Energy-absorbing cement isolation pier and preparation method thereof
By designing the structure of the core layer, buffering energy-absorbing layer and flame-retardant layer in the cement isolation pier, and optimizing the raw material composition and process steps, the problem of the existing cement isolation pier being ineffective in absorbing vehicle impact energy has been solved, and high-strength, The durability, flame retardancy, pressure resistance and energy absorption effect are improved, while the production cost is reduced.
Patent Information
- Application Number
- CN202410805843.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Existing cement isolation piers have limited effect in absorbing vehicle impact energy and cannot effectively reduce collision damage to vehicles and drivers and passengers.
Design an energy-absorbing cement isolation pier, which adopts a structure of core layer, buffering energy-absorbing layer and flame-retardant layer. The core layer is a cavity structure filled with rubber particles and sand particles, the buffering energy-absorbing layer is made of polymer foam, and the flame-retardant layer is made of polyethylene. Urea coating optimizes the internal microstructure through a specific ratio of raw material composition and process steps to improve strength and durability.
It achieves the excellent strength, durability and good flame-retardant, pressure-resistant and energy-absorbing effects of the isolation pier, while reducing production costs and is suitable for large-scale production.
Smart Images

Figure CN118375091B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to an energy-absorbing cement isolation pier and a preparation method thereof. Background Art
[0002] Cement isolation piers are a type of cement component used to separate traffic flows traveling in opposite or same directions, and have the function of prohibiting vehicles from turning left and pedestrians from crossing the road at will. They are mainly used in underground shelters in coal mines and at the bends of tunnels where vehicles are easily hit. They can protect vehicles in the mine, people in the vehicles, mining machinery and tunnel walls.
[0003] Patent CN104975576A discloses a cement anti-collision isolation pier, which mainly relies on the anti-collision layer wrapped in the outer layer of concrete to provide protection. Although this isolation pier can protect vehicles or pedestrians from being scratched or injured by the sharp isolation pier when they hit the isolation pier, this type of isolation pier cannot effectively absorb the energy of vehicle collision, thereby reducing the damage caused by the collision to the vehicle and the driver and passengers, and play a role in protecting the vehicle and the passengers.
[0004] Patent CN111646739B discloses a lightweight isolation pier material, which is prepared from the following raw materials: cement, clay, coarse sand, biochar, asbestos, chitosan, ABS, EVA, polypropylene, epoxy resin, and polyvinyl chloride; the preparation steps are as follows: (1) ABS, EVA, polypropylene, epoxy resin, and polyvinyl chloride are mixed and stirred to obtain a mixture A; (2) cement, clay, coarse sand, asbestos, biochar, chitosan swelling solution, and an appropriate amount of water are mixed to obtain a mixture B; (3) an alloy skeleton that has been prepared is placed in a mold according to the required specifications of the isolation pier, and mixture B is poured in to fill it, and after natural drying, it is demolded and cured to obtain a base tire embryo; (4) a shell made of mixture A is coated on the periphery of the base tire embryo; (5) a fluorescent pattern is painted on the side of the shell, and the isolation pier material is obtained after drying. However, the isolation pier prepared by this method has limited effect in absorbing vehicle impact energy. Summary of the invention
[0005] In view of the deficiencies in the prior art, an object of the present invention is to provide an energy-absorbing cement isolation pier and a preparation method thereof, wherein the isolation pier has excellent strength and durability and good flame retardancy, compressive energy absorption effects, while having low cost.
[0006] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided an energy-absorbing cement isolation pier, which comprises a core layer, a buffer energy-absorbing layer and a flame-retardant layer from the inside to the outside; the core layer is a hollow structure, and the cavity of the hollow structure is filled with rubber particles and first sand particles; wherein the raw material composition of the core layer comprises water, fly ash, cement, second sand particles, polymer emulsion, polypropylene fiber and water-retaining agent, and the mass ratio of water, cement and second sand particles is 0.5:0.7-0.8:1.
[0007] In the present invention, the mass ratio of the rubber particles to the first sand particles is 1:1-3.
[0008] In the present invention, the average particle size of the rubber particles is 0.6-2.5 mm, and the average particle size of the first sand particles is 1-4.5 mm.
[0009] In the present invention, the average particle size of the second sand particles is 0.5-1 mm.
[0010] In the present invention, in the core layer, the added amount of fly ash is 25-35wt%, the added amount of polymer emulsion is 2.5-4wt%, the added amount of polypropylene fiber is 0.2-0.6wt%, and the added amount of water retaining agent is 2-3wt%.
[0011] In the present invention, the polymer emulsion is a mixture of vinyl acetate-ethylene copolymer emulsion and polyacrylate emulsion in a mass ratio of 1-1.5:1.
[0012] In the present invention, the length of the polypropylene fiber is 15-20 mm, and the fiber diameter is 100-120 μm.
[0013] In the present invention, the buffer energy absorbing layer is polymer foam.
[0014] In the present invention, the flame retardant layer is a polyurea coating.
[0015] According to another aspect of the present invention, there is also provided a method for preparing the energy absorbing cement isolation pier as described above, comprising the following steps:
[0016] (1) Mix water, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent evenly, add them into a mold, and demould after leaving them for a certain period of time to form a core layer with a cavity structure;
[0017] (2) mixing the rubber particles and the first sand particles evenly, filling the mixture into the cavity of the cavity structure, and coating the outer surface of the core layer with a buffer and energy absorption layer;
[0018] (3) A flame retardant layer is sprayed on the outer surface of the buffer energy absorption layer to obtain an energy absorbing cement isolation pier.
[0019] The invention provides an energy-absorbing cement isolation pier, which comprises a core layer, a buffer energy-absorbing layer and a flame-retardant layer in sequence from the inside to the outside; the core layer is a cavity structure, and the cavity of the cavity structure is filled with rubber particles and first sand particles.
[0020] In the present invention, the raw material composition of the core layer includes water, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent, and the mass ratio of water, cement and second sand is 0.5:0.7-0.8:1. It can be understood that the mass ratio can be any specific value of 0.5:0.7:1, 0.5:0.71:1, 0.5:0.72:1, 0.5:0.73:1, 0.5:0.74:1, 0.5:0.75:1, 0.5:0.76:1, 0.5:0.77:1, 0.5:0.78:1, 0.5:0.79:1, 0.5:0.8:1 or any value within the range of 0.5:0.7-0.8:1. Preferably, the thickness of the core layer is 35-50 mm.
[0021] In the present invention, in the core layer, the amount of fly ash added is 25-35wt%. It can be understood that the amount can be any specific value of 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt% or any value within the range of 25-35wt%. The inventors found that controlling the amount of fly ash added within the range can ensure that the core layer has suitable crack resistance and durability. The initial fly ash can be filled in the gaps of the cement paste, thereby improving the density of the cement paste, increasing the resistance to crack propagation, and improving the crack resistance of the core layer; in addition, since fly ash is reactive, the activity becomes increasingly obvious over time, thereby improving the mechanical properties and durability of the core layer.
[0022] In the present invention, in the core layer, the amount of the polymer emulsion added is 2.5-4wt%. It is understood that the amount can be any specific value of 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt%, 3wt%, 3.1wt%, 3.2wt%, 3.3wt%, 3.4wt%, 3.5wt%, 3.6wt%, 3.7wt%, 3.8wt%, 3.9wt%, 4wt%, or any value within the range of 2.5-4wt%. In the present invention, the polymer emulsion is a mixture of vinyl acetate-ethylene copolymer emulsion and polyacrylate emulsion in a mass ratio of 1-1.5:1. It is understood that the mass ratio can be any specific value of 1:1, 1.1:1, 1.2:1, 1.4:1, 1.5:1, or any value within the range of 1-1.5:1. In the present invention, the solid content of the vinyl acetate-ethylene copolymer emulsion is 50-55%. In the present invention, the solid content of the polyacrylate emulsion is 35-40%. To the surprise of the inventors of the present invention, a specific ratio of vinyl acetate-ethylene copolymer emulsion and polyacrylate emulsion can synergistically improve the compressive strength and bonding strength of the core layer, because the blending of vinyl acetate-ethylene copolymer emulsion and polyacrylate emulsion in a suitable ratio can optimize the pore structure of the cement paste and effectively improve the mechanical properties of the core layer.
[0023] In the present invention, in the core layer, the amount of the polypropylene fiber added is 0.2-0.6wt%, and it is understood that the amount can be any specific value of 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt% or any value within the range of 0.2-0.6wt%. In the present invention, the length of the polypropylene fiber is 15-20mm, and it is understood that the length can be any specific value of 15mm, 16mm, 17mm, 18mm, 19mm, 20mm or any value within the range of 15-20mm; the fiber diameter is 100-120μm, and it is understood that the diameter can be any specific value of 100μm, 105μm, 110μm, 115μm, 120μm or any value within the range of 100-120μm. The inventors have found that adding polypropylene fibers of the content and size described above to the core layer composition can improve the strength of the core layer, especially the strength after long-term use, because the fibers can better play the role of transferring loads, thereby improving the mechanical properties of the core layer. If the amount of fiber added is too much, it is very easy to agglomerate in the cement paste, thereby reducing the mechanical properties of the core layer. If the size of the fiber is not appropriate, the length is too long or too short, the role of the fiber in transferring loads will drop sharply.
[0024] In the present invention, in the core layer, the water retaining agent is added in an amount of 2-3wt%. It can be understood that the amount can be any specific value of 2wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt%, 3wt% or any value within the range of 2-3wt%. In the present invention, the water retaining agent is cellulose ether.
[0025] In the present invention, in the core layer, the average particle size of the second sand particles is 0.5-1 mm. It can be understood that the average particle size can be any specific value among 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm or any value within the range of 0.5-1 mm.
[0026] In the present invention, the core layer is a hollow structure, and the cavity of the hollow structure is filled with rubber particles and first sand particles. In the present invention, the mass ratio of the rubber particles to the first sand particles is 1:1-3. It can be understood that the mass ratio can be any specific value of 1:1, 1:1.5, 1:2, 1:2.5, 1:3 or any value within the range of 1:1-3. In the present invention, the rubber particles are obtained by mechanically crushing waste tires. In the present invention, the average particle size of the rubber particles is 0.6-2.5 mm. It is understood that the average particle size can be any specific value of 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm or any value within the range of 0.6-2.5 mm. In the present invention, the average particle size of the first sand particles is 1-4.5 mm, preferably 2-4 mm. By selecting a specific ratio of rubber particles and first sand particles for mixing, the energy absorption effect of the rubber particles can be maximized while ensuring appropriate mechanical strength.
[0027] In the present invention, the buffering energy absorbing layer is a polymer foam. Preferably, the polymer foam is a polystyrene foam, and the raw materials of the polystyrene foam include, by weight: 50-100 parts of polystyrene, 3-5 parts of coupling agent, 10-20 parts of foaming agent, 4-6 parts of plasticizer, and 2-4 parts of antioxidant. In the present invention, the density of the polymer foam is preferably 0.30-0.35 g / cm 3 It is understood that its density can be 0.30 g / cm 3 , 0.31g / cm 3 , 0.32g / cm 3 , 0.33g / cm3 , 0.34g / cm 3 , 0.35g / cm 3 Any specific value or 0.30-0.35g / cm 3 Any value in the range.
[0028] Preferably, the coupling agent is silane coupling agent KH550, the foaming agent is azodicarbonamide, and the antioxidant is antioxidant 1010.
[0029] In the present invention, the flame retardant layer is a polyurea coating, and the polyurea coating can be obtained by spraying a flame retardant polyurea coating on the outer surface of the buffer energy absorption layer. Preferably, the flame retardant polyurea coating comprises component A and component B, and the raw materials of component A include 40-50 parts of polyether polyol and 40-50 parts of isocyanate by weight; the raw materials of component B include 35-50 parts of amino-terminated polyether, 30-40 parts of amine chain extender, 20-30 parts of flame retardant, 0.1-0.5 parts of dispersant, and 0.5-1.0 parts of defoamer by weight; the mass ratio of component A to component B is 1:1. In the present invention, the thickness of the flame retardant layer is 0.05-0.2 mm.
[0030] Preferably, the polyether polyol is R2304 polyether polyol, and the isocyanate is toluene diisocyanate; preferably, the amino-terminated polyether is D-2000 amino-terminated polyether, the amine chain extender is diethyltoluenediamine, the flame retardant is dimethyl methyl phosphate, the dispersant is Dispers610 dispersant, and the defoamer is JX883 defoamer.
[0031] According to another aspect of the present invention, there is also provided a method for preparing the energy absorbing cement isolation pier as described above, comprising the following steps:
[0032] (1) Mix water, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent evenly, add them into a mold, and demould after leaving them for a certain period of time to form a core layer with a cavity structure;
[0033] (2) mixing the rubber particles and the first sand particles evenly, adding the mixture into the cavity of the cavity structure, and coating the outer surface of the core layer with a buffering and energy-absorbing layer;
[0034] (3) A flame retardant layer is sprayed on the outer surface of the buffer energy absorption layer to obtain an energy absorbing cement isolation pier.
[0035] In the present invention, in step (1), water, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent are mixed evenly, added to a mold, and demoulded after being placed for a certain period of time to form a core layer with a cavity structure. In the present invention, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent are first stirred evenly, and then poured into water and quickly stirred evenly. The present invention can select a suitable mold according to the actual size requirements. In the present invention, the placement time can be 24-26h. Preferably, a filling port is provided on the top of the core layer with a cavity structure, which is used to fill the rubber particles and the first sand into the cavity of the cavity structure in step (2). More preferably, the number of the filling ports is 1-5, and the diameter of the filling port is 10-20mm.
[0036] In the present invention, in step (2), the rubber particles and the first sand particles are mixed evenly, added to the cavity of the cavity structure, and the outer surface of the core layer is coated with a buffering energy absorbing layer. In the present invention, the outer surface of the core layer is coated with a buffering energy absorbing layer as follows: after the other raw materials other than the foaming agent are mixed evenly, they are kneaded at 110-120°C for 10-15 minutes; then the foaming agent is added and mixed evenly, kneaded at 95-100°C for 5-7 minutes, and then pressure-formed at a pressure of 5-7MPa, demolded after maintaining the pressure for 10-15 minutes, and the obtained polystyrene foam is coated on the outer surface of the core layer to form a buffering energy absorbing layer. In the present invention, the thickness of the buffering energy absorbing layer is 10-20mm.
[0037] In the present invention, in step (3), a flame retardant layer is sprayed on the outer surface of the buffer energy absorption layer to obtain an energy absorbing cement isolation pier. In the present invention, a conventional spray gun in the art can be used to spray the flame retardant layer, specifically: component A and component B are respectively fed into a flow pump from their respective independent feed boxes, and are respectively transported to a mixing chamber according to a pre-adjusted ratio, and after stirring in the mixing chamber, they are sprayed from a nozzle onto the outer surface of the buffer energy absorption layer, and the flame retardant layer is formed after curing at a temperature of 35-50°C. In the present invention, the spray thickness of the flame retardant layer is 0.05-0.2mm.
[0038] The dimensions of the cement isolation pier of the present invention refer to the provisions of standard GB / T18046-2008.
[0039] Compared with the prior art, the beneficial technical effects of the present invention are:
[0040] (1) The present invention designs a cement isolation pier with a special structure and further regulates the types and contents of the components in each layer, especially the types and contents of the components in the core layer, so that the components work synergistically, change the internal microstructure of the cement isolation pier, especially optimize the pore structure, significantly improve the strength and durability of the isolation pier, and make the isolation pier have good flame retardant, compressive energy absorption and other effects.
[0041] (2) The preparation method of the cement isolation pier described in the present invention is simple, the product performance is stable, and it is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a structural schematic diagram of the cement isolation pier described in the present invention.
[0043] Among them, 1 is the cavity, 2 is the core layer, 3 is the buffer energy absorption layer, and 4 is the flame retardant layer. DETAILED DESCRIPTION
[0044] The present invention will be described in detail below by way of examples. It should be understood that the following examples are only used to further explain and illustrate the content of the present invention by way of example, and are not intended to limit the present invention. Among them, Example 1 is the best embodiment.
[0045] The raw materials used in the examples and comparative examples of the present invention are all commercially available, and their specific information is as follows:
[0046] The first sand particle: river sand, with an average particle size of 1-4.5 mm; the second sand particle: river sand, with an average particle size of 0.5-1 mm, purchased from Shanghai Dacheng Building Materials Co., Ltd.; fly ash: purchased from Shandong Shunke Building Materials Technology Co., Ltd.; cement: ordinary Portland cement, purchased from Shandong Huayin Special Cement Co., Ltd.; vinyl acetate-ethylene copolymer emulsion: solid content 55%, purchased from China Petrochemical Group Chongqing Chuanwei Chemical Co., Ltd.; polyacrylate emulsion: solid content 40%, purchased from Jinan Huijinchuan Chemical Co., Ltd.; polypropylene fiber: length 15-20 mm, diameter 100-120 μm , purchased from Changzhou Tianyi Engineering Fiber Co., Ltd.; cellulose ether: purchased from Hebei Huayi Cellulose Co., Ltd.; antioxidant 1010, azodicarbonamide, silane coupling agent KH550, diethyltoluenediamine, dimethyl methyl phosphate: purchased from Aladdin Reagent Co., Ltd.; Dispers610 dispersant: purchased from Evonik; isocyanate R2304 polyether polyol, toluene diisocyanate: purchased from Wanhua Chemical Group Co., Ltd.; D-2000 amino-terminated polyether: purchased from HUNTSMAN, USA; JX883 defoaming agent: purchased from Jiangmen Daguangming Agrochemical Xinhui Co., Ltd.
[0047] Example 1
[0048] As attached Figure 1As shown, the energy-absorbing cement isolation pier in this embodiment includes a core layer 2, a buffer energy-absorbing layer 3 and a flame-retardant layer 4 from the inside to the outside; the core layer 2 is a cavity structure, and the cavity 1 of the cavity structure is filled with rubber particles and first sand particles in a mass ratio of 1:3; the raw material composition of the core layer 2 includes 14.8wt% water, 25wt% fly ash, 23.6wt% cement, 29.6wt% second sand particles, 4wt% polymer emulsion, 0.6wt% polypropylene fiber and 2.4wt% water-retaining agent cellulose ether; wherein the polymer emulsion is a mixture of vinyl acetate-ethylene copolymer emulsion and polyacrylate emulsion in a mass ratio of 1:1; the rubber particles are obtained by mechanical crushing of waste tires, and the average particle size is 0.6-2.5mm. The thickness of the core layer 2 is 40mm.
[0049] The buffer energy absorption layer is a polystyrene foam with a thickness of 20 mm and a density of 0.30 g / cm 3 The raw materials of the polystyrene foam include, by weight: 50 parts of polystyrene, 3 parts of silane coupling agent KH550, 10 parts of foaming agent azodicarbonamide, 4 parts of epoxy soybean oil, and 2 parts of antioxidant 1010.
[0050] The flame retardant layer 4 is a polyurea coating with a thickness of 0.2 mm. The flame retardant polyurea coating includes component A and component B in a mass ratio of 1:1. Component A includes, by weight: 40 parts of R2304 polyether polyol and 40 parts of toluene diisocyanate; component B includes, by weight: 35 parts of D-2000 amino-terminated polyether, 30 parts of diethyltoluenediamine, 30 parts of dimethyl methyl phosphate flame retardant, 0.1 parts of Dispers610 dispersant, and 0.5 parts of JX883 defoamer.
[0051] The method for preparing the energy-absorbing cement isolation pier described in this embodiment comprises the following steps:
[0052] (1) First, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent are mixed evenly, then poured into water and quickly mixed evenly, added into a mold, left for 24 hours and then demolded to form a core layer 2 with a cavity structure;
[0053] (2) The rubber particles and the first sand particles are mixed evenly, and added into the cavity 1 of the cavity structure. After the other raw materials except the foaming agent azodicarbonamide are mixed evenly, kneading is performed at 110° C. for 15 minutes; then the foaming agent azodicarbonamide is added and mixed evenly, kneading is performed at 95° C. for 7 minutes, and then pressure molding is performed at a pressure of 7 MPa. After maintaining the pressure for 10 minutes, demolding is performed, and the obtained polystyrene foam is coated on the outer surface of the core layer 2 to form a buffer energy absorption layer;
[0054] (3) The component A and the component B are respectively fed into flow pumps from their respective independent feed boxes, and are transported to a mixing chamber according to a pre-adjusted ratio. After being stirred in the mixing chamber, they are sprayed from a nozzle onto the outer surface of the buffer energy absorbing layer, and are cured at a temperature of 35° C. to form a flame retardant layer 4.
[0055] Example 2
[0056] As attached Figure 1 As shown, the energy-absorbing cement isolation pier in this embodiment includes a core layer 2, a buffer energy-absorbing layer 3 and a flame-retardant layer 4 from the inside to the outside; the core layer 2 is a cavity structure, and the cavity 1 of the cavity structure is filled with rubber particles and first sand particles in a mass ratio of 1:1; the raw material composition of the core layer 2 includes 13.5wt% water, 35wt% fly ash, 18.8wt% cement, 27wt% second sand particles, 2.5wt% polymer emulsion, 0.2wt% polypropylene fiber and 3wt% water-retaining agent cellulose ether; wherein the polymer emulsion is a mixture of vinyl acetate-ethylene copolymer emulsion and polyacrylate emulsion in a mass ratio of 1.5:1; the rubber particles are obtained by mechanical crushing of waste tires, and the average particle size is 0.6-2.5mm. The thickness of the core layer 2 is 35mm.
[0057] The buffer energy absorbing layer 3 is a polystyrene foam with a thickness of 10 mm and a density of 0.35 g / cm 3 The raw materials of the polystyrene foam include, by weight: 50 parts of polystyrene, 3 parts of silane coupling agent KH550, 10 parts of foaming agent azodicarbonamide, 4 parts of epoxy soybean oil, and 2 parts of antioxidant 1010.
[0058] The flame retardant layer 4 is a 0.2 mm polyurea coating, and the flame retardant polyurea coating includes component A and component B in a mass ratio of 1:1. Component A includes, by weight: 40 parts of R2304 polyether polyol and 40 parts of toluene diisocyanate; component B includes, by weight: 35 parts of D-2000 amino-terminated polyether, 30 parts of diethyltoluenediamine, 20 parts of dimethyl methyl phosphate flame retardant, 0.1 parts of Dispers610 dispersant, and 0.5 parts of JX883 defoamer.
[0059] The method for preparing the energy-absorbing cement isolation pier described in this embodiment comprises the following steps:
[0060] (1) First, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent are mixed evenly, then poured into water and quickly mixed evenly, added into a mold, left for 36 hours and then demolded to form a core layer 2 with a cavity structure;
[0061] (2) The rubber particles and the first sand particles are mixed evenly, and added into the cavity 1 of the cavity structure. After the other raw materials except the foaming agent azodicarbonamide are mixed evenly, kneading is performed at 110° C. for 15 minutes; then the foaming agent azodicarbonamide is added and mixed evenly, kneading is performed at 95° C. for 7 minutes, and then pressure molding is performed at a pressure of 7 MPa. After maintaining the pressure for 10 minutes, demolding is performed, and the obtained polystyrene foam is coated on the outer surface of the core layer 2 to form a buffer energy absorption layer 3;
[0062] (3) The component A and the component B are respectively fed into flow pumps from their respective independent feed boxes, and are transported to a mixing chamber according to a pre-adjusted ratio. After being stirred in the mixing chamber, they are sprayed from a nozzle onto the outer surface of the buffer energy absorbing layer 3, and are cured at a temperature of 50°C to form a flame retardant layer 4.
[0063] Example 3
[0064] As attached Figure 1 As shown, the energy-absorbing cement isolation pier in this embodiment includes a core layer 2, a buffer energy-absorbing layer 3 and a flame-retardant layer 4 from the inside to the outside; the core layer 2 is a cavity structure, and the cavity 1 of the cavity structure is filled with rubber particles and first sand particles in a mass ratio of 1:2; the raw material composition of the core layer 2 includes 14wt% water, 30wt% fly ash, 22.5wt% cement, 28wt% second sand particles, 3wt% polymer emulsion, 0.5wt% polypropylene fiber and 2wt% water-retaining agent cellulose ether; wherein the polymer emulsion is a mixture of vinyl acetate-ethylene copolymer emulsion and polyacrylate emulsion in a mass ratio of 1:1; the rubber particles are obtained by mechanical crushing of waste tires, and the average particle size is 0.6-2.5mm. The thickness of the core layer 2 is 50mm.
[0065] The buffer energy absorbing layer 3 is a polystyrene foam with a thickness of 20 mm and a density of 0.32 g / cm 3 The raw materials of the polystyrene foam include, by weight: 100 parts of polystyrene, 5 parts of silane coupling agent KH550, 20 parts of azodicarbonamide, 6 parts of epoxy soybean oil, and 4 parts of antioxidant 1010.
[0066] The flame retardant layer 4 is a 0.05 mm polyurea coating, and the flame retardant polyurea coating includes component A and component B in a mass ratio of 1:1. Component A includes, by weight: 40 parts of R2304 polyether polyol and 40 parts of toluene diisocyanate; component B includes, by weight: 35 parts of D-2000 amino-terminated polyether, 30 parts of diethyltoluenediamine, 20 parts of dimethyl methyl phosphate flame retardant, 0.1 parts of Dispers610 dispersant, and 0.5 parts of JX883 defoamer.
[0067] The method for preparing the energy-absorbing cement isolation pier described in this embodiment comprises the following steps:
[0068] (1) First, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent are mixed evenly, then poured into water and quickly mixed evenly, added into a mold, left for 24 hours and then demolded to form a core layer 2 with a cavity structure;
[0069] (2) The rubber particles and the first sand particles are mixed evenly, and added into the cavity 1 of the cavity structure. After the other raw materials except the foaming agent azodicarbonamide are mixed evenly, kneading is performed at 110° C. for 15 minutes; then the foaming agent azodicarbonamide is added and mixed evenly, kneading is performed at 95° C. for 7 minutes, and then pressure molding is performed at a pressure of 7 MPa. After maintaining the pressure for 10 minutes, demolding is performed, and the obtained polystyrene foam is coated on the outer surface of the core layer 2 to form a buffer energy absorption layer 3;
[0070] (3) The component A and the component B are respectively fed into flow pumps from their respective independent feed boxes, and are transported to a mixing chamber according to a pre-adjusted ratio. After being stirred in the mixing chamber, they are sprayed from a nozzle onto the outer surface of the buffer energy absorbing layer 3, and are cured at a temperature of 40°C to form a flame retardant layer 4.
[0071] Comparative Example 1
[0072] The energy-absorbing cement isolation pier described in this comparative example is exactly the same as that in Example 1, except that the cavity 1 of the cavity structure is filled with rubber particles and first sand particles in a mass ratio of 2:1.
[0073] Comparative Example 2
[0074] The energy absorbing cement isolation pier of this comparative example is exactly the same as that of Example 1, except that all fly ash is replaced with cement of equal mass in the raw materials of the core layer 2. That is, the raw material composition of the core layer 2 includes 14.8wt% water, 48.6wt% cement, 29.6wt% second sand particles, 4wt% polymer emulsion, 0.6wt% polypropylene fiber and 2.4wt% water retaining agent cellulose ether.
[0075] Performance Test:
[0076] The energy-absorbing cement isolation piers prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to performance tests according to corresponding standard test methods. The specific test results are shown in Table 1.
[0077] Limiting oxygen index (LOI): measured by oxygen index tester (JF-3, Nanjing Analytical Instrument Company, China).
[0078] Maximum compressive strength: The maximum compressive strength is tested after 7d and 28d respectively according to standard GB / T50107-2010.
[0079] Destructive impact energy: According to CECS13-2009 "Fiber Concrete Test Method Standard", the specimens are subjected to impact tests to test the destructive impact energy.
[0080] Crack resistance: Apply lateral pressure to the material and observe whether cracks occur when the material deforms by 50% in volume.
[0081] Table 1 Performance of energy-absorbing cement isolation piers prepared in Examples 1-3 and Comparative Examples 1-2 .
[0082] From the data in Table 1, it can be seen that the energy-absorbing cement isolation piers prepared in Examples 1-3 have a high limiting oxygen index, a high maximum compressive strength, a high destructive impact energy, and no cracks are generated when the material volume deformation is 50%, indicating that the energy-absorbing cement isolation piers of the present application have good flame retardant, compressive energy absorption effects; in addition, the maximum compressive strength after 28 days is significantly improved. By comparing Example 1 with Example 1, the maximum compressive strength of the cement isolation pier in Example 1 is lower, indicating that a certain proportion of rubber particles and the first sand particles can synergistically ensure that the isolation pier has both appropriate strength and energy absorption effects. By comparing Example 2 with Example 1, the destructive impact energy of the cement isolation pier in Example 2 is lower, and cracks are generated, indicating that the addition of a certain amount of fly ash is beneficial to reducing the development and merging of microcracks, thereby improving the durability of the cement isolation pier.
[0083] In summary, the present invention designs a cement isolation pier with a special structure, and further regulates the types and contents of components in each layer. The components work synergistically to change the internal microstructure of the cement isolation pier, especially optimize the pore structure, significantly improve the strength and durability of the isolation pier, and make the isolation pier have good flame retardant, compressive energy absorption effects.
[0084] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. An energy-absorbing cement isolation pier, Features: The core layer includes a core layer, a buffering energy absorbing layer and a flame retardant layer from the inside to the outside; the core layer is a cavity structure, and the cavity of the cavity structure is filled with rubber particles and first sand particles; wherein the raw material composition of the core layer includes water, fly ash, cement, second sand particles, polymer emulsion, polypropylene fiber and water retaining agent, and the mass ratio of water, cement and second sand particles is 0.5:0.7-0.8:1; the buffering energy absorbing layer is a polymer foam, and the raw materials of the buffering energy absorbing layer include, by weight: 50-100 parts of polystyrene, 3-5 parts of coupling agent, 10-20 parts of foaming agent, 4-6 parts of plasticizer, 2 parts of antioxidant -4 parts; the mass ratio of the rubber particles to the first sand particles is 1:1-3; the average particle size of the rubber particles is 0.6-2.5mm, and the average particle size of the first sand particles is 1-4.5mm; in the core layer, the amount of fly ash added is 25-35wt%, the amount of the polymer emulsion added is 2.5-4wt%, the amount of the polypropylene fiber added is 0.2-0.6wt%, and the amount of the water retaining agent added is 2-3wt%; the polymer emulsion is a mixture of vinyl acetate-ethylene copolymer emulsion and polyacrylate emulsion in a mass ratio of 1-1.5:1; The flame retardant layer comprises component A and component B, wherein the raw materials of component A comprise, by weight, 40-50 parts of polyether polyol and 40-50 parts of isocyanate; the raw materials of component B comprise, by weight, 35-50 parts of amino-terminated polyether, 30-40 parts of amine chain extender, 20-30 parts of flame retardant, 0.1-0.5 parts of dispersant and 0.5-1.0 parts of defoamer; the mass ratio of component A to component B is 1:1; The length of the polypropylene fiber is 15-20 mm, and the fiber diameter is 100-120 μm; the average particle size of the second sand particles is 0.5-1 mm.
2. The energy-absorbing cement isolation pier according to claim 1, Features: The coupling agent is silane coupling agent KH550, and the foaming agent is azodicarbonamide.
3. The energy-absorbing cement isolation pier according to claim 1, Features: The isocyanate is toluene diisocyanate, the amine chain extender is diethyl toluene diamine, and the flame retardant is dimethyl methyl phosphate.
4. The energy-absorbing cement isolation pier according to claim 1, Features: The water retaining agent is cellulose ether.
5. A method for preparing the energy-absorbing cement isolation pier according to any one of claims 1 to 4, It is characterized in that The steps include: (1) Mix water, fly ash, cement, second sand, polymer emulsion, polypropylene fiber and water retaining agent evenly, add them into a mold, and demould after leaving them for a certain period of time to form a core layer with a cavity structure; (2) mixing the rubber particles and the first sand particles evenly, filling the mixture into the cavity of the cavity structure, and coating the outer surface of the core layer with a buffer and energy absorption layer; (3) A flame retardant layer is sprayed on the outer surface of the buffer energy absorption layer to obtain an energy absorbing cement isolation pier.