A high temperature resistant non-combustible coating powder and its preparation method and application

By reacting the modified epoxy resin with aluminum phosphate glue solution and combining flame retardants such as aluminum hydroxide, red phosphorus, triphenylphosphine oxide, etc., the high temperature heat resistance and corrosion problems of powder coatings in insulated packaging of electronic components are solved. The coating powder with non-combustible and high flame retardant properties is suitable for high-precision electronic components.

CN118344790BActive Publication Date: 2024-11-15SUZHOU BOJUN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410775452.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-11-15
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

The existing powder coatings are difficult to meet the high temperature and heat resistance requirements in insulated packaging of electronic components, and the strong alkalinity of traditional flame retardant components can easily lead to corrosive problems.

Method used

The reaction of modified epoxy resin and aluminum phosphate glue solution is used to form a modified epoxy resin with phosphate groups, and combine flame retardants such as aluminum hydroxide, red phosphorus and triphenylphosphine oxide to form a non-combustible coating. Powder reduces the pH value and corrosiveness of the system through the synergistic effect of modified resin, filler and flame retardant, and enhances flexibility and flame retardant effects.

Benefits of technology

It realizes the effect of non-combustible and non-flammable drips at high temperatures, reduces the corrosion of electronic components, is suitable for insulating packaging of high-precision electronic components, and enhances flame retardant performance and flexibility through the use of modified epoxy resin. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high temperature resistant non-combustible coating powder and a preparation method and application thereof. The high temperature resistant non-combustible coating powder includes modified epoxy resin, aluminum hydroxide or silicon dioxide, dicyandiamide, 2-methylimidazole, red phosphorus, triphenylphosphine or triphenylphosphine oxide, phthalocyanine blue, white carbon black, fumed alumina, fumed alumina powder, polyethylene wax, benzoate, titanium dioxide R-219, sodium polyacrylate and leveling agent PV-88. The present invention adopts a high acid aluminum gel solution to directly modify bisphenol A epoxy resin to obtain a modified epoxy resin with a phosphate group, which greatly enhances flexibility and flame retardant effect, avoids cracking and alkali corrosion; by matching flame retardants and modifying epoxy resins, it is completely non-combustible and has no flammable dripping at high temperature, and is particularly suitable for insulating packaging of high-precision electronic components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder coatings, and in particular to a high-temperature resistant non-combustible coating powder and a preparation method and application thereof. Background Art

[0002] Powder coating is a coating process in which a dry, fine powdered coating is sprayed onto a surface and then baked at high temperatures to form a solid coating. Compared with traditional liquid coatings, powder coatings have higher durability, better environmental protection and coating efficiency.

[0003] Powder coatings are widely used in various fields, such as automobiles, furniture, construction, electronics, medical equipment, etc. In the insulation packaging process of electronic components, powder coatings gradually replace the traditional liquid dipping method. Powder coatings have the advantages of no volatile organic compound (VOC) emissions, no harmful substances, and recyclability, making them the first choice for environmentally friendly coatings.

[0004] In addition to meeting basic insulation requirements, the insulation package of electronic components also needs to meet high temperature and heat resistance requirements to adapt to the thermal damage to the packaging bonding point caused by the heating process of the electronic components. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a high temperature resistant non-combustible coating powder and a preparation method and application thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A high temperature resistant non-combustible coating powder comprises the following components in parts by weight:

[0008] 20-50 parts of modified epoxy resin;

[0009] 30-80 parts of filler, including any of aluminum hydroxide, silicon dioxide, aluminum oxide, boron nitride, quartz powder, mica powder, aluminum chloride powder, diamond powder, silicon nitride, expanded graphite, and calcium carbonate;

[0010] 3-7 parts of a curing agent, including dicyandiamide and 2-methylimidazole;

[0011] 2-15 parts of flame retardants, including any of organic phosphates, triphenylphosphine, triphenylphosphine oxide, triethyl phosphate, aluminum hydroxide, zinc borate, antimony trioxide, and red phosphorus;

[0012] 0.2-3 parts of pigment, including any of phthalocyanine blue, iron oxide blue, cobalt blue, cobalt chrome blue, and titanium dioxide R-219;

[0013] 0.1-1 part of a bulking agent, including any of white carbon black, fumed alumina, sodium polyacrylate, vinyl bisstearamide, and dispersant-SMA1112;

[0014] 0.5-3 parts of leveling agent, including any one of leveling agent PV-88, leveling agent BYK-3902P, leveling agent BYK-3933 P, leveling agent BYK-360 P, leveling agent ZY-1099, leveling agent LF-9222, and leveling agent VOK-LP 5400;

[0015] 0.5-5 parts of a brightener, including any of paraffin wax, polyethylene wax, and polyamide wax;

[0016] 1-5 parts of plasticizer, including any of dioctyl phthalate, benzoic acid ester, chlorinated polyethylene, modified polyurethane acrylate resin, AGE epoxy diluent, and n-butyl glycidyl ether.

[0017] A further formulation, a high temperature resistant non-combustible coating powder, comprises the following components in parts by weight:

[0018] 43.7 parts of modified epoxy resin;

[0019] 41 parts of aluminum hydroxide or silicon dioxide, which is the main flame retardant component and also provides an inorganic supporting skeleton;

[0020] 4 parts of dicyandiamide, a latent curing agent;

[0021] 4 parts of 2-methylimidazole, a medium temperature curing agent;

[0022] 1 part of red phosphorus, a flame retardant;

[0023] 3 parts of triphenylphosphine or triphenylphosphine oxide, one of the flame retardants;

[0024] 0.3 parts of phthalocyanine blue as pigment;

[0025] 0.2 parts of white carbon black as a bulking agent;

[0026] 1 part of fumed alumina is a loosening agent and provides antistatic effect. When a proper amount of fumed alumina powder is added to the powder coating, through sufficient mechanical stirring, the alumina nanoparticles can be orderly combined on the surface of the matrix particles to form a layer of "coating", thus forming a "shell-core" structure, which moves as a whole, can effectively reduce the electrostatic attraction between particles and avoid powder adhesion caused by van der Waals force, moisture absorption, particle friction, etc.

[0027] 1 part of polyethylene wax as lubricant;

[0028] 1 part of benzoate, which is a plasticizer and has the functions of deodorizing and promoting leveling;

[0029] 2 parts of titanium dioxide R-219, a brightener;

[0030] 2 parts of sodium polyacrylate, which is a brightener and has the function of promoting particle dispersion;

[0031] 0.8 parts of leveling agent PV-88.

[0032] Preferably, the preparation process of the modified epoxy resin is as follows:

[0033] 1) Preparation of aluminum gel solution:

[0034] Deionized water and Al(OH)3 were mixed and stirred at a weight ratio of 1:20, and the obtained Al(OH)3 hydrosol was added to H3PO4 with a weight concentration of 85%, and the molar ratio of Al(OH)3 and H3PO4 was controlled to be 1:3.1. The mixture was heated to 60°C in a water bath, stirred while adding, and stirred for 2 hours until there was no precipitation, to obtain a transparent, colorless and odorless aluminum dihydrogen phosphate viscous liquid, i.e., an aluminum gel solution, and the tested pH was 1.6;

[0035] 2) Modification reaction:

[0036] Add bisphenol A epoxy resin (Guodu YD-012 epoxy resin) into toluene, heat to 60°C, stir until completely dissolved, add 60°C aluminum gel solution dropwise, and complete the addition within 5 minutes. Stir and react at a constant temperature of 60°C for 2.5 hours to obtain a slightly turbid milky white transparent sol system. Pour the system into an evaporating dish, evaporate in vacuum at 60°C and 0.1 kPa for 24 hours to obtain a cake-like gel, which is then extruded and granulated at 110°C to obtain a granular modified epoxy resin.

[0037] Furthermore, in 2), the weight ratio of bisphenol A epoxy resin to toluene is 1:5.

[0038] Furthermore, in 2), the weight ratio of bisphenol A epoxy resin to aluminum gel solution is 3:1, phosphoric acid in the aluminum gel solution reacts with the epoxy group of the bisphenol A epoxy resin, and a small amount of water in the aluminum gel solution is conducive to the hydrolysis reaction, thereby obtaining a modified epoxy resin with phosphate groups, which greatly enhances the flexibility and flame retardant effect (as demonstrated by flammability tests), and the phosphate groups are conducive to the combination of inorganic flame retardant components and polymer phases, avoiding cracking caused by phase separation after curing.

[0039] The present invention also provides a method for preparing the aforementioned high temperature resistant non-combustible coating powder, comprising the following steps:

[0040] S1, premixing the modified epoxy resin, aluminum hydroxide or silicon dioxide, red phosphorus, triphenylphosphine or triphenylphosphine oxide, dicyandiamide and 2-methylimidazole in a high-speed mixer at a rotation speed of 500-1500 rpm;

[0041] S2, then add it into a twin-screw extruder, set the temperature at 90-150°C, melt the resin under the shearing state of the screw, add phthalocyanine blue, white carbon black, fumed alumina, polyethylene wax, benzoate, titanium dioxide R-219, sodium polyacrylate and leveling agent PV-88, mix well to obtain a melt;

[0042] S3, after the melt is cooled by the cooling roller, it enters the ACM mill for crushing;

[0043] S4, after air selection and screening, collect particles with a particle size of 20-80 μm to obtain high temperature resistant non-combustible coating powder;

[0044] S5. Before use, add thixotropic agent to the high temperature resistant non-flammable coating powder to make the powder fluidized and fluffy.

[0045] Preferably, the thixotropic agent is the liquid thixotropic agent HY-605 produced by Huiyan or the thixotropic agent 750B produced by Kyoeisha, and the weight ratio of the thixotropic agent to the high temperature resistant non-flammable coating powder is 0.03-0.05:1.

[0046] The application of the high temperature resistant non-flammable coating powder obtained by the above preparation method in the insulation packaging process of electronic components adopts the transfer molding method:

[0047] The high temperature resistant non-flammable coating powder material with thixotropic agent added is beaten into a cake sheet, which is sealed in a mold for positioning electronic components after preheating.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] 1. The present invention uses a highly acidic aluminum gel solution produced by phosphoric acid and aluminum hydroxide to directly modify the bisphenol A epoxy resin. The phosphoric acid in the aluminum gel solution reacts with the epoxy group of the bisphenol A epoxy resin, and a small amount of water in the aluminum gel solution is conducive to the hydrolysis reaction, thereby obtaining a modified epoxy resin with a phosphate ester group, which greatly enhances the flexibility and flame retardant effect; and the phosphate ester group is conducive to the combination of the inorganic flame retardant component and the polymer phase, avoiding cracking caused by phase separation after curing; and at the same time, the pH value of the existing resin system obtained by using a strong alkaline flame retardant component is reduced, thereby reducing the corrosiveness to electronic components.

[0050] 2. The present invention also uses red phosphorus and triphenylphosphine oxide as auxiliary flame retardants. Red phosphorus has a strong dehydration effect, which promotes the dehydration, crystallization and heat absorption of aluminum hydroxide, thereby increasing the flame retardant effect of the flame retardant system. The product of triphenylphosphine oxide after thermal decomposition is polymetaphosphoric acid, which promotes the rapid dehydration and carbonization of the polymer surface to form a dense carbonized layer. Under the synergistic effect of the modified resin, filler and flame retardant, the epoxy powder composition can achieve a non-flammable effect.

[0051] 3. The present invention achieves complete non-flammability and no flammable dripping at high temperature by matching flame retardants and modifying epoxy resins, and is particularly suitable for insulating packaging of high-precision electronic components. DETAILED DESCRIPTION

[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.

[0053] Preparation Example 1:

[0054] The preparation process of modified epoxy resin is as follows:

[0055] 1) Preparation of aluminum gel solution:

[0056] Deionized water and Al(OH)3 were mixed and stirred at a weight ratio of 1:20, and the obtained Al(OH)3 hydrosol was added to H3PO4 with a weight concentration of 85%, and the molar ratio of Al(OH)3 and H3PO4 was controlled to be 1:3.1. The mixture was heated to 60°C in a water bath, stirred while adding, and stirred for 2 hours until there was no precipitation, to obtain a transparent, colorless and odorless aluminum dihydrogen phosphate viscous liquid, i.e., an aluminum gel solution, and the tested pH was 1.6;

[0057] 2) Modification reaction:

[0058] Add bisphenol A epoxy resin (Guodu YD-012 epoxy resin) into toluene, heat to 60°C, stir until completely dissolved, add 60°C aluminum gel solution dropwise, and complete the addition within 5 minutes. Stir and react at a constant temperature of 60°C for 2.5 hours to obtain a slightly turbid milky white transparent sol system. Pour the system into an evaporating dish, evaporate in vacuum at 60°C and 0.1 kPa for 24 hours to obtain a cake-like gel, which is then extruded and granulated at 110°C to obtain a granular modified epoxy resin.

[0059] Wherein, the weight ratio of bisphenol A epoxy resin to toluene in 2) is 1:5.

[0060] Among them, in 2), the weight ratio of bisphenol A epoxy resin to aluminum gel solution is 3:1, phosphoric acid in the aluminum gel solution reacts with the epoxy group of bisphenol A epoxy resin, and a small amount of water in the aluminum gel solution is conducive to the hydrolysis reaction, thereby obtaining a modified epoxy resin with phosphate groups, which greatly enhances the flexibility and flame retardant effect (demonstrated by flammability test), and the phosphate groups are conducive to the combination of inorganic flame retardant components and polymer phases, avoiding cracking caused by phase separation after curing.

[0061] Embodiment group:

[0062] A method for preparing a high temperature resistant non-combustible coating powder comprises the following steps:

[0063] S1, premixing the modified epoxy resin obtained in Preparation Example 1, aluminum hydroxide or silicon dioxide, red phosphorus, triphenylphosphine or triphenylphosphine oxide, dicyandiamide and 2-methylimidazole in a high-speed mixer at a rotation speed of 500-1500 rpm;

[0064] S2, then add it into a twin-screw extruder, set the temperature at 90-150°C, melt the resin under the shearing state of the screw, add phthalocyanine blue, white carbon black, fumed alumina, polyethylene wax, benzoate, titanium dioxide R-219, sodium polyacrylate and leveling agent PV-88, mix well to obtain a melt;

[0065] S3, after the melt is cooled by the cooling roller, it enters the ACM mill for crushing;

[0066] S4, after air selection and screening, collect particles with a particle size of 20-80 μm to obtain high temperature resistant non-combustible coating powder;

[0067] S5. Before use, add thixotropic agent to the high temperature resistant non-flammable coating powder to make the powder fluidized and fluffy.

[0068] The thixotropic agent is the liquid thixotropic agent HY-605 produced by Huiyan or the thixotropic agent 750B produced by Kyoeisha, and the weight ratio of the thixotropic agent to the high temperature resistant non-flammable coating powder is 0.03-0.05:1.

[0069] Comparative Example 1 is set up, in which bisphenol A epoxy resin YD-012 is used to replace the modified epoxy resin in the embodiment group. The specific formula and flame retardant test are shown in Table 1 below:

[0070] Table 1. Formula and flame retardant test of non-combustible coating powder

[0071]

[0072] It should be noted that some product models and specifications in Table 1 are as follows: aluminum hydroxide particle size is 40μm, silica model is SHA0065, dicyandiamide model is DDA-5, phthalocyanine blue model is L6930, polyethylene wax model is GY-303, benzoate model is Benzoflex 2088, white carbon black model is TS720, and fumed alumina model is SpectrAl® 100.

[0073] According to the UL94 flammability rating test method, V-0 means that after two 10-second combustion tests on the sample, the flame is extinguished within 30 seconds and no burning materials fall off.

[0074] The main flame retardant component in existing powder coatings is generally a strong alkaline hydroxide, which has a strong alkalinity and is easy to cause corrosion during coating. The modified epoxy resin of the present application adopts a highly acidic aluminum gel solution, which has a significant neutralizing effect on the strong alkaline flame retardant components of the system. After the mixed high-temperature resistant non-combustible coating powder is sprayed with water, the pH test paper shows that the test pH is 8.4.

[0075] Furthermore, the modified epoxy resin proposed by the present invention is non-flammable and does not produce flammable drippings. Phosphazene generates phosphoric acid, metaphosphoric acid and polyphosphoric acid during thermal decomposition, and forms a non-volatile protective film on the surface of the polymer to isolate the air.

[0076] 1. Modify the epoxy resin by adding flame retardants, phosphides and other ingredients to the epoxy resin. The synthesized resin has high non-combustible thermal stability, dehydrates into carbon when decomposed at high temperature, releases water, carbon dioxide and nitrogen when burned, and the non-combustible gas produced reduces the contact between the object and the flame. By comparing Comparative Example 1 with Example 1, it can be seen that the flame retardant effect of adding modified epoxy resin is better than that of adding bisphenol A epoxy resin, and can be extinguished in a shorter time.

[0077] 2. Using highly flame-retardant aluminum hydroxide as a filler can increase the flame retardant effect; using red phosphorus and triphenylphosphine oxide as flame retardants at the same time, red phosphorus has a strong dehydration effect, which promotes the dehydration, crystallization and heat absorption of aluminum hydroxide, thereby increasing the flame retardant effect of the flame retardant system. The product of triphenylphosphine oxide after thermal decomposition is polymetaphosphoric acid, which promotes the rapid dehydration and carbonization of the polymer surface to form a dense carbonized layer. By comparing Example 2 and Example 3, it can be seen that under the synergistic effect of the modified resin, filler and flame retardant, the epoxy powder composition can achieve a non-flammable effect.

[0078] Application Group:

[0079] The high temperature resistant non-combustible coating powder obtained in Examples 1-3 is applied in the electronic component insulation packaging process, using a transfer molding method: the high temperature resistant non-combustible coating powder material with a thixotropic agent added is beaten into a cake, which is then sealed in a mold for positioning the electronic component after preheating.

[0080] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high temperature resistant non-combustible coating powder, characterized in that: It includes the following components by weight: 20-50 parts of modified epoxy resin; 30-80 parts of filler, including any of aluminum hydroxide, silicon dioxide, aluminum oxide, boron nitride, quartz powder, mica powder, aluminum chloride powder, diamond powder, silicon nitride, expanded graphite, and calcium carbonate; 3-7 parts of a curing agent, including dicyandiamide and 2-methylimidazole; 2-15 parts of a flame retardant, wherein the flame retardant is triphenylphosphine or triphenylphosphine oxide and red phosphorus, and the weight ratio of triphenylphosphine or triphenylphosphine oxide to red phosphorus is 3:1; 0.2-3 parts of pigment, including any of phthalocyanine blue, iron oxide blue, cobalt blue, cobalt chrome blue, and titanium dioxide R-219; 0.1-1 part of a bulking agent, including any of white carbon black, fumed alumina, sodium polyacrylate, vinyl bisstearamide, and dispersant SMA1112; 0.5-3 parts of leveling agent, including any one of leveling agent PV-88, leveling agent BYK-3902P, leveling agent BYK-3933 P, leveling agent BYK-360 P, leveling agent ZY-1099, leveling agent LF-9222, and leveling agent VOK-LP 5400; 0.5-5 parts of a brightener, including any of paraffin wax, polyethylene wax, and polyamide wax; 1-5 parts of plasticizer, including any of dioctyl phthalate, benzoate, chlorinated polyethylene, modified polyurethane acrylate resin, AGE epoxy diluent, and n-butyl glycidyl ether; The preparation process of the modified epoxy resin is as follows: 1) Preparation of aluminum gel solution: Deionized water and Al(OH)3 were mixed and stirred at a weight ratio of 1:20, and the obtained Al(OH)3 hydrosol was added to H3PO4 with a weight concentration of 85%, and the molar ratio of Al(OH)3 and H3PO4 was controlled to be 1:3.

1. The mixture was heated to 60°C in a water bath, stirred while adding, and stirred for 2 hours until there was no precipitation, to obtain a transparent, colorless and odorless aluminum dihydrogen phosphate viscous liquid, i.e., an aluminum gel solution, and the tested pH was 1.6; 2) Modification reaction: Add bisphenol A epoxy resin into toluene, heat to 60°C, stir until completely dissolved, add 60°C aluminum gel solution dropwise, and complete the addition within 5 minutes. Stir and react at a constant temperature of 60°C for 2.5 hours to obtain a slightly turbid milky white transparent sol system. Pour the system into an evaporating dish, evaporate under vacuum at 60°C and 0.1 kPa for 24 hours to obtain a cake-like gel, which is then extruded and granulated at 110°C to obtain a granular modified epoxy resin.

2. The high temperature resistant non-combustible coating powder according to claim 1, characterized in that: The weight ratio of bisphenol A epoxy resin to toluene in the above 2) is 1:

5.

3. The high temperature resistant non-combustible coating powder according to claim 1, characterized in that: The weight ratio of bisphenol A epoxy resin to aluminum gel solution in 2) is 3:

1.

4. The high temperature resistant non-combustible coating powder according to claim 1, characterized in that: Specifically include the following components by weight: 43.7 parts of modified epoxy resin; 41 parts of aluminum hydroxide or silicon dioxide; 4 parts of dicyandiamide; 4 parts of 2-methylimidazole; 1 part of red phosphorus; 3 parts of triphenylphosphine or triphenylphosphine oxide; 0.3 parts of phthalocyanine blue; 0.2 parts of white carbon black; 1 part of fumed alumina; 1 part of polyethylene wax; 1 part of parabens; 2 parts of titanium dioxide R-219; 2 parts of sodium polyacrylate; 0.8 parts of leveling agent PV-88.

5. The method for preparing a high temperature resistant non-combustible coating powder according to claim 4, characterized in that: The following steps are involved: S1, premixing the modified epoxy resin, aluminum hydroxide or silicon dioxide, red phosphorus, triphenylphosphine or triphenylphosphine oxide, dicyandiamide and 2-methylimidazole in a high-speed mixer at a rotation speed of 500-1500 rpm; S2, then add it into a twin-screw extruder, set the temperature at 90-150°C, melt the resin under the shearing state of the screw, add phthalocyanine blue, white carbon black, fumed alumina, polyethylene wax, benzoate, titanium dioxide R-219, sodium polyacrylate and leveling agent PV-88, mix well to obtain a melt; S3, after the melt is cooled by the cooling roller, it enters the ACM mill for crushing; S4, after air selection and screening, collect particles with a particle size of 20-80 μm to obtain high temperature resistant non-combustible coating powder; S5. Before use, add thixotropic agent to the high temperature resistant non-flammable coating powder to make the powder fluidized and fluffy.

6. The method for preparing a high temperature resistant non-combustible coating powder according to claim 5, characterized in that: The thixotropic agent is the liquid thixotropic agent HY-605 produced by Huiyan or the thixotropic agent 750B produced by Kyoeisha, and the weight ratio of the thixotropic agent to the high temperature resistant non-flammable coating powder is 0.03-0.05:

1.

7. Application of the high temperature resistant non-combustible coating powder obtained by the preparation method of claim 5 in the insulation packaging process of electronic components, characterized in that: The use process adopts transfer molding method: The high temperature resistant non-flammable coating powder material with thixotropic agent added is beaten into a cake sheet, which is sealed in a mold for positioning electronic components after preheating.