antioxidants slow down the rate of oxidation reaction by capturing free radicals and oxygen molecules, thus maintaining the quality and stability of the product; phenolic antioxidants resist oxidation by capturing free radicals and inhibiting oxidation reactions. The above-mentioned amine antioxidants and phenolic antioxidants can slow down the aging rate of resins and are easy to obtain.
[0037] Typically, but not limiting, the UV absorber includes at least one of a benzophenone UV absorber and a triazine UV absorber. Among them, the benzophenone UV absorber is at least one of 2-hydroxy-4-n-octyloxybenzophenone (UV-531), 2,4-dihydroxybenzophenone (UV-0), 2-hydroxy-4-methoxybenzophenone (UV-9), etc. and their derivatives; the triazine UV absorber is at least one of 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-octyloxyphenol (UV-1164), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol (UV-1577), UV-1990, etc. and their derivatives.
[0038] Benzophenone UV absorbers can absorb ultraviolet rays and convert them into heat energy, thereby protecting the resin; triazine UV absorbers have the same effect. The above two types of UV absorbers can significantly slow down the aging rate of the resin and increase its service life.
[0039] In a preferred embodiment of the present invention, the components of the photosensitive resin composition further include 0.01-3 parts of a coloring additive, which is titanium dioxide. Titanium dioxide has a high refractive index, high whiteness, light resistance, weather resistance and non-toxicity, and is suitable for preparing dental models.
[0040] In a preferred embodiment of the present invention, among the components of the photosensitive resin composition, the weight parts of multifunctional polyurethane acrylate are 5-10, the weight parts of aliphatic urethane dimethacrylate are 40-55, the weight parts of reactive diluent are 20-25, the weight parts of filler are 10-20, and the weight parts of initiator are 1.5-2.
[0041] The weight of each component in the photosensitive resin composition has a great influence on its viscosity and mechanical properties. By making the above selection of the weight of multifunctional polyurethane acrylate, aliphatic urethane dimethacrylate, reactive diluent, filler and initiator, the prepared photosensitive resin composition has a suitable viscosity, good leveling performance, high printing efficiency, and the obtained dental models such as crowns are also of high precision; at the same time, its strength, hardness and toughness are also high, and it has good comprehensive performance.
[0042] In another typical embodiment of the present invention, a method for preparing the photosensitive resin composition of the above embodiment is provided, and the preparation method is: mixing the components according to a ratio, stirring, and obtaining a photosensitive resin composition; wherein the stirring speed is 500-2000 rpm, that is, providing a shear line speed of 0.087-0.35 m / s, the stirring time is 2-6 h, and the stirring temperature is 40-70°C.
[0043] The preparation method is simple, and the obtained photosensitive resin composition has good uniformity, is suitable for 3D printing, and can prepare dental models with high strength and high hardness.
[0044] In another typical embodiment of the present invention, there is provided an application of the photosensitive resin composition in the above embodiment of the present invention in the field of 3D printing dental restoration models, such as 3D printing crowns.
[0045] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0046] Fillers: Silica AEROSIL®OX 50 (Evonik, 40nm), zirconium oxide XFI01 (Xianfeng Nano, 20-40nm), aluminum oxide XFI09 (Xianfeng Nano, 150-500nm), halloysite nanotubes XFI50 (Xianfeng Nano, diameter 50-300nm, length 1-10μm), carbon nanotubes XFD01 (Xianfeng Nano, diameter 2-4nm, length 50μm).
[0047] Examples 1-5
[0048] The embodiments of the photosensitive resin composition of the present invention, the components of embodiments 1-5 are shown in Table 1, and the preparation method is as follows:
[0049] The components were added into a stirring and dispersing kettle in sequence, the rotation speed was adjusted to 1000 r / min, the temperature was controlled to 50° C., and the mixture was stirred and dispersed for 4 hours to obtain the photosensitive resin composition described in Examples 1-5.
[0050] Comparative Example 1-2
[0051] Comparative Example 1-2 is a photosensitive resin composition. The components of Comparative Example 1-2 are shown in Table 1, and the preparation method is the same as that of Example 1-5.
[0052] Table 1 (parts by weight)
[0053]
[0054]
[0055] Performance Testing
[0056] 1. The photosensitive resin compositions in the embodiments and comparative examples were subjected to viscosity tests, with reference to GB / T 2794-2022 "Determination of viscosity of adhesives". The test temperature was 25° C. The test results are recorded in Table 2.
[0057] Table 2
[0058]
[0059] 2. The flexural strength and bending modulus of the crown and bridge materials prepared in the examples and comparative examples were tested with reference to YY 0710-2009 “Polymer-based crown and bridge materials for dentistry”. The test results are recorded in Table 3.
[0060] 4. Referring to GB / T 2411-2008 “Determination of indentation hardness (Shore hardness) of plastics and hard rubber using a hardness tester”, hardness tests were performed on the samples prepared in the embodiments and comparative examples. The test results are recorded in Table 3.
[0061] 5. The samples prepared in the embodiments and comparative examples were tested for wear resistance according to YY / T 0113-2015 “Test Method for Wear Resistance of Composite Resins in Dentistry”. The test results are recorded in Table 3.
[0062] 6. The total fracture work of the samples prepared in the examples and comparative examples was calculated with reference to YY 0270.1-2011 “Dental Base Polymers”. The test results are recorded in Table 3.
[0063] The curing method of the sample is as follows: the model is printed and cleaned on the AccuFab D1s equipment of Xinlin 3D, and then cured in a curing box (light source: 405nm, power: 40mW / cm 2 ) Curing for 10 minutes.
[0064] Table 3
[0065]
[0066] From the above test results, it can be seen that the samples prepared in Examples 1-5 have high flexural strength, are not easy to break in a bent state, have high flexural modulus, and have strong ability to resist deformation; and have high hardness, wear resistance, and good toughness, and are suitable for 3D printing to prepare dental models such as crowns. The components of the resin composition in Comparative Examples 1-2 are not within the scope defined by the present invention, and its viscosity is high, and the processing performance is relatively poor. The wear resistance and toughness of the prepared samples are obviously inferior to those of the present invention.
[0067] In addition, by comparing the test results of Examples 1-5, it can be found that when the components of the photosensitive resin composition meet the following conditions: the weight parts of the multifunctional polyurethane acrylate are 5-10, the weight parts of the aliphatic urethane dimethacrylate are 40-55, the weight parts of the reactive diluent are 20-25, the weight parts of the filler are 10-20, and the weight parts of the initiator are 1.5-2, the viscosity is below 900 mPa·s, the flexural strength is above 140 MPa, the flexural modulus is higher than 5500 MPa, and the abrasion loss is below 0.15 mm. 3 Below, the total fracture work is 1200J / m 2 The above has more outstanding comprehensive performance.
[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A photosensitive resin composition, characterized in that: The invention comprises the following components in parts by weight: 5-10 parts of multifunctional polyurethane acrylate, 40-55 parts of aliphatic carbamate dimethacrylate, 20-25 parts of reactive diluent, 10-20 parts of filler, 1.5-2 parts of initiator, 0.05-1 parts of antioxidant and 0.01-1 parts of ultraviolet absorber; the functionality of the multifunctional polyurethane acrylate is 3-6; the reactive diluent comprises cyclotrimethylolpropane methylal acrylate, isobornyl methacrylate, isobornyl acrylate, dipropylene glycol diacrylate and tripropylene glycol diacrylate. The initiator comprises at least one of ester, hydroxyethyl methacrylate, hydroxypropyl methacrylate, ethoxylated bisphenol A dimethacrylate, tricyclodecane dimethanol diacrylate, trimethylolpropane triacrylate, and ethoxylated trimethylolpropane triacrylate; the initiator comprises at least one of (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide, (2,4,6-trimethylbenzoyl)-phenylphosphonic acid ethyl ester, phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide, camphorquinone, and 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.
2. The photosensitive resin composition according to claim 1, characterized in that: The multifunctional polyurethane acrylate includes at least one of CN8898 NS, CN9245, CN929, CN989 NS, CN8007 NS, CN8000 NS, CN9110 NS, and CN8885 NS; the aliphatic urethane dimethacrylate includes at least one of GENOMER 4297, GENOMER 4256, GENOMER 4205, CN1963CG, CN1993CG, and CN2254NS.
3. The photosensitive resin composition according to claim 1, characterized in that: The filler includes at least one of silicon dioxide, zirconium oxide, aluminum oxide, halloysite nanotubes, and carbon nanotubes.
4. The photosensitive resin composition according to claim 1, characterized in that: The antioxidant includes at least one of an amine antioxidant and a phenolic antioxidant; the ultraviolet absorber includes at least one of a benzophenone ultraviolet absorber and a triazine ultraviolet absorber.
5. The photosensitive resin composition according to claim 1, characterized in that: The invention also comprises 0.01-3 parts of a coloring additive, wherein the coloring additive is titanium dioxide.
6. A method for preparing a photosensitive resin composition according to any one of claims 1 to 5, characterized in that: The preparation method comprises: mixing the components according to a proportion, stirring, and obtaining the photosensitive resin composition; the stirring speed is 500-2000 rpm, the time is 2-6 hours, and the temperature is 40-70°C.
7. Use of the photosensitive resin composition according to any one of claims 1 to 5 in the field of 3D printing dental restoration models.
Citation Information
Cited By
Photocuring elastomer slurry and preparation method and application thereof
CN119978255A
A photocured elastomer paste, its preparation method and use
CN119978255B
Model resin for additive manufacturing, preparation method of model resin and application of model resin in preparation of dental model through 3D printing
CN122685815A