A device and method for continuous atomic layer deposition of coated powder

By designing the continuous reaction chamber and multiple ALD growth cycle units in the atomic layer deposition and coating powder technology, and using inert carrier gas for powder treatment, the long-term problem in the prior art is solved, and the process efficiency is improved. Uniformity of the deposited layer.

CN118360592BActive Publication Date: 2024-11-19BATTFLEX (WUHAN) TECH CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410559402.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2024-11-19
Estimated Expiration
2044-05-08

AI Technical Summary

Technical Problem

The existing atomic layer deposition and coating powder technology requires a long time to purge inert carrier gas and reinjection into the precursor each time, resulting in a long process time and cannot increase the yield per unit time.

Method used

A device for depositing and covering powders in a continuous atomic layer is designed. By setting up a plurality of continuous reaction chambers and valve devices, the powder is transported and processed with inert carrier gas, which reduces the time for precursor replacement and passes through multiple ALDs. The growth cycle units are connected in series to achieve continuous deposition.

Benefits of technology

The time of each ALD growth cycle is significantly reduced, the amount of inert gas used for purge is saved, process efficiency is improved, and a more uniform atomic layer deposition layer formation is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118360592B_ABST
    Figure CN118360592B_ABST
Patent Text Reader

Abstract

The present invention discloses a device and method for continuous atomic layer deposition coating of powders, comprising a plurality of ALD growth cycle units connected in series, completing continuous atomic layer deposition through multiple reactions, and each ALD cycle unit is divided into a first reactor and a second reactor, which can respectively carry out reactions of different precursors, thus reducing the waiting time for cleaning in the same reaction chamber, and each process can be carried out separately, saving time, reducing production costs, improving production efficiency, and having a simple structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of vacuum atomic deposition coating, and in particular to a device and method for continuous atomic layer deposition coating of powder. Background Art

[0002] Atomic layer deposition (ALD) is a thin film deposition technology that grows thin films layer by layer at the atomic level. The ideal ALD growth process selectively and alternately exposes different precursors to the substrate surface, where they chemically adsorb and react to form the deposited film.

[0003] A complete ALD growth cycle can be divided into four steps:

[0004] 1. Pulsing the first precursor onto the substrate surface simultaneously forms covalent bonds with the first precursor at the surface group sites, saturating the surface sites to a monolayer. Once the surface is saturated, due to the precursor chemistry and process conditions, the excess precursor will not react further with the substrate surface.

[0005] 2. Inert carrier gas blows away the remaining unreacted precursor;

[0006] 3. Pulse the second precursor to chemically react on the surface of the monolayer formed by the first precursor to obtain the desired thin film material;

[0007] 4. Inert carrier gas blows away the remaining precursor and reaction by-products.

[0008] Atomic layer deposition typically involves a cycle of the above four steps, repeated as many times as necessary to achieve the desired coating thickness. During the growth process, the surface is alternately exposed to two complementary chemical precursors. In this case, each precursor is fed into the reactor separately. To prevent the precursors from reacting anywhere other than the surface, thereby causing chemical vapor deposition (CVD), after each precursor forms a monolayer and saturates the substrate surface, the different precursor deposition steps must be separated by purging with an inert carrier gas; this means that the coating after each pulse is self-limited to a single monolayer, allowing it to coat complex shapes with atomic precision.

[0009] One ALD growth cycle can form a single-layer coating of 0.1-0.2nm. To form a coating with a thickness of 10-20nm, 100-200 ALD growth cycles are required. In the existing technology of atomic layer deposition coating powder, one ALD growth cycle is completed in the reaction chamber. Each purge of the inert carrier takes 30s to expel the original precursor in the reaction chamber. After the purge, it also takes a certain amount of time to re-inject the precursor to the target pressure in the reaction chamber. 100-200 ALD growth cycles require at least 100-200 minutes to purge the inert carrier, and a certain amount of time is required to re-inject the precursor to the pressure. This makes the time for atomic layer deposition coating powder longer and cannot increase the output per unit time. Summary of the Invention

[0010] The technical problem to be solved by the present invention is to provide a device for continuous atomic layer deposition coating of powders, which overcomes the current process problems by setting up multiple continuous reaction chambers, has a simple structure and a reasonable design.

[0011] A reactor, comprising: a reaction chamber and a purification chamber, wherein the purification chamber is located below the reaction chamber, a valve device is provided between the reaction chamber and the purification chamber, the valve device being operable between an open position and a closed position, the valve device comprising a disc plate, and when the valve device is in the closed position, the purification chamber and the reaction chamber are isolated by the disc plate, the disc plate being constructed to include flow-equalizing holes uniformly distributed on a side of the disc plate facing the reaction chamber, and a fluidizing gas exhaust pipe located within the disc plate and communicating with all the flow-equalizing holes;

[0012] The reaction chamber is provided with an air pressure detection device and a temperature sensor, and a heating device is provided outside the reaction chamber. The reaction chamber is connected to a differential electrochemical mass spectrometer and a vacuum pump in sequence through an exhaust gas exhaust pipe. A filter is provided at the inlet of the exhaust gas exhaust pipe to prevent particle inhalation. The reaction chamber is also connected to the outlet of the feed inlet pipe. The fluidizing gas exhaust pipe is connected to the air inlet pipe, and the air inlet pipe is connected to a common reaction gas inlet pipe and an independent air inlet pipe attached to the common inlet pipe of the inert carrier gas through a reaction gas exhaust valve and an inert carrier gas exhaust valve, respectively.

[0013] The bottom of the clean room is connected to the inlet of the material delivery pipe. The clean room is also connected to an independent air inlet pipe attached to the inert carrier gas common air inlet pipe through an inert carrier gas exhaust valve. The clean room is also connected to the differential electrochemical mass spectrometer and the vacuum pump in sequence through the tail gas pipe.

[0014] The disc plate is provided with an exhaust hole on the side facing the purification chamber, and the exhaust hole is connected to the inert carrier gas exhaust valve and the independent air inlet pipe attached to the inert carrier gas common air inlet pipe in sequence through another fluidizing gas exhaust pipe in the disc plate.

[0015] A stirring device is arranged in the reaction chamber.

[0016] The disc plate includes an opening and closing device, which can be operated between blocking the flow balancing hole and not blocking the flow balancing hole.

[0017] Preferably, the disc plate includes an outer shell, a fluidizing gas exhaust pipe is arranged inside the outer shell along the center axis of the disc plate, a plurality of independent exhaust pipes are attached to the fluidizing gas exhaust pipe, the starting end of the independent exhaust pipe is connected to the fluidizing gas exhaust pipe, the end of the independent exhaust pipe is away from the fluidizing gas exhaust pipe and is closed, each independent exhaust pipe is evenly provided with equal flow holes, the equal flow holes extend from the independent exhaust pipe to the surface of the outer shell, each independent exhaust pipe is sleeved with a hollow sleeve that can slide along the independent exhaust pipe, and an elastic body or a magnetic body that can apply pressure or tension to the sleeve, the pressure or tension is directed to the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe, the sleeve Through holes are evenly arranged on the tube, and one end of the sleeve close to the end of the independent exhaust pipe is closed. The length of the independent exhaust pipe is greater than the length of the sleeve inside the independent exhaust pipe. When the independent exhaust pipe is ventilated so that the sleeve overcomes the pressure or tension and moves along the axial direction of the independent exhaust pipe away from the fluidizing gas exhaust pipe to the end of the independent exhaust pipe, the through holes on the sleeve are aligned one-to-one with the equalizing flow holes of the independent exhaust pipe. When the ventilation to the independent exhaust pipe is stopped or the air pressure is lower than the threshold, the sleeve moves along the axial direction of the independent exhaust pipe close to the fluidizing gas exhaust pipe to the beginning of the independent exhaust pipe under the pressure or tension, and the sleeve blocks the equalizing flow holes of the independent exhaust pipe.

[0018] Preferably, the disc plate includes an outer shell, a fluidizing gas exhaust pipe is arranged inside the outer shell along the center axis of the disc plate, a plurality of independent exhaust pipes are attached to the fluidizing gas exhaust pipe, the starting end of the independent exhaust pipe is connected to the fluidizing gas exhaust pipe, the end of the independent exhaust pipe is away from the fluidizing gas exhaust pipe and is not closed, equal flow holes are evenly arranged on each independent exhaust pipe, the outer shell is provided with a window aligned with each independent exhaust pipe, a hollow sleeve that can slide along the independent exhaust pipe is arranged outside each independent exhaust pipe, an elastic body or a magnetic body that can apply pressure or tension to the sleeve is provided inside the outer shell or outside the independent exhaust pipe, the pressure or tension is directed to the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe, through holes are evenly arranged on the sleeve, and the length of the window along the axial direction of the independent exhaust pipe is smaller than the sleeve and the independent exhaust pipe Tube, the width of the window is not greater than the diameter of the sleeve, the length of the sleeve is less than the shortest distance from the starting end of the independent exhaust pipe in the sleeve to the shell along the axial direction of the independent exhaust pipe, the length of the sleeve is greater than the length of the independent exhaust pipe in the sleeve, and the end of the sleeve close to the end of the independent exhaust pipe is closed. When the independent exhaust pipe is ventilated to make the sleeve overcome the pressure or tension and move away from the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe to the end of the independent exhaust pipe, the through hole on the sleeve is aligned one-to-one with the equalizing hole of the independent exhaust pipe. When the ventilation to the independent exhaust pipe is stopped or the air pressure is lower than the threshold, the sleeve moves close to the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe under the pressure or tension to the starting end of the independent exhaust pipe, and the sleeve blocks the equalizing hole of the independent exhaust pipe.

[0019] A device for continuous atomic layer deposition of coated powders, comprising the reactors described above, wherein two of the reactors form an ALD growth cycle unit, wherein the outlet of the material delivery pipe of the first reactor is connected to the inlet of the material delivery pipe of the second reactor, the common reaction gas inlet pipe of the first reactor is supplied with gas from a first reaction gas source, the common reaction gas inlet pipe of the second reactor is supplied with gas from a second reaction gas source, and the common inert carrier gas inlet pipes are both supplied with gas from an inert carrier gas source;

[0020] Multiple ALD growth cycle units are connected in series in sequence, the inlet of the material feed pipe of the first reactor of the first ALD growth cycle unit is connected to the loading tank, starting from the first ALD growth cycle unit, the outlet of the material feed pipe of the second reactor of the ALD growth cycle unit is connected to the inlet of the material feed pipe of the first reactor of the next ALD growth cycle unit, and the outlet of the material feed pipe of the second reactor of the last ALD growth cycle unit is connected to the unloading tank.

[0021] A device for continuous atomic layer deposition of coated powders, comprising the reactors described above, wherein each four reactors constitute an ALD growth cycle unit, wherein the outlet of the material delivery pipe of the preceding reactor among the first to fourth reactors is connected to the inlet of the material delivery pipe of the succeeding reactor, the common reaction gas inlet pipe of the first reactor is supplied by a first reaction gas source, the common reaction gas inlet pipes of the second and fourth reactors are supplied by a second reaction gas source, the common reaction gas inlet pipe of the third reactor is supplied by a third reaction gas source, and the common inert carrier gas inlet pipes are all supplied by an inert carrier gas source;

[0022] Multiple ALD growth cycle units are connected in series in sequence, the inlet of the material feed pipe of the first reactor of the first ALD growth cycle unit is connected to the loading tank, the outlet of the material feed pipe of the fourth reactor of the ALD growth cycle unit starting from the first ALD growth cycle unit is connected to the inlet of the material feed pipe of the first reactor of the next ALD growth cycle unit, and the outlet of the material feed pipe of the fourth reactor of the last ALD growth cycle unit is connected to the unloading tank.

[0023] A method for coating powders by continuous atomic layer deposition, using the above-mentioned apparatus for coating powders by continuous atomic layer deposition, comprises the following steps:

[0024] S1. Using an inert carrier gas, the uncoated powder is transported to the reaction chamber of the first reactor of the ALD growth cycle unit. The inert carrier gas is continuously introduced into the reaction chamber of the first reactor to heat the fluidized powder and maintain the powder temperature within a predetermined temperature range.

[0025] S2. Pulsing a first reaction gas into the powder in the reaction chamber of the first reactor, maintaining the pressure in the reaction chamber of the first reactor within the target pressure value, and detecting the exhaust gas composition discharged from the reaction chamber of the first reactor until it is determined that the first reaction gas is excessive;

[0026] S3. When the first reaction gas is excessive, the powder is discharged into the purge chamber of the first reactor, and the purge chamber of the first reactor is filled with an inert carrier gas until the exhaust gas discharged from the purge chamber of the first reactor does not contain the first reaction gas and by-products;

[0027] S4. The powder in the clean room of the first reactor is transported to the reaction chamber of the second reactor using an inert carrier gas. The inert carrier gas is continuously introduced into the reaction chamber of the second reactor to heat the fluidized powder so that the powder temperature is maintained within a preset temperature value.

[0028] S5. Pulsing a second reaction gas into the powder in the reaction chamber of the second reactor, maintaining the pressure in the reaction chamber of the second reactor within the target pressure value, and detecting the exhaust gas composition discharged from the reaction chamber of the second reactor until it is determined that the second reaction gas is excessive;

[0029] S6. If the second reaction gas is excessive, the powder is discharged into the purge chamber of the second reactor and an inert carrier gas is introduced into the purge chamber of the second reactor until the exhaust gas from the purge chamber of the second reactor is free of the second reaction gas and byproducts, thus completing one ALD growth cycle on the powder surface.

[0030] S7. Repeat steps S1 to S6 in the next ALD growth cycle unit, completing multiple ALD growth cycles on the partially coated powder surface in the upstream step until the coating on the powder surface reaches the target thickness;

[0031] S8. The coated powder is transported to the feeding tank using an inert carrier gas for cooling;

[0032] The powder includes powder that is not coated with a coating or partially coated powder from an upstream step in the coating process.

[0033] A method for coating powders by continuous atomic layer deposition, using the above-mentioned apparatus for coating powders by continuous atomic layer deposition, comprises the following steps:

[0034] F1. Using an inert carrier gas, the uncoated powder is transported to the reaction chamber of the first reactor of the ALD growth cycle. The inert carrier gas is continuously flowed into the reaction chamber of the first reactor to heat the fluidized powder and maintain the powder temperature within a predetermined range.

[0035] F2. Pulsing the first reaction gas into the powder in the reaction chamber of the first reactor, maintaining the pressure in the reaction chamber of the first reactor within the target pressure value, and detecting the composition of the exhaust gas discharged from the reaction chamber of the first reactor until it is determined that the first reaction gas is in excess;

[0036] F3. When the first reaction gas is excessive, the powder is discharged into the purge chamber of the first reactor, and an inert carrier gas is filled into the purge chamber of the first reactor until the exhaust gas discharged from the purge chamber of the first reactor does not contain the first reaction gas and by-products;

[0037] F4. The powder in the clean room of the first reactor is transported to the reaction chamber of the second reactor using an inert carrier gas. The inert carrier gas is continuously introduced into the reaction chamber of the second reactor to heat the fluidized powder and maintain the powder temperature within a preset temperature range.

[0038] F5. Pulsing a second reaction gas toward the powder in the reaction chamber of the second reactor, maintaining the pressure in the reaction chamber of the second reactor within the target pressure, and detecting the composition of the exhaust gas discharged from the reaction chamber of the second reactor until it is determined that the second reaction gas is in excess;

[0039] F6. If the second reaction gas is excessive, discharge the powder into the purge chamber of the second reactor and fill the purge chamber of the second reactor with an inert carrier gas until the exhaust gas from the purge chamber of the second reactor is free of the second reaction gas and byproducts.

[0040] F7. Using an inert carrier gas, the powder in the clean room of the second reactor is transferred to the reaction chamber of the third reactor. The inert carrier gas is continuously introduced into the reaction chamber of the third reactor to heat the fluidized powder and maintain the powder temperature within a predetermined range.

[0041] F8. Pulsing a third reaction gas toward the powder in the reaction chamber of the third reactor, maintaining the pressure in the reaction chamber of the third reactor within a target pressure, and detecting the composition of exhaust gas exhausted from the reaction chamber of the third reactor until it is determined that the third reaction gas is in excess;

[0042] F9. If the third reaction gas is excessive, discharge the powder into the purge chamber of the third reactor and fill the purge chamber of the third reactor with an inert carrier gas until the exhaust gas from the purge chamber of the third reactor is free of the third reaction gas and byproducts.

[0043] F10. The powder in the clean room of the third reactor is transported to the reaction chamber of the fourth reactor using an inert carrier gas. The inert carrier gas is continuously introduced into the reaction chamber of the fourth reactor to heat the fluidized powder and maintain the powder temperature within a preset temperature range.

[0044] F11. Pulsing the second reaction gas into the powder in the reaction chamber of the fourth reactor, maintaining the pressure in the reaction chamber of the fourth reactor within the target pressure, and detecting the composition of the exhaust gas discharged from the reaction chamber of the fourth reactor until it is determined that the second reaction gas is in excess;

[0045] F12. If the second reactant gas is excessive, discharge the powder into the purge chamber of the fourth reactor. Inert carrier gas is then introduced into the purge chamber of the fourth reactor until the exhaust gas from the purge chamber is free of the second reactant gas and byproducts, completing one ALD growth cycle on the powder surface.

[0046] F13. Repeat steps F1 to F12 in the next ALD growth cycle unit, completing multiple ALD growth cycles on the partially coated powder surface in the upstream step until the coating on the powder surface reaches the target thickness;

[0047] F14. Use an inert carrier gas to transport the coated powder to a feed tank for cooling.

[0048] The powder includes powder that is not coated with a coating or partially coated powder from an upstream step in the coating process.

[0049] Furthermore, the excess of the first reaction gas, the second reaction gas, or the third reaction gas is determined by the following steps:

[0050] Detecting the concentration C1 of the first reaction gas / the second reaction gas / the third reaction gas in the exhaust gas, and the concentration C2 of by-products generated by the reaction of the first reaction gas / the second reaction gas / the third reaction gas with the powder;

[0051] The excess of the first reaction gas, the second reaction gas, or the third reaction gas is determined based on whether C2 and C1 meet the judgment conditions.

[0052] The conditions for determining whether the first reaction gas, the second reaction gas, or the third reaction gas is excessive include:

[0053] C1 is not less than the first threshold, but C2 is not greater than the second threshold.

[0054] The beneficial effects of the present invention are: first, it includes multiple ALD growth cycle units connected in series, which can complete continuous atomic layer deposition, and each ALD cycle unit is divided into multiple reactors, which can respectively carry out reactions with different precursors, thereby reducing the time for replacing precursors in the same reaction chamber. In the present invention, when the cleanroom of the previous reactor discharges powder to the next reaction chamber, since the gas carrying the powder into the reaction chamber is an inert gas, the powder does not need to be purged and replaced after entering the new reaction chamber; when the reaction chamber discharges powder to the cleanroom, since only inert gas penetrates into the reaction chamber, it is not necessary to purge and replace the gas in the reaction chamber; and since the process of powder falling into the cleanroom is a process of volume exchange between gas and powder, the time of the pulse reaction gas in the reaction chamber is short, the content of residual reaction gas is small, the reaction gas brought into the cleanroom with the powder is small, and the volume of the cleanroom is approximately equal to the total volume of the powder in the reaction chamber. After the powder is discharged into the cleanroom, the gas brought in is very small. By introducing a small amount of inert gas to extract the residual gas, the gas in the cleanroom can be replaced in a very short time. Therefore, the entire ALD growth cycle saves the time of replacing the precursor gas in the reaction chamber, and the time saved by 100 ALD growth cycles is greater than 1 hour.

[0055] Secondly, the reaction chamber does not need to repeatedly replace the precursor gas, and the volume of inert gas used for purging in the purification chamber each time is much smaller than the capacity of the reaction chamber, saving the amount of inert gas used for purging.

[0056] Thirdly, a valve device between the reaction chamber and the cleanroom can be used to isolate the reaction chamber from the cleanroom, discharge powder from the reaction chamber to the cleanroom, and fluidize the powder within the reaction chamber. Fluidizing the powder within the reaction chamber allows for a more uniform atomic layer deposition layer to be formed on the powder surface. Currently, no device exists that can both fluidize and discharge powder within the reaction chamber.

[0057] Fourthly, since a plurality of independent exhaust pipes are attached to the fluidizing gas exhaust pipe in the valve device, the starting end of the independent exhaust pipe is connected to the fluidizing gas exhaust pipe, and the end of the independent exhaust pipe is away from the fluidizing gas exhaust pipe, each independent exhaust pipe is evenly provided with equal flow holes, and a hollow sleeve that can slide along the independent exhaust pipe is provided inside or outside the pipe, as well as an elastic body or a magnetic body that can apply pressure or tension to the sleeve, and the pressure or tension is directed to the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe, and through holes are evenly provided on the sleeve. When the independent exhaust pipe is ventilated so that the sleeve overcomes the pressure or tension and moves away from the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe to the end of the independent exhaust pipe, the through holes on the sleeve and the equal flow of the independent exhaust pipe are connected. The holes are aligned one by one, and the gas is discharged into the reaction chamber from the independent exhaust pipe. When the ventilation to the independent exhaust pipe stops or the air pressure is lower than the threshold, the sleeve approaches the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe under the pressure or tension until it approaches the starting end of the independent exhaust pipe. The through holes on the sleeve are staggered one by one with the equalizing flow holes of the independent exhaust pipe, and the gas stops being discharged into the reaction chamber from the independent exhaust pipe. The powder in the reaction chamber stops fluidizing and falls onto the surface of the valve device. The sleeve can effectively intercept the powder from entering the independent exhaust pipe or the fluidizing gas exhaust pipe, resulting in blockage of the equalizing flow holes, affecting the fluidization and coating effect of the powder, or causing the powder with saturated surface sites to enter the reaction chamber again, but the introduction of reaction gas makes it impossible for it to react with the reaction gas, resulting in waste of reaction gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] Figure 1 A structural diagram of a device for continuous atomic layer deposition of coated powders according to the present invention;

[0059] Figure 2 Another structural diagram of the apparatus for continuous atomic layer deposition of coated powders according to the present invention;

[0060] Figure 3 A structural diagram of a valve device;

[0061] Figure 4 for Figure 3 A partial enlarged view of the upper part;

[0062] Figure 5 Another structural diagram of the valve device

[0063] Figure 6 for Figure 5 A partial enlargement of the upper part. DETAILED DESCRIPTION

[0064] The principles and features of the present invention are described below with reference to the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0065] like Figure 1As shown, a device for continuous atomic layer deposition coating of powder includes multiple groups of ALD growth cycle units 3 connected in series through pipes, each ALD growth cycle unit 3 includes a first reactor 1 and a second reactor 2 connected in series, the first reactor 1 and the second reactor 2 both include a reaction chamber 4 and a purification chamber 5, and the purification chamber 5 is located below the reaction chamber 4.

[0066] Preferably, the reaction chamber 4 is further provided with a temperature detector and an air pressure detection device, as well as a stirring device 7 at the upper portion of the reaction chamber, the blades of the stirring device 7 extending to the bottom of the reaction chamber. The air pressure detection device can monitor the air pressure value inside the reaction chamber in real time. A heating device 8 is provided on the outer side of the lower portion of the reaction chamber. Each reaction chamber is connected to the inlet of a differential electrochemical mass spectrometer 10 through an exhaust gas exhaust pipe 9. The outlet of the differential electrochemical mass spectrometer 10 is connected to a vacuum pump 11. A filter device 12 is provided at the inlet of the exhaust gas exhaust pipe 9. The filter device 12 is used to prevent powder from flowing out of the reaction chamber along the exhaust gas. The side of the reaction chamber is also connected to the inlet of the material feed pipe 13, and the bottom of the clean room is connected to the inlet of the material feed pipe 14. The material feed pipe 13 and the material feed pipe 14 are both provided with vacuum valves, including butterfly valves or gate valves. Each clean room is also connected to the differential electrochemical mass spectrometer 10 and the vacuum pump 11 in sequence through the exhaust pipe. The capacity of the lower portion of the reaction chamber is greater than that of the clean room.

[0067] Preferably, a valve device is provided between the reaction chamber 4 and the purification chamber 5. The valve device can be operated between an open position and a closed position. The valve device has a disc plate 6. When the valve device is in the closed position, the purification chamber 5 and the reaction chamber 4 are isolated by the disc plate 6. The disc plate 6 includes flow-balancing holes evenly distributed on the side of the disc plate facing the reaction chamber. The flow-balancing holes are all connected to a fluidizing gas exhaust pipe in the disc plate. The flow-balancing holes can be used to evenly disperse the fluidizing gas and fluidized powder. The fluidizing gas exhaust pipe in the disc plate 6 is connected to the air inlet pipe 15. The air inlet pipe 15 is connected to the independent air inlet pipe attached to the common reaction gas inlet pipe (21a or 21b) and the common inert carrier gas inlet pipe 20 through the reaction gas exhaust valve 16 and the inert gas exhaust valve 17.

[0068] Preferably, the side of the disc plate 6 facing the purification chamber 5 is also provided with an exhaust hole, which is connected to the inert carrier gas exhaust valve 18 and the independent air inlet pipe attached to the inert carrier gas common air inlet pipe 20 in sequence through another fluidizing gas exhaust pipe in the disc plate 6.

[0069] To improve temperature uniformity, the inert gas introduced into the first reactor 1 or the second reactor 2 can be preheated. A stirring device 7, whose blades can be simple rod-shaped or fan-shaped, can stir the powder to achieve a more uniform temperature and facilitate fluidization. A pressure monitoring device is used to monitor the pressure inside the reaction chamber in real time, determining whether to introduce inert gas or reaction gas through the fluidizing gas inlet pipe and the amount of gas to be introduced. A heating device 8 located outside the reaction chamber can be used to heat the fluidized powder.

[0070] Furthermore, the disc plate 6 is made of heat-resistant material and can be a porous sintered plate sintered from stainless steel powder. The aperture of the flow-distributing hole is selected according to the particle size of the powder to be coated. While being as large as possible to facilitate the passage of airflow, it can effectively intercept the powder to prevent the powder from entering or preventing the powder from falling into the disc plate 6.

[0071] Preferably, the disc plate 6 includes an opening and closing device, which can be operated between blocking the flow-balancing hole and not blocking the flow-balancing hole.

[0072] As a preferred embodiment, Figure 3 As shown, Figure 4 for Figure 3A partial enlarged view of the upper part shows that the disc plate 6 includes an outer shell 64, in which a fluidizing gas exhaust pipe 61 is arranged along the central axis of the disc plate 6. A plurality of independent exhaust pipes 62 are attached to the fluidizing gas exhaust pipe 61. The starting end of the independent exhaust pipe 6 is connected to the fluidizing gas exhaust pipe, and the end of the independent exhaust pipe is away from the fluidizing gas exhaust pipe and is closed. Flow equalization holes 63 are evenly arranged on each independent exhaust pipe 62, and the flow equalization holes extend from the independent exhaust pipe to the surface of the outer shell 64. A hollow sleeve 65 that can slide along the independent exhaust pipe is sleeved in each independent exhaust pipe 62, as well as an elastic body 66 or a magnetic body that can apply pressure or tension to the sleeve 65, and the pressure or tension is directed to the fluidizing gas exhaust pipe 61 along the axial direction of the independent exhaust pipe 62. Through holes 67 are evenly arranged on the sleeve 65, and the end of the sleeve 65 close to the end of the independent exhaust pipe 62 is closed. The length of the independent exhaust pipe 62 is greater than the length of the sleeve 65 in the independent exhaust pipe 62. When When ventilation to the independent exhaust pipe causes the sleeve to overcome pressure or tension and move along the axial direction of the independent exhaust pipe away from the fluidizing gas exhaust pipe to the end of the independent exhaust pipe, the through holes on the sleeve are aligned one-to-one with the equalizing flow holes of the independent exhaust pipe, and the gas is discharged into the reaction chamber from the independent exhaust pipe. When ventilation to the independent exhaust pipe stops or the air pressure is lower than the threshold, the sleeve moves along the axial direction of the independent exhaust pipe close to the fluidizing gas exhaust pipe to the beginning of the independent exhaust pipe under the pressure or tension, and the sleeve blocks the equalizing flow holes of the independent exhaust pipe outside the sleeve, and the gas stops being discharged into the reaction chamber from the independent exhaust pipe. The powder in the reaction chamber stops fluidizing and falls onto the surface of the valve device, and the sleeve can effectively intercept the powder from entering the independent exhaust pipe or the fluidizing gas exhaust pipe, resulting in blockage of the equalizing flow holes, affecting the fluidization and coating effect of the powder, or causing the powder with saturated surface sites to enter the reaction chamber again, but the introduction of reaction gas prevents it from reacting with the reaction gas, resulting in waste of reaction gas.

[0073] As another preferred embodiment, Figure 5 As shown, Figure 6 for Figure 5The upper part of the partial enlarged view shows that the disc plate 6 includes a shell 64. A fluidizing gas exhaust pipe 61 is arranged along the central axis of the disc plate 6 in the shell. A plurality of independent exhaust pipes 62 are attached to the fluidizing gas exhaust pipe 61. The starting end of the independent exhaust pipe is connected to the fluidizing gas exhaust pipe, and the end of the independent exhaust pipe is away from the fluidizing gas exhaust pipe and is not closed. Each independent exhaust pipe is evenly provided with flow holes. The shell 64 is provided with a window 68 aligned with each independent exhaust pipe. A hollow sleeve 65 that can slide along the independent exhaust pipe 62 is arranged on the outer surface of each independent exhaust pipe 62. An elastic body 66 or a magnetic body is provided inside the shell or outside the independent exhaust pipe to apply pressure or tension to the sleeve 65. The pressure or tension is directed along the axial direction of the independent exhaust pipe 62 to the fluidizing gas exhaust pipe 61. Through holes 67 are evenly provided on the sleeve 65. The length of the window 68 along the axial direction of the independent exhaust pipe is smaller than the sleeve 65 and the independent exhaust pipe 62. The width of the window 68 is not greater than the diameter of the sleeve 65. The length of the sleeve 65 is smaller than the shortest distance from the starting end of the corresponding independent exhaust pipe 62 to the shell 64 along the axial direction of the independent exhaust pipe. The length of 65 is greater than the length of the independent exhaust pipe 62 in the sleeve 65, and the end of the sleeve 65 near the end of the independent exhaust pipe is closed. When the independent exhaust pipe is ventilated to make the sleeve overcome the pressure or tension and move along the axial direction of the independent exhaust pipe away from the fluidizing gas exhaust pipe to the end of the independent exhaust pipe, the sleeve blocks the equalizing flow hole of the independent exhaust pipe in the sleeve, and the gas is discharged into the reaction chamber from the independent exhaust pipe. When the independent exhaust pipe is stopped from being ventilated or the air pressure is lower than the threshold, the sleeve moves along the axial direction of the independent exhaust pipe close to the fluidizing gas exhaust pipe to the beginning of the independent exhaust pipe under the pressure or tension. The through hole on the sleeve is staggered one-to-one with the equalizing flow hole of the independent exhaust pipe, and the gas stops being discharged into the reaction chamber from the independent exhaust pipe. The powder in the reaction chamber stops fluidizing and falls on the surface of the valve device. The sleeve and the window cooperate to effectively intercept the powder from entering the independent exhaust pipe or the fluidizing gas exhaust pipe, resulting in blockage of the equalizing flow hole affecting the fluidization and coating effect of the powder, or causing the powder with saturated surface sites to enter the reaction chamber again, but the introduction of reaction gas makes it impossible to react with the reaction gas, resulting in waste of reaction gas.

[0074] Furthermore, the outlet of the feed outlet pipe 14 of the first reactor 1 in each ALD growth cycle unit 3 is connected to the inlet of the feed inlet pipe 13 of the second reactor 2. During the AlD coating reaction, the powder undergoes separate reactions with multiple precursor gases, which are not completed within a single reaction chamber. The reaction gas exhaust valves 16 of the two reactor inlet pipes 15 in each ALD growth cycle unit 3 are respectively connected to the common reaction gas inlet pipe 21a and the independent inlet pipe attached to the common reaction gas inlet pipe 21b. The common reaction gas inlet pipe 21a of the first reactor 1 is supplied with gas from a first reaction gas source 22a, the common reaction gas inlet pipe 21b of the second reactor 2 is supplied with gas from a second reaction gas source 22b, and the common inert carrier gas inlet pipe 20 is supplied with gas from an inert carrier gas source 23.

[0075] Specifically, multiple ALD growth cycle units 3 are connected in series through pipelines, the inlet of the material feed pipe 13 of the first reactor of the first ALD growth cycle unit 3 is connected to the loading tank 24, starting from the first ALD growth cycle unit 3, the outlet of the material feed pipe 14 of the second reactor 2 of the ALD growth cycle unit is connected to the inlet of the material feed pipe 13 of the first reactor 1 of the next ALD growth cycle unit 3, and the outlet of the material feed pipe 14 of the second reactor 2 of the last ALD growth cycle unit 3 is connected to the unloading tank 19. There are at least two ALD growth cycle units 3, and the number of ALD growth cycle units 3 is set according to the number of ALD growth cycles required to form a coating on the powder surface. The number of ALD growth cycle units 3 is equal to the number of ALD growth cycles.

[0076] A method for coating powders by continuous atomic layer deposition, using the above-mentioned apparatus for coating powders by continuous atomic layer deposition, comprises the following steps:

[0077] Step 1: Using an inert carrier gas, uncoated powder is transported to the reaction chamber of the first reactor 1 of the ALD growth cycle unit 3. The inert carrier gas is continuously introduced into the reaction chamber 4 of the first reactor 1 to heat the fluidized powder and maintain the powder temperature within a predetermined range. The total volume of the powder does not exceed the volume of the cleanroom.

[0078] Step 2: Pulsing the first reaction gas into the powder in the reaction chamber 4 of the first reactor 1, maintaining the pressure of the reaction chamber 4 of the first reactor 1 within the target pressure value, and detecting the composition of the tail gas discharged from the reaction chamber of the first reactor 1 until it is determined that the first reaction gas is excessive;

[0079] Step 3: When it is determined that the first reaction gas is excessive, the powder is discharged into the purification chamber 5 of the first reactor 1, and an inert carrier gas is filled into the purification chamber 5 of the first reactor 1 until the tail gas discharged from the purification chamber 5 of the first reactor 1 does not contain the first reaction gas and by-products;

[0080] Step 4: Using an inert carrier gas, the powder in the purification chamber 5 of the first reactor 1 is transported to the reaction chamber 4 of the second reactor 2. The inert carrier gas is continuously introduced into the reaction chamber 4 of the second reactor to heat the fluidized powder so that the powder temperature is maintained within a preset temperature value.

[0081] Step 5: Pulsing the second reaction gas into the powder in the reaction chamber 4 of the second reactor 2, maintaining the pressure of the reaction chamber 4 of the second reactor 2 within the target pressure value, and detecting the components of the tail gas discharged from the reaction chamber 4 of the second reactor 2 until it is determined that the second reaction gas is excessive;

[0082] Step 6: When it is determined that the second reaction gas is excessive, the powder is discharged into the purge chamber of the second reactor, and an inert carrier gas is introduced into the purge chamber 5 of the second reactor until the exhaust gas discharged from the purge chamber 5 of the second reactor 2 is free of the second reaction gas and by-products, thus completing one ALD growth cycle on the powder surface.

[0083] Step 7: Repeat steps 1 to 6 in the next ALD growth cycle unit 3, completing multiple ALD growth cycles on the partially coated powder surface in the upstream step until the coating on the powder surface reaches the target thickness;

[0084] Step 8: Use an inert carrier gas to transport the coated powder to the discharge tank 19 for cooling.

[0085] Furthermore, the following steps are performed to determine whether the first reaction gas or the second reaction gas is excessive in step 2 and step 5:

[0086] Detecting the concentration C1 of the first reaction gas / the second reaction gas in the exhaust gas, and the concentration C2 of by-products generated by the reaction between the first reaction gas / the second reaction gas and the powder;

[0087] The first reaction gas or the second reaction gas is judged to be excessive based on whether C2 and C1 meet the judgment condition. Specifically, the judgment condition for judging the first reaction gas or the second reaction gas to be excessive includes: C1 is not less than a first threshold, but C2 is not greater than a second threshold.

[0088] Furthermore, if an ALD growth cycle requires the alternating introduction of three reaction gases, for example, when coating the powder surface with Li3PO4, it is necessary to first introduce the first reaction gas, lithium tert-butoxide, into the reaction chamber, then introduce an inert gas to replace the lithium tert-butoxide, then introduce the second reaction gas, water vapor, then introduce an inert gas to replace the water vapor, then introduce the third reaction gas, trimethyl phosphate, then introduce an inert gas to replace the trimethyl phosphate, and then introduce the second reaction gas, water vapor, to complete an ALD growth cycle. At this time, if Figure 2 As shown, each ALD growth cycle unit 3 includes two groups of first reactors 1 and second reactors 2 that are alternately connected in series in the order of first reactor 1 to second reactor 2. The outlet of the material outlet pipe 14 of the first reactor 1 in each ALD growth cycle unit 3 is connected to the inlet of the material inlet pipe 13 of the second reactor 2, and the outlet of the material outlet pipe 14 of the first second reactor 2 in each ALD growth cycle unit 3 is connected to the inlet of the material inlet pipe 13 of the second first reactor 1.

[0089] The reaction gas exhaust valve 16 of the inlet pipe 15 of the first first reactor 1 in each ALD growth cycle unit 3 is connected to an independent inlet pipe attached to the reaction gas common inlet pipe 21a, the reaction gas exhaust valve 16 of the inlet pipe 15 of the second first reactor 1 is connected to an independent inlet pipe attached to the reaction gas common inlet pipe 21c, the reaction gas exhaust valve 16 of the inlet pipes 15 of the first and second second reactors 2 are connected to independent inlet pipes attached to the reaction gas common inlet pipe 21b, and the inlet pipes 15 of all reactors are also connected to independent inlet pipes attached to the inert carrier gas common inlet pipe 20 through the inert gas exhaust valve 17. The reaction gas common inlet pipe 21a of the first first reactor 1 is supplied by the first reaction gas source 22a, the reaction gas common inlet pipes 21b of the two second reactors 2 are supplied by the second reaction gas source 22b, the reaction gas common inlet pipe 21c of the second first reactor 1 is supplied by the third reaction gas source 22c, and the inert carrier gas common inlet pipes 20 are all supplied by the inert carrier gas source 23.

[0090] Multiple ALD growth cycle units 3 are connected in series via pipelines. The inlet of the feed inlet pipe 13 of the first first reactor of the first ALD growth cycle unit 3 is connected to the loading tank 24. Starting from the first ALD growth cycle unit 3, the outlet of the feed outlet pipe 14 of the second second reactor 2 of the ALD growth cycle unit is connected to the inlet of the feed inlet pipe 13 of the first first reactor 1 of the next ALD growth cycle unit 3. The outlet of the feed outlet pipe 14 of the second second reactor 2 of the last ALD growth cycle unit 3 is connected to the unloading tank 19. The number of ALD growth cycle units 3 is equal to the number of ALD growth cycles, and the number of ALD growth cycle units 3 is at least two.

[0091] Preferably, the side of the disc plate 6 facing the purification chamber 5 is also provided with an exhaust hole, which is connected to the inert carrier gas exhaust valve 18 and the independent air inlet pipe attached to the inert carrier gas common air inlet pipe 20 in sequence through another fluidizing gas exhaust pipe in the disc plate 6.

[0092] A method for coating powders by continuous atomic layer deposition, using the above-mentioned apparatus for coating powders by continuous atomic layer deposition, comprises the following steps:

[0093] Step 1: Using an inert carrier gas, the uncoated powder is transported to the reaction chamber of the first reactor 1 of the ALD growth cycle unit 3. The inert carrier gas is continuously introduced into the reaction chamber 4 of the first reactor 1 to heat the fluidized powder and maintain the powder temperature within a predetermined temperature range.

[0094] Step 2: Pulsing the first reaction gas into the powder in the reaction chamber 4 of the first reactor 1, maintaining the pressure of the reaction chamber 4 of the first reactor 1 within the target pressure value, and detecting the composition of the tail gas discharged from the reaction chamber of the first reactor 1 until it is determined that the first reaction gas is excessive;

[0095] Step 3: When it is determined that the first reaction gas is excessive, the powder is discharged into the purification chamber 5 of the first first reactor 1, and an inert carrier gas is filled into the purification chamber 5 of the first first reactor until the exhaust gas discharged from the purification chamber 5 of the first first reactor 1 does not contain the first reaction gas and by-products;

[0096] Step 4: Using an inert carrier gas, the powder in the purification chamber 5 of the first reactor 1 is transported to the reaction chamber 4 of the first second reactor 2. The inert carrier gas is continuously introduced into the reaction chamber 4 of the first second reactor to heat the fluidized powder and maintain the powder temperature within a preset temperature value.

[0097] Step 5: Pulsing the second reaction gas into the powder in the reaction chamber 4 of the first second reactor 2, maintaining the pressure of the reaction chamber 4 of the first second reactor 2 within the target pressure value, and detecting the composition of the tail gas discharged from the reaction chamber 4 of the first second reactor 2 until it is determined that the second reaction gas is excessive;

[0098] Step 6: When it is determined that the second reaction gas is excessive, the powder is discharged into the purification chamber of the first second reactor, and an inert carrier gas is filled into the purification chamber 5 of the first second reactor until the tail gas discharged from the purification chamber 5 of the first second reactor 2 does not contain the second reaction gas and by-products;

[0099] Step 7: Using an inert carrier gas, the powder in the purification chamber 5 of the first second reactor 2 is transported to the reaction chamber 4 of the second first reactor 1. The inert carrier gas is continuously introduced into the reaction chamber 4 of the second first reactor to heat the fluidized powder and maintain the powder temperature within a preset temperature value.

[0100] Step 8: Pulsing the third reaction gas into the powder in the reaction chamber 4 of the second first reactor 1, maintaining the pressure of the reaction chamber 4 of the second first reactor 1 within the target pressure value, and detecting the components of the exhaust gas discharged from the reaction chamber 4 of the second first reactor 1 until it is determined that the third reaction gas is excessive;

[0101] Step 9: When it is determined that the third reaction gas is excessive, the powder is discharged into the purification chamber of the second first reactor, and an inert carrier gas is filled into the purification chamber 5 of the second first reactor until the tail gas discharged from the purification chamber 5 of the second first reactor 1 does not contain the third reaction gas and by-products;

[0102] Step 10: Using an inert carrier gas, the powder in the purification chamber 5 of the second first reactor 1 is transported to the reaction chamber 4 of the second second reactor 2. The inert carrier gas is continuously introduced into the reaction chamber 4 of the second second reactor to heat the fluidized powder and maintain the powder temperature within a preset temperature value.

[0103] Step 11: Pulsing the second reaction gas into the powder in the reaction chamber 4 of the second second reactor 2, maintaining the pressure of the reaction chamber 4 of the second second reactor 2 within the target pressure value, and detecting the composition of the tail gas discharged from the reaction chamber 4 of the second second reactor 2 until it is determined that the second reaction gas is excessive;

[0104] Step 12: When it is determined that the second reaction gas is excessive, the powder is discharged into the purge chamber of the second second reactor, and an inert carrier gas is filled into the purge chamber 5 of the second second reactor until the exhaust gas discharged from the purge chamber 5 of the second second reactor 1 is free of the second reaction gas and by-products, i.e., one ALD growth cycle is completed on the powder surface.

[0105] Step 13: Repeat steps 1 to 13 in the next ALD growth cycle unit 3 to complete multiple ALD growth cycles on the powder surface partially coated in the upstream step until the coating on the powder surface reaches the target thickness;

[0106] Step 14: Use an inert carrier gas to transport the coated powder to the discharge tank 19 for cooling.

[0107] Furthermore, the following steps are performed to determine whether the first reaction gas or the third reaction gas is excessive in step 2 and step 8, or whether the second reaction gas is excessive in step 5 and step 12:

[0108] Detecting the concentration C1 of the first reaction gas / the second reaction gas / the third reaction gas in the exhaust gas, and the concentration C2 of by-products generated by the reaction of the first reaction gas / the second reaction gas / the third reaction gas with the powder;

[0109] The first reaction gas, the second reaction gas, or / and the third reaction gas is judged to be excessive based on whether C2 and C1 meet the discrimination conditions. Specifically, the discrimination conditions for judging the first reaction gas, the second reaction gas, or / and the third reaction gas to be excessive include: C1 is not less than a first threshold value, but C2 is not greater than a second threshold value.

[0110] Example 1

[0111] The method for coating powder using the continuous atomic layer deposition coating powder device of the present invention can realize coating multiple layers of aluminum oxide on graphite powder. The specific operation steps are as follows:

[0112] Step 1: Graphite powder is transported to the reaction chamber of the first reactor 1 of the ALD growth cycle unit 3 using an inert carrier gas. An inert carrier gas such as nitrogen or hydrogen is continuously introduced into the reaction chamber 4 of the first reactor 1 to heat the fluidized powder until the powder temperature reaches 180°C, which is required for coating.

[0113] Step 2: In the reaction chamber 4 of the first reactor 1, an inert carrier gas is continuously sprayed toward the powder through the flow-balancing holes of the butterfly plate 6 to fluidize the powder. At the same time, the first reaction gas TMA (TMA stands for trimethylaluminum) is pulsed for 0.1 second at a time interval of 5 seconds. The tail gas pipe in the reaction chamber 4 of the first reactor 1 is simultaneously evacuated to maintain the pressure of the reaction chamber 4 of the first reactor 1 within the target pressure value. The components of the tail gas discharged from the reaction chamber of the first reactor 1 are detected by differential electrochemical mass spectrometry.

[0114] Step 3: When the concentration of TMA detected in the tail gas component reaches a preset threshold value C1 and the by-product methane is not greater than the preset threshold value C2, it means that as TMA increases, no more methane is produced, the oxygen-containing functional group sites on the surface of the powder have all reacted with TMA, the surface sites of the powder are saturated into a monolayer, and TMA is excessive. Stop venting to the reaction chamber of the first reactor 1, wait for the powder to settle, and then discharge the powder into the purification chamber 5 of the first reactor 1. Inert carrier gas such as nitrogen or hydrogen is filled into the purification chamber 5 of the first reactor 1, and the tail gas pipe in the purification chamber 5 of the first reactor 1 is vacuumed at the same time until the tail gas discharged from the purification chamber 5 of the first reactor 1 does not contain TMA and by-products;

[0115] Step 4: Use an inert carrier gas to transport the powder in the clean room of the first reactor to the reaction chamber 4 of the second reactor 2. Continuously introduce an inert carrier gas such as nitrogen or hydrogen into the reaction chamber 4 of the second reactor to heat the fluidized powder until the powder temperature reaches 180°C required for coating.

[0116] Step 5: In the reaction chamber 4 of the second reactor 2, an inert carrier gas is continuously sprayed toward the powder through the flow-balancing holes of the butterfly plate 6 to fluidize the powder. At the same time, water vapor is pulsed toward the powder for 0.1 seconds at a time interval of 5 seconds. The tail gas pipe in the reaction chamber 4 of the second reactor 2 is simultaneously evacuated to maintain the pressure of the reaction chamber 4 of the second reactor 2 within the target pressure value. The components of the tail gas discharged from the reaction chamber 4 of the second reactor 2 are detected. At high temperature, trimethylaluminum reacts with water vapor to generate aluminum oxide and methane.

[0117] Step 6: When the exhaust gas component detects that the water vapor reaches a preset threshold value C1 and the methane concentration does not exceed the preset threshold value C2, the ventilation to the reaction chamber of the second reactor 2 is stopped, and the powder is discharged into the purification chamber of the second reactor after settling. The purification chamber 5 of the second reactor is filled with an inert carrier gas, and the exhaust pipe in the purification chamber of the second reactor 2 is simultaneously evacuated until the exhaust gas discharged from the purification chamber 5 of the second reactor 2 does not contain water vapor and by-product methane, that is, the aluminum oxide coating is completed once on the powder surface;

[0118] Step 7: Repeat steps 1 to 6 in the next ALD growth cycle unit 3, completing multiple ALD growth cycles on the partially coated powder surface in the upstream step until the coating on the powder surface reaches the target thickness;

[0119] Step 8: Use an inert carrier gas to transport the coated powder to the discharge tank 19 for cooling.

[0120] Example 2

[0121] The continuous atomic layer deposition coating powder coating method of the present invention can realize the coating of Li3PO4 on graphite powder. The specific operation steps are as follows:

[0122] Step 1: Graphite powder is transported to the reaction chamber of the first reactor 1 of the ALD growth cycle unit 3 using an inert carrier gas. An inert carrier gas such as nitrogen or hydrogen is continuously introduced into the reaction chamber 4 of the first reactor 1 to heat the fluidized powder until the powder temperature reaches 180°C, which is required for coating.

[0123] Step 2: In the reaction chamber 4 of the first reactor 1, an inert carrier gas is continuously sprayed toward the powder through the flow-balancing holes of the butterfly plate 6 to fluidize the powder. Simultaneously, the first reaction gas, lithium tert-butoxide, is pulsed toward the powder for 0.1 seconds at 5 second intervals. Simultaneously, a vacuum is evacuated in the tail gas pipe in the reaction chamber 4 of the first reactor to maintain the pressure in the reaction chamber 4 of the first reactor 1 within the target pressure value. The components of the tail gas discharged from the reaction chamber of the first reactor 1 are detected until it is determined that the first reaction gas is in excess.

[0124] Step 3: When the tail gas component detects that the concentration of lithium tert-butoxide reaches a preset threshold value C1 and the by-product methane is not greater than the preset threshold value C2, it means that as the lithium tert-butoxide increases, no more methane is produced, the oxygen-containing functional group sites on the surface of the powder have all reacted with lithium tert-butoxide, the surface sites of the powder are saturated into a monolayer, and the lithium tert-butoxide is excessive. The ventilation to the reaction chamber of the first first reactor 1 is stopped, and the powder is allowed to settle. At this time, the powder is discharged into the purification chamber 5 of the first first reactor 1, and an inert carrier gas is filled into the purification chamber 5 of the first first reactor. The tail gas pipe in the purification chamber of the first first reactor is simultaneously evacuated until the tail gas discharged from the purification chamber 5 of the first first reactor 1 does not contain lithium tert-butoxide and methane;

[0125] Step 4: Using an inert carrier gas, the powder in the purification chamber 5 of the first reactor 1 is transported to the reaction chamber 4 of the first second reactor 2. The inert carrier gas is continuously introduced into the reaction chamber 4 of the first second reactor to heat the fluidized powder until the powder temperature reaches 180°C, which is required for coating.

[0126] Step 5: In the reaction chamber 4 of the first second reactor 2, an inert carrier gas is continuously sprayed toward the powder through the flow-balancing holes of the butterfly plate 6 to fluidize the powder. Simultaneously, the second reaction gas, water vapor, is pulsed toward the powder for 0.1 seconds at 5 second intervals. The tail gas pipe in the reaction chamber of the first second reactor 2 is simultaneously evacuated to maintain the pressure in the reaction chamber 4 of the first second reactor 2 within the target pressure value. The components of the tail gas discharged from the reaction chamber 4 of the first second reactor 2 are detected until it is determined that the second reaction gas is excessive. Lithium tert-butoxide reacts with water vapor at high temperature to generate lithium oxide and methane.

[0127] Step 6: When the exhaust gas component detects that the water vapor reaches a preset threshold value C1 and the methane concentration does not exceed the preset threshold value C2, stop venting to the reaction chamber of the first second reactor 2, wait for the powder to settle, discharge the powder into the purification chamber of the first second reactor, fill the purification chamber 5 of the first second reactor with an inert carrier gas, and simultaneously evacuate the exhaust pipe in the purification chamber of the first second reactor until the exhaust gas discharged from the purification chamber 5 of the first second reactor 2 does not contain the second reaction gas and by-products;

[0128] Step 7: Using an inert carrier gas, the powder in the purification chamber 5 of the first second reactor 2 is transported to the reaction chamber 4 of the second first reactor 1. The inert carrier gas is continuously introduced into the reaction chamber 4 of the second first reactor to heat the fluidized powder until the powder temperature reaches 180° C. required for coating.

[0129] Step 8: In the reaction chamber 4 of the second first reactor 1, an inert carrier gas is continuously sprayed toward the powder through the flow-balancing holes of the butterfly plate 6 to fluidize the powder. Simultaneously, a third reaction gas, trimethyl phosphate, is pulsed toward the powder for 0.1 seconds at 5-second intervals. Simultaneously, a vacuum is evacuated in the tail gas pipe of the reaction chamber of the second first reactor to maintain the pressure in the reaction chamber 4 of the second first reactor 1 within the target pressure value. The components of the tail gas discharged from the reaction chamber 4 of the second first reactor 1 are detected until it is determined that the third reaction gas is in excess.

[0130] Step 9: When the concentration of trimethyl phosphate detected in the tail gas component reaches a preset threshold value C1 and the by-product methane is not greater than the preset threshold value C2, it means that as the trimethyl phosphate increases, no more methane is produced, the oxygen-containing functional group sites on the surface of the powder have all reacted with trimethyl phosphate, the surface sites of the powder are saturated into a monolayer, and the trimethyl phosphate is excessive. Stop ventilation to the reaction chamber of the second first reactor 1, wait for the powder to settle, and then discharge the powder into the purification chamber of the second first reactor. Fill the purification chamber 5 of the second first reactor with inert carrier gas, and simultaneously evacuate the tail gas pipe in the purification chamber of the second first reactor until the tail gas discharged from the purification chamber 5 of the second first reactor 1 does not contain trimethyl phosphate and methane;

[0131] Step 10: Using an inert carrier gas, the powder in the purification chamber 5 of the second first reactor 1 is transported to the reaction chamber 4 of the second second reactor 2. The inert carrier gas is continuously introduced into the reaction chamber 4 of the second second reactor to heat the fluidized powder and maintain the powder temperature within a preset temperature value.

[0132] Step 11: In the reaction chamber 4 of the second-second reactor 2, an inert carrier gas is continuously sprayed toward the powder through the equalizing holes of the butterfly plate 6 to fluidize the powder. Simultaneously, the second reaction gas, water vapor, is pulsed toward the powder for 0.1 seconds at a time interval of 5 seconds. The tail gas pipe in the reaction chamber of the second-second reactor is simultaneously evacuated to maintain the pressure of the reaction chamber 4 of the second-second reactor 2 within the target pressure value. The components of the tail gas discharged from the reaction chamber 4 of the second-second reactor 2 are detected until it is determined that the second reaction gas is excessive. Lithium oxide reacts with trimethyl phosphate and water vapor at high temperature to generate lithium phosphate and methane.

[0133] Step 12: When the exhaust gas component detects that the water vapor concentration reaches a preset threshold value C1 and the methane concentration does not exceed a preset threshold value C2, the ventilation to the reaction chamber of the second second reactor 2 is stopped. After the powder settles, the powder is discharged into the purge chamber of the second second reactor. An inert carrier gas is filled into the purge chamber 5 of the second second reactor. The exhaust pipe in the purge chamber of the second second reactor is simultaneously evacuated until the exhaust gas discharged from the purge chamber 5 of the second second reactor 1 does not contain the second reaction gas and by-products. In other words, one ALD growth cycle is completed on the powder surface.

[0134] Step 13: Repeat steps 1 to 12 in the next ALD growth cycle unit 3 to complete multiple ALD growth cycles on the powder surface partially coated in the upstream step until the coating on the powder surface reaches the target thickness;

[0135] Step 14: Use an inert carrier gas to transport the coated powder to the discharge tank 19 for cooling.

[0136] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the scope of protection of the present invention.

Claims

1. A reactor, characterized in that: include: A reaction chamber and a purification chamber, wherein the purification chamber is located below the reaction chamber, a valve device is provided between the reaction chamber and the purification chamber, the valve device can be operated between an open position and a closed position, the valve device has a disc plate, when the valve device is in the closed position, the purification chamber and the reaction chamber are isolated by the disc plate, the disc plate is constructed to include flow balancing holes uniformly distributed on the side of the disc plate facing the reaction chamber, and a fluidizing gas exhaust pipe located in the disc plate and connected to all the flow balancing holes; The reaction chamber is provided with an air pressure detection device and a temperature sensor, the reaction chamber is provided with a heating device outside, the reaction chamber is connected to a differential electrochemical mass spectrometer and a vacuum pump in sequence through an exhaust gas exhaust pipe, a filter is provided at the inlet of the exhaust gas exhaust pipe to prevent particle inhalation, the reaction chamber is also connected to the outlet of the feed inlet pipe, the fluidizing gas exhaust pipe is connected to the air inlet pipe, and the air inlet pipe is connected to a reaction gas common air inlet pipe and an independent air inlet pipe attached to the inert carrier gas common air inlet pipe through a reaction gas exhaust valve and an inert carrier gas exhaust valve respectively; The bottom of the purification chamber is connected to the inlet of the material delivery pipe, and the purification chamber is also connected to an independent air inlet pipe attached to the inert carrier gas common air inlet pipe through an inert carrier gas exhaust valve, and the purification chamber is also connected to the differential electrochemical mass spectrometer and the vacuum pump in sequence through the tail gas pipe; The disc plate comprises a shell, a fluidizing gas exhaust pipe is arranged inside the shell along the center axis of the disc plate, a plurality of independent exhaust pipes are attached to the fluidizing gas exhaust pipe, the start end of the independent exhaust pipe is connected to the fluidizing gas exhaust pipe, the end of the independent exhaust pipe is far away from the fluidizing gas exhaust pipe, and each independent exhaust pipe is evenly provided with flow equalization holes; The disc plate also includes an opening and closing device, which operates in blocking the flow-balancing hole and not blocking the flow-balancing hole. The opening and closing device is arranged in the housing in the following manner: The end of the independent exhaust pipe is closed, and the flow-averaging hole extends from the independent exhaust pipe to the surface of the shell. A hollow sleeve that can slide along the independent exhaust pipe is sleeved in each independent exhaust pipe, and an elastic body or a magnetic body that can apply pressure or tension to the sleeve, and the pressure or tension is directed to the fluidizing gas exhaust pipe along the axis of the independent exhaust pipe. Through holes are evenly arranged on the sleeve, and one end of the sleeve close to the end of the independent exhaust pipe is closed, and the length of the independent exhaust pipe is greater than the length of the sleeve in the independent exhaust pipe; When ventilation to the independent exhaust pipe causes the sleeve to overcome the pressure or tension and move axially away from the fluidizing gas exhaust pipe along the independent exhaust pipe to near the end of the independent exhaust pipe, the through holes on the sleeve are aligned one-to-one with the flow equalizing holes of the independent exhaust pipe; when ventilation to the independent exhaust pipe is stopped or the air pressure is lower than the threshold, the sleeve moves axially close to the fluidizing gas exhaust pipe along the independent exhaust pipe under the pressure or tension to near the beginning of the independent exhaust pipe, and the sleeve blocks the flow equalizing holes of the independent exhaust pipe.

2. The reactor according to claim 1, characterized in that The disc plate is provided with an exhaust hole on the side facing the purification chamber, and the exhaust hole is connected to the inert carrier gas exhaust valve and the independent air inlet pipe attached to the inert carrier gas common air inlet pipe in sequence through another fluidizing gas exhaust pipe in the disc plate.

3. The reactor according to claim 1, characterized in that A stirring device is arranged in the reaction chamber.

4. The reactor according to claim 1, characterized in that The opening and closing device can also be arranged in the shell in another way, the end of the independent exhaust pipe is not closed, the shell is provided with a window aligned with each independent exhaust pipe, each independent exhaust pipe is provided with a hollow sleeve that can slide along the independent exhaust pipe, an elastic body or a magnetic body that can apply pressure or tension to the sleeve is provided inside the shell or outside the independent exhaust pipe, the pressure or tension is directed to the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe, through holes are evenly arranged on the sleeve, the length of the window along the axial direction of the independent exhaust pipe is smaller than the sleeve and the independent exhaust pipe, the width of the window is not larger than the diameter of the sleeve, and the length of the sleeve is smaller than the diameter of the independent exhaust pipe in the sleeve. The shortest distance from the end of the independent exhaust pipe to the shell along the axial direction of the independent exhaust pipe, the length of the sleeve is greater than the length of the independent exhaust pipe in the sleeve, and the end of the sleeve close to the end of the independent exhaust pipe is closed. When the independent exhaust pipe is ventilated to make the sleeve overcome the pressure or tension and move along the axial direction of the independent exhaust pipe away from the fluidizing gas exhaust pipe to the end of the independent exhaust pipe, the through holes on the sleeve are aligned one-to-one with the equalizing holes of the independent exhaust pipe. When the independent exhaust pipe is stopped from being ventilated or the air pressure is lower than the threshold, the sleeve moves close to the fluidizing gas exhaust pipe along the axial direction of the independent exhaust pipe under the pressure or tension to the starting end of the independent exhaust pipe, and the sleeve blocks the equalizing holes of the independent exhaust pipe.

5. A device for continuous atomic layer deposition of coated powders, characterized in that: The invention comprises a reactor as claimed in any one of claims 1 to 4, wherein every two of the reactors constitute an ALD growth cycle unit, the outlet of the material delivery pipe of the first reactor is connected to the inlet of the material delivery pipe of the second reactor, the common reaction gas inlet pipe of the first reactor is supplied with gas by a first reaction gas source, the common reaction gas inlet pipe of the second reactor is supplied with gas by a second reaction gas source, and the common inert carrier gas inlet pipes are both supplied with gas by an inert carrier gas source; Multiple ALD growth cycle units are connected in series in sequence, the inlet of the feed inlet pipe of the first reactor of the first ALD growth cycle unit is connected to the loading tank, the outlet of the feed outlet pipe of the second reactor of the ALD growth cycle unit starting from the first ALD growth cycle unit is connected to the inlet of the feed inlet pipe of the first reactor of the next ALD growth cycle unit, and the outlet of the feed outlet pipe of the second reactor of the last ALD growth cycle unit is connected to the unloading tank.

6. A method for coating powder by continuous atomic layer deposition, characterized in that: The apparatus for continuous atomic layer deposition coating powder as claimed in claim 5 comprises the following steps: S1. Using an inert carrier gas to transport the uncoated powder to the reaction chamber of the first reactor of the ALD growth cycle unit, continuously passing an inert carrier gas into the reaction chamber of the first reactor to heat the fluidized powder so that the powder temperature is maintained within a preset temperature value; S2. Pulsing a first reaction gas to the powder in the reaction chamber of the first reactor, maintaining the pressure of the reaction chamber of the first reactor within the target pressure value, and detecting the exhaust gas components discharged from the reaction chamber of the first reactor until it is determined that the first reaction gas is excessive; S3. When the first reaction gas is judged to be excessive, the powder is discharged into the purification chamber of the first reactor, and an inert carrier gas is filled into the purification chamber of the first reactor until the exhaust gas discharged from the purification chamber of the first reactor does not contain the first reaction gas and by-products; S4. The powder in the clean room of the first reactor is transported to the reaction chamber of the second reactor by an inert carrier gas, and the inert carrier gas is continuously introduced into the reaction chamber of the second reactor to heat the fluidized powder so that the powder temperature is maintained within a preset temperature value; S5. Pulsing a second reaction gas to the powder in the reaction chamber of the second reactor, maintaining the pressure in the reaction chamber of the second reactor within the target pressure value, and detecting the exhaust gas components discharged from the reaction chamber of the second reactor until it is determined that the second reaction gas is excessive; S6. When it is determined that the second reaction gas is excessive, the powder is discharged into the purification chamber of the second reactor, and an inert carrier gas is filled into the purification chamber of the second reactor until the exhaust gas discharged from the purification chamber of the second reactor does not contain the second reaction gas and by-products, that is, an ALD growth cycle is completed on the powder surface; S7. Repeating steps S1 to S6 in the next ALD growth cycle unit, completing multiple ALD growth cycles on the powder surface partially coated in the upstream step until the coating on the powder surface reaches the target thickness; S8. Use an inert carrier gas to transport the coated powder to a feed tank for cooling; the powder includes powder that is not coated with a coating or powder that is partially coated from an upstream step in the coating process.

7. The method for coating powder by continuous atomic layer deposition according to claim 6, characterized in that: Determine whether the first reaction gas or the second reaction gas is excessive by the following steps: Detecting the concentration C1 of the first reaction gas / the second reaction gas in the tail gas, and the concentration C2 of the by-products generated by the reaction of the first reaction gas / the second reaction gas with the powder; The first reaction gas or the second reaction gas is judged to be excessive according to whether C2 and C1 meet the judgment condition.

8. The method for coating powder by continuous atomic layer deposition according to claim 7, characterized in that: The judgment conditions for judging the excess of the first reaction gas or the second reaction gas include: C1 is not less than the first threshold, but C2 is not greater than the second threshold.

9. A device for continuous atomic layer deposition of coated powders, characterized in that: Comprising the reactor according to any one of claims 1 to 4, each four of the reactors constitute an ALD growth cycle unit, the outlet of the material delivery pipe of the first reactor among the first to fourth reactors is connected to the inlet of the material delivery pipe of the next reactor, the reaction gas common inlet pipe of the first reactor is supplied by a first reaction gas source, the reaction gas common inlet pipes of the second and fourth reactors are supplied by a second reaction gas source, the reaction gas common inlet pipe of the third reactor is supplied by a third reaction gas source, and the inert carrier gas common inlet pipes are all supplied by an inert carrier gas source; Multiple ALD growth cycle units are connected in series in sequence, the inlet of the feed inlet pipe of the first reactor of the first ALD growth cycle unit is connected to the loading tank, the outlet of the feed outlet pipe of the fourth reactor of the ALD growth cycle unit starting from the first ALD growth cycle unit is connected to the inlet of the feed inlet pipe of the first reactor of the next ALD growth cycle unit, and the outlet of the feed outlet pipe of the fourth reactor of the last ALD growth cycle unit is connected to the unloading tank.

10. A method for coating powder by continuous atomic layer deposition, characterized in that: The apparatus for continuous atomic layer deposition coating powder as claimed in claim 9 comprises the following steps: F1. Using an inert carrier gas to transport the uncoated powder to the reaction chamber of the first reactor of the ALD growth cycle unit, the inert carrier gas is continuously introduced into the reaction chamber of the first reactor to heat the fluidized powder so that the powder temperature is maintained within a preset temperature value; F2. Pulsing a first reaction gas to the powder in the reaction chamber of the first reactor, maintaining the pressure of the reaction chamber of the first reactor within the target pressure value, and detecting the exhaust gas components discharged from the reaction chamber of the first reactor until it is determined that the first reaction gas is excessive; F3. When the first reaction gas is judged to be excessive, the powder is discharged into the purification chamber of the first reactor, and an inert carrier gas is filled into the purification chamber of the first reactor until the exhaust gas discharged from the purification chamber of the first reactor does not contain the first reaction gas and by-products; F4. The powder in the clean room of the first reactor is transported to the reaction chamber of the second reactor by an inert carrier gas, and the inert carrier gas is continuously introduced into the reaction chamber of the second reactor to heat the fluidized powder so that the powder temperature is maintained within a preset temperature value; F5. Pulsing a second reaction gas to the powder in the reaction chamber of the second reactor, maintaining the pressure of the reaction chamber of the second reactor within the target pressure value, and detecting the exhaust gas components discharged from the reaction chamber of the second reactor until it is determined that the second reaction gas is excessive; F6. When it is determined that the second reaction gas is excessive, the powder is discharged into the purification chamber of the second reactor, and an inert carrier gas is filled into the purification chamber of the second reactor until the exhaust gas discharged from the purification chamber of the second reactor does not contain the second reaction gas and by-products; F7. The powder in the clean room of the second reactor is transported to the reaction chamber of the third reactor by using an inert carrier gas, and the inert carrier gas is continuously introduced into the reaction chamber of the third reactor to heat the fluidized powder so that the powder temperature is maintained within a preset temperature value; F8. Pulsing a third reaction gas to the powder in the reaction chamber of the third reactor, maintaining the pressure of the reaction chamber of the third reactor within the target pressure value, and detecting the exhaust gas components discharged from the reaction chamber of the third reactor until it is determined that the third reaction gas is excessive; F9. When it is determined that the third reaction gas is excessive, the powder is discharged into the purification chamber of the third reactor, and an inert carrier gas is filled into the purification chamber of the third reactor until the exhaust gas discharged from the purification chamber of the third reactor does not contain the third reaction gas and by-products; F10. The powder in the clean room of the third reactor is transported to the reaction chamber of the fourth reactor by an inert carrier gas, and the inert carrier gas is continuously introduced into the reaction chamber of the fourth reactor to heat the fluidized powder so that the powder temperature is maintained within a preset temperature value; F11. Pulsing the second reaction gas to the powder in the reaction chamber of the fourth reactor, maintaining the pressure of the reaction chamber of the fourth reactor within the target pressure value, and detecting the exhaust gas components discharged from the reaction chamber of the fourth reactor until it is determined that the second reaction gas is excessive; F12. When it is determined that the second reaction gas is excessive, the powder is discharged into the purification chamber of the fourth reactor, and an inert carrier gas is filled into the purification chamber of the fourth reactor until the exhaust gas discharged from the purification chamber of the fourth reactor does not contain the second reaction gas and by-products, that is, an ALD growth cycle is completed on the powder surface; F13. Repeating steps F1 to F12 in the next ALD growth cycle unit, completing multiple ALD growth cycles on the powder surface partially coated in the upstream step until the coating on the powder surface reaches the target thickness; F14. Use an inert carrier gas to transport the coated powder to a discharge tank for cooling; the powder includes powder that is not coated with a coating or partially coated powder from an upstream step in the coating process.

11. The method for coating powder by continuous atomic layer deposition according to claim 10, characterized in that: The following steps are used to determine whether the first reaction gas, the second reaction gas, or the third reaction gas is excessive: Detecting the concentration C1 of the first reaction gas / the second reaction gas / the third reaction gas in the tail gas, and the concentration C2 of the by-products generated by the reaction of the first reaction gas / the second reaction gas / the third reaction gas with the powder; The excess of the first reaction gas, the second reaction gas or the third reaction gas is determined according to whether C2 and C1 meet the discrimination condition.

12. The method for coating powder by continuous atomic layer deposition according to claim 11, characterized in that: The judgment conditions for judging the excess of the first reaction gas, the second reaction gas or the third reaction gas include: C1 is not less than the first threshold, but C2 is not greater than the second threshold.

Citation Information

Cited By

  • Positive electrode material and preparation method and application thereof

    CN120511293A

  • A cathode material, its preparation method and application

    CN120511293B