A method for preparing a high-uniformity 2050 aluminum-lithium alloy plate

By using high-temperature hot rolling, annealing, cold rolling, solid solution quenching and aging treatment technical means in the preparation of 2050 aluminum-lithium alloy sheets, the problems of sheet uniformity and fracture toughness are solved, and the mechanical properties are improved and uniformity are achieved. Improved, suitable for boards with thickness of 10~50mm.

CN118357270BActive Publication Date: 2024-11-29CENT SOUTH UNIV
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410584146.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-11-29
Estimated Expiration
2044-05-11

Smart Images

  • Figure CN118357270B_ABST
    Figure CN118357270B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a 2050 aluminum-lithium alloy plate with high uniformity, comprising the following steps: S1) heating a 2050 aluminum-lithium alloy ingot, and rolling and blanking after heat preservation; S2) annealing the plate obtained in step S1); S3) cold rolling the plate obtained in step S2), and then heating the plate obtained, and rolling and forming after heat preservation; S4) performing a solid solution treatment on the plate obtained in step S3), and then performing a pre-stretching, and finally performing an aging treatment to obtain a 2050 aluminum-lithium alloy plate. The method for preparing a 2050 aluminum-lithium alloy plate provided by the present invention is based on the goal of uniform organization control, and through coordinated control of high-temperature large deformation hot rolling blanking, pre-precipitation, cold rolling, and high-temperature hot rolling forming, a uniform deformation organization is obtained, and a 2050 aluminum-lithium alloy plate with high uniformity of 10 to 50 mm in thickness is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aluminum-lithium alloys, and in particular to a method for preparing a high-uniformity 2050 aluminum-lithium alloy plate. Background Art

[0002] 2050 aluminum-lithium alloy is an advanced third-generation aluminum-lithium alloy currently used in the aerospace field. It has good hardenability, high strength, high modulus (75GPa), low density (2.71g / cm 3 ), good fracture toughness, high stress corrosion resistance and low crack growth rate; compared with 7050, it can effectively reduce the weight of parts, improve the corrosion resistance and life of the structure, and is the preferred material for aluminum alloy main load-bearing structural parts such as large aircraft, new generation fighter structural frames, beams and wall panels

[0003] However, due to the complex phase composition of 2050 aluminum-lithium alloy, it is difficult to control the uniformity of the structure during the sheet preparation process, resulting in a large dispersion of mechanical properties. In order to solve the above problems, relevant research work has been carried out at home and abroad:

[0004] The Chinese patent application with publication number CN113718096A discloses a preparation process for aluminum-lithium alloy plates with high comprehensive performance. The main idea of ​​the scheme is: the ingot is subjected to temperature-controlled initial rolling (400±30℃) and quickly cooled to room temperature, then placed in a high-temperature air circulation furnace for heating, kept warm for a period of time, cooled to a specific temperature, and then taken out of the furnace for secondary hot rolling. After hot rolling to a specified size, it is quickly cooled to room temperature. This scheme is based on the idea of ​​forming partial recrystallization through temperature-controlled initial rolling pretreatment and then converting it into a deformed structure. It has been verified for a typical specification of 80mm thickness, and no solution for overall uniformity has been proposed. The Chinese patent application with publication number CN108034909A discloses a method for preparing 2050 aluminum-lithium alloy fine-grained plates. The main idea of ​​the scheme is: solid solution water quenching + rolling pre-deformation + overaging treatment + medium temperature rolling deformation + recrystallization annealing; this scheme is mainly aimed at grain refinement of thin plates (2mm) and the formation of recrystallized structures, which is not conducive to fracture toughness and is not suitable for the preparation of medium and thick plates. The Chinese patent application with publication number CN101903546A discloses a method for preparing rolled products made of aluminum-lithium alloy for aviation applications. The main idea of ​​the scheme is: by controlling the final rolling temperature ≥410°C and the total homogenization + solution time not exceeding 30h, a non-recrystallized plate can be obtained, thereby obtaining a higher fracture toughness. However, the scheme is limited to plates with specifications greater than 30mm. For plates with smaller thickness, the difficulty of controlling the recrystallization structure increases due to the increase in deformation. Therefore, the scheme is not suitable for plates with a thickness of less than 30mm.

[0005] In summary, among the existing disclosed solutions, there is no preparation solution that can fully meet the high uniformity of 2050 aluminum-lithium alloy plates with a thickness of 10~50mm. Therefore, it is urgent to develop new processes to solve the problem. Summary of the invention

[0006] The technical problem solved by the present invention is to provide a method for preparing a 2050 aluminum-lithium alloy plate with high uniformity. The 2050 aluminum-lithium alloy plate prepared in the present application can obtain a uniform deformation structure and has good mechanical properties.

[0007] In view of this, the present application provides a method for preparing a high-uniformity 2050 aluminum-lithium alloy plate, characterized in that it comprises the following steps:

[0008] S1) heating the 2050 aluminum-lithium alloy ingot to 450-530°C, keeping the temperature, and then rolling the ingot;

[0009] S2) heating the plate obtained in step S1) to 350-450° C. for annealing;

[0010] S3) cold rolling the plate obtained in step S2), then heating the plate to 450-530°C, keeping the temperature, and rolling it into shape;

[0011] S4) subjecting the plate obtained in step S3) to a solution treatment, a pre-stretching treatment, and finally an aging treatment to obtain a 2050 aluminum-lithium alloy plate.

[0012] Preferably, in step S1), the heating temperature is 470-510° C. and the heating time is 12-20 hours.

[0013] Preferably, in step S1), the deformation amount of a single rolling pass is 5-20%.

[0014] Preferably, in step S2), the annealing temperature is 380-430° C., and the temperature is kept for 2-8 hours, and the annealing cooling method is air cooling.

[0015] Preferably, in step S3), the total deformation of the cold rolling is 15-30%, and the deformation of a single pass is 4-8%.

[0016] Preferably, in step S3), the heating temperature is 470-510° C. and the heat preservation time is 4-8 hours; and the deformation amount of a single rolling pass is 8-25%.

[0017] Preferably, in step S4), the temperature of the solution treatment is 500-520° C., and the temperature is kept for 1-4 hours.

[0018] Preferably, in step S4), the pre-stretching amount is 2-5%.

[0019] Preferably, in step S4), the aging treatment is performed at a temperature of 145-160° C. and for a time of 20-35 h.

[0020] Preferably, the thickness of the 2050 aluminum-lithium alloy ingot is 300-400 mm, and the thickness of the 2050 aluminum-lithium alloy plate is 10-50 mm.

[0021] The present application provides a method for preparing a 2050 aluminum-lithium alloy plate with high uniformity, which first heats a 2050 aluminum-lithium alloy ingot to 450-530°C, rolls the plate after heat preservation, heats the plate to 350-450°C for annealing to increase recrystallization nucleation points, and then cold rolls the plate to obtain a high dislocation density billet to further improve the recrystallization driving force, heats the plate after cold rolling, and then rolls the plate to obtain a completely recrystallized structure in the heating stage, which is then transformed into a completely deformed structure during rolling, and finally the plate is solution treated, stretched, and aged to obtain a 2050 aluminum-lithium alloy plate; in the preparation process of the 2050 aluminum-lithium alloy plate, high-temperature hot rolling for billet opening-annealing-cold rolling-high-temperature hot rolling forming-solution quenching-pre-stretching-aging are sequentially performed, and the above stages are combined to obtain a uniform deformation structure, which ultimately improves the uniformity and fracture toughness of the aluminum-lithium alloy plate BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a microstructure characteristic diagram of the aluminum-lithium alloy prepared in Example 1 of the present invention;

[0023] Figure 2 This is a microstructure characteristic diagram of the aluminum-lithium alloy prepared in Comparative Example 1 of the present invention;

[0024] Figure 3 This is a microstructure characteristic diagram of the aluminum-lithium alloy prepared in Comparative Example 2 of the present invention;

[0025] Figure 4 This is a characteristic diagram of the microstructure of the aluminum-lithium alloy prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0026] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0027] In view of the difficulty in controlling the uniformity of the structure during the preparation of 2050 aluminum-lithium alloy plates (thickness 10~50mm) in the prior art, resulting in large dispersion of mechanical properties, especially low toughness, the present application provides a method for preparing a high-uniformity 2050 aluminum-lithium alloy plate, which obtains a uniform deformation structure by adopting the technical means of high-temperature hot rolling blanking-annealing-cold rolling-high-temperature hot rolling forming-solution quenching-pre-stretching-aging in sequence, and finally improves the uniformity of mechanical properties and fracture toughness. Specifically, the embodiment of the present invention discloses a method for preparing a high-uniformity 2050 aluminum-lithium alloy plate, comprising the following steps:

[0028] S1) heating the 2050 aluminum-lithium alloy ingot to 450-530°C, keeping the temperature, and then rolling the ingot;

[0029] S2) heating the plate obtained in step S1) to 350-450° C. for annealing;

[0030] S3) cold rolling the plate obtained in step S2), then heating the plate to 450-530°C, keeping the temperature, and rolling it into shape;

[0031] S4) subjecting the plate obtained in step S3) to a solution treatment, a pre-stretching treatment, and finally an aging treatment to obtain a 2050 aluminum-lithium alloy plate.

[0032] In the preparation process of 2050 aluminum-lithium alloy plate, the present application first heats the 2050 aluminum-lithium alloy ingot to 450-530°C, keeps it warm and then rolls it into a blank. This step is the high-temperature large deformation hot rolling of the aluminum-lithium alloy ingot; specifically, the heating temperature is 470-510°C, and the holding time is 12-20h. More specifically, the heating temperature is 470°C, 480°C, 490°C, 500°C or 510°C, and the holding time is 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h or 20h. The deformation of a single rolling pass is 5-20%, and the rolling can be performed in multiple passes, and the deformation of each pass can be the same or different; specifically, the deformation of a single rolling pass is 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%. The total deformation of the rolling is 70-97%.

[0033] The present application then anneals the plate obtained by slab rolling, wherein the annealing temperature is 350-450°C, and the temperature is kept for 2-8 hours. Specifically, the annealing temperature is 380-430°C, and the temperature is kept for 2-6 hours. More specifically, the annealing temperature is 380°C, 390°C, 400°C, 410°C, 420°C or 430°C, and the temperature is kept for 2 hours, 3 hours, 4 hours, 5 hours or 6 hours. The annealing is performed to increase the recrystallization nucleation points.

[0034] According to the present invention, the annealed sheet is cold rolled to obtain a high dislocation density sheet, the single-pass deformation of the cold rolling is 4-8%, and the total deformation is 15-30%. Specifically, the single-pass deformation is 4%, 5%, 6%, 7% or 8%, and the total deformation is 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%; in the present application, the cold rolling is preferably performed in multiple passes.

[0035] The present application then heats the obtained plate to 450-530°C, keeps it warm and then rolls it into shape; the plate is finally formed by high-temperature hot rolling. In this stage, the heating stage is to obtain a completely recrystallized structure, and the rolling is to transform it into a completely deformed structure. The heating temperature is 470-510°C, and the temperature is kept warm for 4-8 hours. Specifically, the heating temperature is 470°C, 480°C, 490°C, 500°C or 510°C, and the holding time is 4h, 5h, 6h, 7h or 8h. The deformation of the rolling is 8-25% in a single pass. Specifically, the deformation of the rolling is 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%. The rolling is preferably carried out in multiple passes in the present application.

[0036] After rolling, solution treatment is carried out in sequence, followed by pre-stretching and finally aging treatment to obtain 2050 aluminum-lithium alloy sheet. The above steps are used to relieve stress to further improve strength. The temperature of the solution treatment is 500~520℃, and the insulation time is 1~4h. Specifically, the temperature of the solution treatment is 500℃, 510℃ or 520℃, and the insulation time is 1h, 2h, 3h or 4h. The stretching amount of the pre-stretching is 2~5%. Specifically, the stretching amount of the pre-stretching is 2%, 3%, 4% or 5%. The temperature of the aging treatment is 145-160°C, and the time is 20-35h. Specifically, the temperature of the aging treatment is 145°C, 147°C, 149°C, 150°C, 151°C, 153°C, 155°C, 156°C, 157°C, 158°C, 159°C or 160°C, and the time of the aging treatment is 20h, 22h, 23h, 24h, 26h, 27h, 29h, 30h, 31h, 32h, 33h, 34h or 35h.

[0037] For the preparation of 10~50mm aluminum-lithium alloy plates, the conventional hot rolling process (opening-hot rolling-cold rolling forming-annealing) forms a mixed crystal structure of deformation structure and partial recrystallization structure, which has poor performance and uniformity. Therefore, the present invention provides a preparation method of 2050 aluminum-lithium alloy plates with high uniformity. Based on the uniform structure control target, the method obtains uniform deformation structure through high-temperature large deformation hot rolling opening, pre-precipitation annealing and cold rolling, high-temperature hot rolling forming and other coordinated control, and forms a 10~50mm thick high uniformity 2050 aluminum-lithium alloy plate process. At the same time, the method adopted by the present invention can be realized by existing production equipment and has engineering implementation conditions.

[0038] In order to further understand the present invention, the preparation method of the high-uniformity 2050 aluminum-lithium alloy plate provided by the present invention is described in detail below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0039] Example 1

[0040] A method for preparing a high-uniformity 2050 aluminum-lithium alloy plate, wherein the alloy composition is: 3.7wt% Cu, 1wt% Li, 0.5wt% Mg, 0.3wt% Mn, 0.35wt% Ag, 0.11wt% Zr and the balance Al, and the plate thickness is 15 mm, comprising the following steps:

[0041] Step 1: Heat the 380mm thick flat ingot to 490℃ in a heating furnace and keep it warm for 16h; after the insulation is completed, roll it on a rolling mill, first with a rolling amount of 15mm per pass to a thickness of 230mm, then with a rolling amount of 30mm per pass to a thickness of 140mm, and then with a rolling amount of 15mm per pass to a thickness of 110mm;

[0042] Step 2: Place the plate into a heating furnace for annealing, set the furnace temperature to 420°C, and keep it warm for 6 hours;

[0043] Step 3: After the plate is annealed, it is cold rolled on a rolling mill with a rolling amount of 4 mm per pass to a thickness of 90 mm;

[0044] Step 4: After the cold rolling is completed, the plate is heated to 490°C in a heating furnace and kept warm for 6 hours; after the insulation is completed, it is rolled on a rolling mill, first with a rolling amount of 15mm per pass to a thickness of 45mm, then with a rolling amount of 6mm per pass to a thickness of 21mm, and then with a rolling amount of 2mm per pass to a thickness of 15mm;

[0045] Step 5: After rolling, solution quenching is performed by heating the plate to 510°C and keeping it warm for 2 hours. After the insulation is completed, quenching is performed with room temperature water;

[0046] Step 6: After solution quenching, pre-stretching is performed, and the stretching amount is controlled at 3%;

[0047] Step 7: After the pre-stretching is completed, an aging treatment is performed, the aging temperature is 155°C, the aging time is 24 hours, and an aluminum-lithium alloy plate with a thickness of 15 mm is obtained.

[0048] Example 2

[0049] A method for preparing a high-uniformity 2050 aluminum-lithium alloy plate, wherein the alloy composition is: 3.7wt% Cu, 1wt% Li, 0.5wt% Mg, 0.3wt% Mn, 0.35wt% Ag, 0.11wt% Zr and the balance Al, and the plate thickness is 45mm, comprising the following steps:

[0050] Step 1: Heat the 380mm thick flat ingot to 490℃ in a heating furnace and keep it warm for 16h; after the insulation is completed, roll it on a rolling mill, first with a rolling amount of 15mm per pass to a thickness of 230mm, then with a rolling amount of 30mm per pass to a thickness of 170mm, and then with a rolling amount of 15mm per pass to a thickness of 140mm;

[0051] Step 2: Place the plate into a heating furnace for annealing, set the furnace temperature to 420°C, and keep it warm for 6 hours;

[0052] Step 3: After the plate is annealed, it is cold rolled on a rolling mill with a rolling amount of 4 mm per pass to a thickness of 120 mm;

[0053] Step 4: After the cold rolling is completed, the plate is heated to 490°C in a heating furnace and kept warm for 6 hours; after the insulation is completed, it is rolled on a rolling mill with a rolling amount of 15 mm per pass to a thickness of 45 mm;

[0054] Step 5: After rolling, solution quenching is performed by heating the plate to 510°C and keeping it warm for 4 hours. After the insulation is completed, quenching is performed with room temperature water;

[0055] Step 6: After solution quenching, pre-stretching is performed, and the stretching amount is controlled at 3%;

[0056] Step 7: After the pre-stretching is completed, an aging treatment is performed, the aging temperature is 155°C, the aging time is 24 hours, and an aluminum-lithium alloy plate with a thickness of 45 mm is obtained.

[0057] Comparative Example 1

[0058] A method for preparing a 2050 aluminum-lithium alloy plate, which is different from Example 1 in that no annealing process is used.

[0059] Step 1: Heat the 380mm thick flat ingot to 490℃ in a heating furnace and keep it warm for 16h; after the insulation is completed, roll it on a rolling mill, first with a rolling amount of 15mm per pass to a thickness of 230mm, then with a rolling amount of 30mm per pass to a thickness of 140mm, and then with a rolling amount of 15mm per pass to a thickness of 110mm;

[0060] Step 2: After the hot rolling of the plate, it is cold rolled on the rolling mill, with a rolling amount of 4 mm per pass, until the thickness reaches 90 mm;

[0061] Step 3: After the cold rolling is completed, the plate is heated to 490°C in a heating furnace and kept warm for 6 hours; after the insulation is completed, it is rolled on a rolling mill, first with a rolling amount of 15mm per pass to a thickness of 45mm, then with a rolling amount of 6mm per pass to a thickness of 21mm, and then with a rolling amount of 2mm per pass to a thickness of 15mm;

[0062] Step 4: After rolling, solution quenching is performed. The plate is heated to 510°C and kept warm for 2 hours. After the heat preservation is completed, room temperature water is used for quenching.

[0063] Step 5: After solution quenching, pre-stretching is performed, and the stretching amount is controlled at 3%;

[0064] Step 6: After the pre-stretching is completed, an aging treatment is performed, the aging temperature is 155°C, and the aging time is 24 hours to obtain an aluminum-lithium alloy plate with a thickness of 15 mm.

[0065] Comparative Example 2

[0066] A method for preparing a 2050 aluminum-lithium alloy plate, which differs from Example 1 in that no cold rolling process is used.

[0067] Step 1: Heat the 380mm thick flat ingot to 490℃ in a heating furnace and keep it warm for 16h; after the insulation is completed, roll it on a rolling mill, first with a rolling amount of 15mm per pass to a thickness of 230mm, then with a rolling amount of 30mm per pass to a thickness of 140mm, and then with a rolling amount of 15mm per pass to a thickness of 110mm;

[0068] Step 2: Place the plate into a heating furnace for annealing, set the furnace temperature to 420°C, and keep it warm for 6 hours;

[0069] Step 3: After annealing, the plate is heated to 490°C in a heating furnace and kept warm for 6 hours; after the heat preservation is completed, it is rolled on a rolling mill, first with a rolling amount of 15mm per pass, rolled to a thickness of 50mm, then with a rolling amount of 5-6mm per pass, rolled to a thickness of 21mm, and then with a rolling amount of 2mm per pass, rolled to a thickness of 15mm;

[0070] Step 4: After rolling, solution quenching is performed. The plate is heated to 510°C and kept warm for 2 hours. After the heat preservation is completed, room temperature water is used for quenching.

[0071] Step 5: After solution quenching, pre-stretching is performed, and the stretching amount is controlled at 3%;

[0072] Step 6: After the pre-stretching is completed, an aging treatment is performed, the aging temperature is 155°C, and the aging time is 24 hours to obtain an aluminum-lithium alloy plate with a thickness of 15 mm.

[0073] Comparative Example 3

[0074] A method for preparing a 2050 aluminum-lithium alloy plate, which is different from Example 1 in that only conventional hot rolling is used.

[0075] Step 1: Heat the 380mm thick flat ingot to 490℃ in a heating furnace and keep it warm for 16h; after the insulation is completed, roll it on a rolling mill, first with a rolling amount of 15mm per pass, rolling to a thickness of 230mm, then with a rolling amount of 30mm per pass, rolling to a thickness of 140mm, then with a rolling amount of 15mm per pass, rolling to a thickness of 50mm, then with a rolling amount of 5-6mm per pass, rolling to a thickness of 21mm, and finally with a rolling amount of 2mm per pass, rolling to a thickness of 15mm;

[0076] Step 2: After rolling, solution quenching is performed. The plate is heated to 510°C and kept warm for 2 hours. After the insulation is completed, room temperature water is used for quenching.

[0077] Step 3: After solution quenching, pre-stretching is performed, and the stretching amount is controlled at 3%;

[0078] Step 4: After the pre-stretching is completed, an aging treatment is performed, the aging temperature is 155°C, and the aging time is 24 hours to obtain an aluminum-lithium alloy plate with a thickness of 15 mm.

[0079] The performance data of the embodiments of the present invention and the comparative examples are shown in Table 1;

[0080] Table 1 Performance data of aluminum-lithium alloy plates prepared in Examples and Comparative Examples

[0081]

[0082] It can be seen from Table 1 that the mechanical properties of the aluminum-lithium alloy sheet prepared by the present invention are higher than those of the comparative example; at the same time, the uniformity is significantly improved. Figure 1~Figure 4 As shown, the embodiments of the present invention obtain a completely uniform deformation structure, while the comparative examples all have mixed crystal structures to varying degrees, that is, partial deformation structure and recrystallization structure, which is also the reason for the low performance and poor uniformity.

[0083] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0084] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a high-uniformity 2050 aluminum-lithium alloy sheet, characterized in that: The following steps are involved: S1) heating a 2050 aluminum-lithium alloy ingot to 450-530° C., keeping the temperature, and then rolling the ingot into a blank; S2) heating the plate obtained in step S1) to 350-450° C. for annealing; S3) cold rolling the plate obtained in step S2), then heating the plate to 470-510° C., keeping the temperature for 4-8 hours and then rolling it into shape; the deformation of a single rolling pass is 8-25%; S4) subjecting the plate obtained in step S3) to a solution treatment, a pre-stretching treatment, and finally an aging treatment to obtain a 2050 aluminum-lithium alloy plate.

2. The preparation method according to claim 1, characterized in that: In step S1), the heating temperature is 470-510° C. and the heating time is 12-20 hours.

3. The preparation method according to claim 1, characterized in that: In step S1), the deformation amount of a single rolling pass is 5 to 20%.

4. The preparation method according to claim 1, characterized in that: In step S2), the annealing temperature is 380-430° C., and the temperature is kept for 2-8 hours. The annealing cooling method is air cooling.

5. The preparation method according to claim 1, characterized in that: In step S3), the total deformation of the cold rolling is 15-30%, and the deformation of a single pass is 4-8%.

6. The preparation method according to claim 1, characterized in that: In step S4), the temperature of the solution treatment is 500-520° C. and the temperature is kept for 1-4 hours.

7. The preparation method according to claim 1, characterized in that: In step S4), the pre-stretching amount is 2-5%.

8. The preparation method according to claim 1, characterized in that: In step S4), the aging treatment is carried out at a temperature of 145 to 160° C. and for a time of 20 to 35 hours.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The thickness of the 2050 aluminum-lithium alloy ingot is 300-400 mm, and the thickness of the 2050 aluminum-lithium alloy plate is 10-50 mm.

Citation Information

Patent Citations

  • Rolled product made of aluminum-lithium alloy for aeronautical applications

    CN101903546A

  • Preparation method of 2050 aluminium-lithium alloy fine-grain plate

    CN108034909A

  • Preparation technology of high-comprehensive-performance aluminum-lithium alloy plate

    CN113718096A

  • Preparation method of Al-Cu-Li-X series aluminum lithium alloy sheet

    CN103540876A

  • Method for improving forming property of 6000-series aluminum alloy plate

    CN109954752A