A polypropylene composite material for 5G antenna cover and preparation method thereof
By using nanosilicon dioxide/polymer hybrid microspheres in polypropylene composites, the problems of excessive dielectric constant and density, insufficient flame retardant and weathering performance in 5G antenna covers are solved, and low The polypropylene composite material with density, low dielectric constant and excellent flame retardant and weathering properties avoids the precipitation of flame retardants and ultraviolet stabilizers.
Patent Information
- Application Number
- CN202410402615.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-04-03
AI Technical Summary
Existing polypropylene composites have problems such as excessive dielectric constant and density, insufficient flame retardant and weather resistance in 5G antenna cover applications, and the compatibility problems of flame retardant and UV stabilizer lead to precipitation during long-term use. Impacts the stability of the material.
Nanosilia modified nanosilia/polymer hybrid microspheres were prepared by pickering emulsion method, and mixed with polypropylene, and then molded by injection molding to form low density and low The polypropylene composite material with dielectric constant uses copolymers and flame retardants in microspheres to improve the flame retardant and weather resistance of the material.
The low density, low dielectric constant and excellent flame retardant and weather resistance of the polypropylene composite material for 5G radomes are realized, and the precipitation of flame retardant and ultraviolet stabilizers is avoided, and the lightweight and high performance requirements of the material are met.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer materials and relates to a polypropylene composite material, and in particular to a polypropylene composite material for a 5G antenna cover and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is a non-polar polymer with a very low dielectric constant and dielectric loss. Its dielectric properties remain stable under changes in temperature and frequency, which can ensure that the base station antenna cover has good wave transmittance and is very suitable for manufacturing base station antenna covers.
[0003] The strength of polypropylene material itself is insufficient. The use of glass fiber reinforced polypropylene can improve the mechanical properties of the material and meet the mechanical property requirements of the antenna cover material. However, the addition of glass fiber will increase the dielectric constant and density of the material, which cannot meet the requirements of the base station antenna cover for low dielectric and lightweight development. In addition, the antenna cover also has certain requirements for the weather resistance and flame retardancy of the material. Although the flame retardancy and weather resistance of polypropylene materials can be improved by adding flame retardants and UV stabilizers, flame retardants and UV stabilizers will inevitably precipitate a little during long-term use due to compatibility issues. The above problems restrict the widespread application of polypropylene composite materials in antenna cover materials. Summary of the invention
[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a polypropylene composite material for a 5G antenna cover and a preparation method thereof. The polypropylene composite material provided by the present invention can be used to produce components such as 5G base station antenna covers and vehicle-mounted millimeter-wave radar covers. The product is lightweight and has a low dielectric constant and dielectric loss as well as excellent flame retardancy and weather resistance.
[0005] The present invention is achieved through the following technical solutions:
[0006] A polypropylene composite material for a 5G antenna cover comprises the following components in parts by weight: 40-50 parts of polypropylene, 3-5 parts of maleic anhydride grafted polypropylene, 25-35 parts of glass fiber, 10-20 parts of nano-silica / polymer hybrid microspheres, 5-10 parts of a toughening agent, 0.1-0.5 parts of a PTFE anti-dripping agent, 0.1-1 parts of an antioxidant, and 0.1-0.5 parts of a lubricant.
[0007] Furthermore, the polypropylene is copolymerized polypropylene, and the melt flow rate at 230° C. and 2.16 kg is 0.35-5 g / 10 min.
[0008] Furthermore, the glass fibers are chopped glass fibers.
[0009] Furthermore, the nano-silica / polymer hybrid microspheres are prepared by the following steps:
[0010] S1: Disperse 3-5 parts of aminosilane-modified nano-silica in 100 parts of water and stir evenly to obtain aqueous solution A;
[0011] S2: 30-40 parts of acrylate monomers, 40-50 parts of acrylonitrile monomers, 20-30 parts of double-bond functionalized cyclotriphosphazene derivatives, 1-3 parts of 4, 4'-di(methacrylate)-2, 2'-dihydroxybenzophenone, 1-2 parts of benzoyl peroxide and 20-30 parts of foaming agent are mixed and stirred to obtain an oil phase solution B;
[0012] S3: mixing the aqueous solution A and the oily solution B in a weight ratio of 7:3, and then beating at a high speed of 10000-12000 r / min for 5-10 min to obtain an O / W type pickering emulsion C;
[0013] S4: Deoxygenate the emulsion C by passing nitrogen, react at 60-80°C for 10-20h, and then obtain nano-silica / polymer hybrid microspheres by centrifugation, washing and drying.
[0014] Furthermore, the aminosilane-modified nano-silica is KH550-modified nano-silica with a particle size of 20 to 50 nm;
[0015] And / or, the acrylic acid ester monomer is at least one of methyl methacrylate and butyl methacrylate;
[0016] And / or, the acrylonitrile monomer is at least one of acrylonitrile and methacrylonitrile;
[0017] And / or, the foaming agent is at least one of isooctane and isoheptane.
[0018] Furthermore, the double bond functionalized cyclotriphosphazene derivative is prepared by the following steps:
[0019] 1-2 parts of phosphorus trichloride and 1-2 parts of triethanolamine are dissolved in acetone, and 4-10 parts of an acetone solution of a substitution reagent are slowly added thereto at 50°C. After the addition is completed, the temperature is raised to reflux for reaction for 8-12 hours, and then the solution is filtered and distilled to remove the solvent, and then washed with n-heptane, filtered and dried to obtain a double-bond functionalized cyclotriphosphazene derivative.
[0020] Furthermore, the substitution reagent is at least one of 2-aminoethyl methacrylate hydrochloride, 2-methylallylamine and 3-butenylamine hydrochloride.
[0021] Further, the 4,4'-di(methacrylate)-2,2'-dihydroxybenzophenone is prepared by the following steps:
[0022] Dissolve 4-5 parts of methacryloyl chloride and 5 parts of 2,2',4,4'-tetrahydroxybenzophenone in anhydrous pyridine, react at 50-60°C for 2-4 hours, pour the reaction solution into methanol for precipitation, filter and dry to obtain a solid powder, which is 4, 4'-di(methacrylate)-2, 2'-dihydroxybenzophenone.
[0023] Furthermore, the toughening agent is POE;
[0024] And / or, the antioxidant is a composite antioxidant formed by mixing antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1;
[0025] And / or, the lubricant is at least one of oxidized polyethylene wax and vinyl bisstearamide.
[0026] A further improvement of the present invention is:
[0027] A method for preparing a polypropylene composite material for a 5G antenna cover comprises the following steps:
[0028] S1: Weigh each component according to weight, mix the polypropylene resin, toughening agent, PTFE anti-drip agent, antioxidant and lubricant evenly, and add them to the main feed port of the twin-screw extruder; add the glass fiber to the side feed port of the twin-screw extruder, and obtain mixed particles through melting, extrusion and granulation.
[0029] S2: After the mixed particles obtained in step S1 and 15# industrial white oil are stirred and evenly mixed in a mass ratio of 100:1, maleic anhydride grafted polypropylene and nano-silica / polymer hybrid microspheres weighed in parts by weight are added, and after stirring evenly, a polypropylene composite material for a 5G antenna cover is obtained by injection molding.
[0030] The beneficial effects of the present invention are:
[0031] The present invention adopts aminosilane-modified nano-silica stabilized pickering emulsion method to prepare nano-silica / polymer hybrid microspheres coated with low-boiling point liquid alkane, mixes the nano-silica / polymer hybrid microspheres with polypropylene mixed particles, and then obtains polypropylene composite materials for 5G antenna covers by injection molding. When the material is heated during the injection molding process, the polymer of the microsphere shell softens, and the low-boiling point liquid alkane coated inside is vaporized, causing the microspheres to expand, thereby reducing the density and dielectric constant of the polypropylene composite material.
[0032] The microspheres are formed by copolymerization of acrylate, acrylonitrile, double-bond functionalized cyclotriphosphazene derivatives and 4, 4'-di(methacrylate)-2, 2'-dihydroxybenzophenone. 4, 4'-di(methacrylate)-2, 2'-dihydroxybenzophenone acts as both a crosslinker and a UV stabilizer in the microspheres. The two active double bonds in its molecules participate in the copolymerization reaction, so that the polymer forms a network crosslinking structure, which improves the strength of the microspheres and avoids the rupture of the spheres during foaming and expansion. At the same time, the intramolecular hydrogen bonds formed between the hydroxyl group and the ketone group on the benzene ring in the molecule form a chelate ring. After absorbing ultraviolet light energy, the molecule undergoes thermal vibration, the hydrogen bonds break, and the chelate ring opens, thus converting the energy of ultraviolet light into heat energy and releasing it. In addition, the ketone group in the molecule will be excited by the absorbed ultraviolet light energy, resulting in tautomerism and generating an enol structure, which also consumes part of the energy. On the other hand, the high content of phosphorus, nitrogen and nano-silica in cyclotriphosphazene derivatives can play a good synergistic flame retardant effect. Therefore, adding hybrid microspheres to polypropylene can also improve the weather resistance and flame retardant properties of the material. Finally, the aminosilane-modified nano-silica in the hybrid microspheres can react with maleic anhydride-grafted polypropylene to graft the microspheres onto the polypropylene molecular chain, thereby improving the compatibility of the microspheres and polypropylene and avoiding the precipitation of benzophenone ultraviolet absorbers and cyclotriphosphazene flame retardants. DETAILED DESCRIPTION
[0033] The present invention is described in detail below in conjunction with specific embodiments. Example 1
[0034] Preparation of double bond functionalized cyclotriphosphazene derivatives:
[0035] 200 g of phosphorus trichloride and 100 g of triethanolamine were dissolved in 5 L of acetone, and 400 g of 2-aminoethyl methacrylate hydrochloride in 4 L of acetone was slowly added dropwise at 50° C. After the addition was completed, the temperature was raised and refluxed for 10 h. The solution was then filtered and the solvent was removed by distillation. The solution was then washed with n-heptane, filtered, and dried to obtain a double-bond functionalized cyclotriphosphazene derivative.
[0036] Preparation of 4,4'-di(methacrylate)-2,2'-dihydroxybenzophenone:
[0037] 40 g of methacryloyl chloride and 50 g of 2, 2', 4, 4'-tetrahydroxybenzophenone were dissolved in 1000 mL of anhydrous pyridine, reacted at 60° C. for 2 h, and then the reaction solution was poured into methanol for precipitation. After filtering and drying, 4, 4'-di(methacrylate)-2, 2'-dihydroxybenzophenone was obtained.
[0038] Preparation of Nano-Silica / Polymer Hybrid Microspheres:
[0039] S1: Disperse 30g KH550 modified nano-silica in 1kg water and stir evenly to obtain aqueous solution A;
[0040] S2: 400 g of methyl methacrylate, 400 g of methacrylonitrile, 200 g of a double-bond functionalized cyclotriphosphazene derivative, 15 g of 4, 4'-di(methacrylate)-2, 2'-dihydroxybenzophenone, 10 g of benzoyl peroxide and 200 g of isoheptane were mixed and stirred to obtain an oil phase solution B;
[0041] S3: 700 g of aqueous solution A and 300 g of oil solution B were mixed, and then high-speed beating was performed at a stirring speed of 12000 r / min for 10 min to obtain an O / W type pickering emulsion C;
[0042] S4: The emulsion C is deoxygenated by nitrogen, reacted at 80°C for 10 hours, and then centrifuged, washed, and dried to obtain nano-silica / polymer hybrid microspheres.
[0043] Preparation of polypropylene composite materials for 5G radomes:
[0044] S1: 4 kg of polypropylene, 700 g of POE, 30 g of PTFE anti-drip agent, 25 g of antioxidant 1010, 25 g of antioxidant 168 and 30 g of oxidized polyethylene wax were mixed evenly, and added to the main feed port of a twin-screw extruder; 3 kg of chopped glass fibers were added to the side feed port of the twin-screw extruder, and mixed particles were obtained through melting, extrusion and granulation.
[0045] S2: After 5 kg of the mixed particles obtained in step S1 and 50 g of 15# industrial white oil are stirred and evenly mixed, 250 g of maleic anhydride grafted polypropylene and 1 kg of nano-silica / polymer hybrid microspheres are added, and after stirring evenly, a polypropylene composite material for a 5G antenna cover is obtained by injection molding. Example 2
[0046] In this embodiment, the amount of nano-silica / polymer hybrid microspheres added to the polypropylene composite material for the 5G antenna cover is 1.5 kg. Other than this, this embodiment is exactly the same as Embodiment 1 and will not be described in detail here. Example 3
[0047] In this embodiment, the amount of nano-silica / polymer hybrid microspheres added to the polypropylene composite material for the 5G antenna cover is 2 kg. Other than this, this embodiment is exactly the same as Example 1 and will not be described in detail here.
[0048] Comparative Example 1
[0049] Preparation of polypropylene composites:
[0050] S1: 4 kg of polypropylene, 700 g of POE, 30 g of PTFE anti-drip agent, 25 g of antioxidant 1010, 25 g of antioxidant 168 and 30 g of oxidized polyethylene wax were mixed evenly, and added to the main feed port of a twin-screw extruder; 3 kg of chopped glass fibers were added to the side feed port of the twin-screw extruder, and mixed particles were obtained through melting, extrusion and granulation.
[0051] S2: 5 kg of the mixed particles obtained in step S1 and 250 g of maleic anhydride grafted polypropylene are mixed and stirred uniformly, and a polypropylene composite material is obtained by injection molding.
[0052] Comparative Example 2
[0053] S1: 4 kg of polypropylene, 700 g of POE, 30 g of PTFE anti-drip agent, 25 g of antioxidant 1010, 25 g of antioxidant 168 and 30 g of oxidized polyethylene wax were mixed evenly, and added to the main feed port of a twin-screw extruder; 3 kg of chopped glass fibers were added to the side feed port of the twin-screw extruder, and mixed particles were obtained through melting, extrusion and granulation.
[0054] S2: After 5 kg of the mixed particles obtained in step S1 and 50 g of 15# industrial white oil are stirred and mixed evenly, 250 g of maleic anhydride grafted polypropylene and 2 kg of expandable microspheres (brand DU260, purchased from Kuaisui Technology Co., Ltd.) are added, stirred evenly, and then injection molded to obtain a polypropylene composite material.
[0055] The relevant performance test results of the above-mentioned embodiments and comparative examples are shown in Table 1, wherein the density test standard is ISO1183-1; the tensile performance test standard is ISO527-2, the sample size is 115mm×10mm×4mm, and the tensile speed is 50mm / min; the bending performance test standard is ISO178, the sample size is 80mm×10mm×4mm, and the bending speed is 2mm / min; the Izod notched impact strength test standard is ISO180, and the sample size is 80mm×10mm×4mm (notch retention width is 8mm); the dielectric performance test standard is ISO:IEC61189, and the test frequency is 2.5GHz; the flame retardant grade test standard is UL94; and the weather resistance test standard is ISO4582.
[0056] Table 1 Performance test data of embodiments and comparative examples
[0057] Test items Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 <![CDATA[Density (g / cm 3 ).]]> 1.17 1.12 1.08 1.23 1.06 Tensile strength (MPa) 64 60 58 70 55 Bending strength (MPa) 82 80 77 85 70 Flexural modulus (MPa) 4086 4105 4112 4000 4098 <![CDATA[Impact strength (KJ / m 2 )]]> 37 39 38 35 37 Dielectric constant (2.5GHz) 2.51 2.39 2.17 2.72 2.21 Dielectric loss (2.5GHz) 0.0032 0.0028 0.0027 0.0035 0.0028 Flame retardant grade (1.5mm) V1 V0 V0 HB HB Color difference (ΔE) 3.2 2.5 2.1 10.7 10.4
[0058] The difference between Comparative Example 1 and Examples 1 to 3 is that nano-silica / polymer hybrid microspheres are not added in the comparative example, while microspheres are added in Examples 1 to 3, and the amount of microspheres added is gradually increased. As shown in Table 1, the polypropylene composite material for 5G antenna cover prepared by the method of the present invention has low density, low dielectric constant and low dielectric loss, as well as excellent flame retardant and weather resistance. Compared with the material without adding nano-silica / polymer hybrid microspheres, the composite material with added microspheres has slightly reduced tensile strength and bending strength, but the density, dielectric constant, dielectric loss, flame retardant and weather resistance are significantly improved, meeting the performance requirements of the 5G antenna cover for the material. Within the range set by the present invention, the microspheres have a good foaming effect and excellent comprehensive material performance. As the amount of microspheres added gradually increases, the foaming rate of the material gradually increases, and the content of flame retardants and ultraviolet light stabilizers also gradually increases, so the density, dielectric constant and dielectric loss of the polypropylene composite material gradually decrease, and the flame retardant grade and weather resistance gradually increase. When the amount of microspheres added exceeds the range set by the present invention, if the amount added is too high, the foaming ratio of the polypropylene composite material is too large, and the microspheres are easily squeezed and broken after foaming, which destroys the continuous phase structure of the polypropylene, resulting in a significant decrease in the mechanical properties of the polypropylene composite material and a slight increase in the dielectric constant; if the amount added is too low, the foaming degree of the polypropylene composite material is low, and the content of the flame retardant and the ultraviolet light stabilizer is also low, and the dielectric, flame retardant and weather resistance of the material are not significantly improved.
[0059] The microspheres added in Comparative Example 2 are purchased expandable microspheres. Compared with Example 3, the flame retardant grade is lower, the weather resistance is also poor, and the color difference increases by 395.2%.
[0060] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A polypropylene composite material for a 5G antenna cover, characterized in that: The invention comprises the following components in parts by weight: 40-50 parts of polypropylene, 3-5 parts of maleic anhydride grafted polypropylene, 25-35 parts of glass fiber, 10-20 parts of nano-silica / polymer hybrid microspheres, 5-10 parts of toughening agent, 0.1-0.5 parts of PTFE anti-dripping agent, 0.1-1 parts of antioxidant and 0.1-0.5 parts of lubricant; The nano-silicon dioxide / polymer hybrid microspheres are prepared by the following steps: S1: Disperse 3-5 parts of aminosilane-modified nano-silica in 100 parts of water and stir evenly to obtain aqueous solution A; S2: 30-40 parts of acrylate monomers, 40-50 parts of acrylonitrile monomers, 20-30 parts of double-bond functionalized cyclotriphosphazene derivatives, 1-3 parts of 4, 4'-di(methacrylate)-2, 2'-dihydroxybenzophenone, 1-2 parts of benzoyl peroxide and 20-30 parts of foaming agent are mixed and stirred to obtain an oil phase solution B; S3: mixing the aqueous solution A and the oily solution B in a weight ratio of 7:3, and then beating at a high speed of 10000-12000 r / min for 5-10 min to obtain an O / W type pickering emulsion C; S4: Deoxygenate the emulsion C by nitrogen, react at 60-80°C for 10-20h, and then centrifuge, wash, and dry to obtain nano-silica / polymer hybrid microspheres; The double bond functionalized cyclotriphosphazene derivative is prepared by the following steps: 1-2 parts of phosphorus trichloride and 1-2 parts of triethanolamine are dissolved in acetone, and an acetone solution containing 4-10 parts of a substitution reagent is slowly added dropwise at 50°C. After the addition is completed, the temperature is raised and refluxed for reaction for 8-12 hours. The solution is then filtered and distilled to remove the solvent, and then washed with n-heptane, filtered and dried to obtain a double-bond functionalized cyclotriphosphazene derivative; the substitution reagent is at least one of 2-aminoethyl methacrylate hydrochloride, 2-methylallylamine and 3-butenylamine hydrochloride; The 4,4'-di(methacrylate)-2,2'-dihydroxybenzophenone is prepared by the following steps: Dissolve 4-5 parts of methacryloyl chloride and 5 parts of 2, 2', 4, 4'-tetrahydroxybenzophenone in anhydrous pyridine, react at 50-60°C for 2-4 hours, pour the reaction solution into methanol for precipitation, filter and dry to obtain a solid powder, which is 4, 4'-di(methacrylate)-2, 2'-dihydroxybenzophenone.
2. The polypropylene composite material for 5G antenna cover according to claim 1, characterized in that: The polypropylene is copolymer polypropylene, and the melt flow rate at 230° C. and 2.16 kg is 0.35-5 g / 10 min.
3. The polypropylene composite material for 5G antenna cover according to claim 1, characterized in that: The glass fibers are chopped glass fibers.
4. The polypropylene composite material for 5G antenna cover according to claim 1, characterized in that: The aminosilane-modified nano-silica is KH550-modified nano-silica with a particle size of 20-50 nm; And / or, the acrylic acid ester monomer is at least one of methyl methacrylate and butyl methacrylate; And / or, the acrylonitrile monomer is at least one of acrylonitrile and methacrylonitrile; And / or, the foaming agent is at least one of isooctane and isoheptane.
5. The polypropylene composite material for 5G antenna cover according to claim 1, characterized in that: The toughening agent is POE; And / or, the antioxidant is a composite antioxidant formed by mixing antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1; And / or, the lubricant is at least one of oxidized polyethylene wax and vinyl bisstearamide.
6. The method for preparing a polypropylene composite material for a 5G antenna cover according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: Weigh each component according to weight, mix the polypropylene resin, toughening agent, PTFE anti-drip agent, antioxidant and lubricant evenly, and add the mixture to the main feed port of the twin-screw extruder; add the glass fiber to the side feed port of the twin-screw extruder, and obtain mixed particles through melting, extrusion and granulation; S2: After the mixed particles obtained in step S1 and 15# industrial white oil are stirred and evenly mixed in a mass ratio of 100:1, maleic anhydride grafted polypropylene and nano-silica / polymer hybrid microspheres weighed in parts by weight are added, and after stirring evenly, a polypropylene composite material for a 5G antenna cover is obtained by injection molding.
Citation Information
Patent Citations
Production method for water-based organic polyphosphazene resin and heat reflection, high temperature resistant and antiflaming water-based paint
CN103772711A
Simple and efficient synthesis method of hexaanilinocyclotriphosphazene
CN104650147A
Flame-retardant heat-expanding microcapsule and preparation method thereof
CN108641033A
Long glass fiber reinforced polypropylene material as well as preparation method and application thereof
CN114437452A
Polypropylene material and preparation method thereof
CN116855012A