An electro-shaped memory composite material and its preparation method and application

By grafting on graphene and silver nanowires, a composite material of GP-m-AgNWs and PEEK was formed, which solved the problem of low conductivity of the composite material, achieved low driving voltage and fast shape memory effects, and satisfies high Performance and environmental protection and energy saving requirements.

CN118388923BActive Publication Date: 2024-11-26常州君华医疗科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410506357.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-11-26
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

Graphene and silver nanowires have poor interfacial compatibility with polyetherketone thermoplastic polymers in composite applications, resulting in lower-than-expected conductivity of composite materials, affecting the performance of electrochemical shape memory polymers, especially at low voltages and fast There are safety and energy consumption problems in shape memory.

Method used

Graphene and silver nanowires are grafted by using sulfhydryl-containing silane coupling agent to form GP-m-AgNWs as a composite material between conductive filler and PEEK matrix, improving interface compatibility and forming a complete conductive path, achieving low Drive voltage and fast shape memory effects.

Benefits of technology

It realizes fast shape memory reply at lower than the human body's safety voltage (30V), with a reply time of less than 60s, and a shape fixation rate and recovery rate of more than 90%, which improves the conductivity and safety of composite materials, and is in line with green energy-saving and high-efficiency materials. demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118388923B_ABST
    Figure CN118388923B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of functional polymer materials, and in particular to an electro-shaped memory composite material and a preparation method and application thereof, comprising the following materials in weight percentage: GP-m-AgNWs as a conductive filler and PEEK as a matrix; the amount of GP-m-AgNWs used is 5-30% of the weight of PEEK; the GP-m-AgNWs is obtained by grafting GP and AgNWs using a mercapto-containing silane coupling agent; the materials are uniformly mixed according to a ratio, and then melt-blended, extruded, and then molded or injection molded to obtain the electro-shaped memory composite material, the composite material has a driving voltage lower than the safety voltage of the human body and a rapid shape memory recovery effect; the composite material is used in the preparation of implantable medical device materials, including the preparation of cardiovascular and cerebrovascular stents, orthopedic implants, and dental brace materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional polymer materials, and in particular to an electro-shaped memory composite material and a preparation method and application thereof. Background Art

[0002] In the field of modern materials science and engineering, graphene (GP) and silver nanowires (AgNWs) have become hot materials for research and application due to their excellent electrical conductivity. GP, a two-dimensional material composed of a single layer of carbon atoms, is known for its excellent mechanical strength, high thermal conductivity and high electrical conductivity. AgNWs, with its extremely high electrical conductivity and good flexibility, show great application potential in microelectronics and flexible electronic devices. These two materials play a vital role in many high-end technology fields such as fuel cells, aerospace, and biomedicine.

[0003] Despite the obvious performance advantages of GP and AgNWs, they face the challenge of poor compatibility in composite applications with high-performance thermoplastic polymers such as polyetheretherketone (PEEK). As an engineering plastic, PEEK is widely used in the manufacture of high-performance composite materials due to its high temperature resistance, chemical corrosion resistance and excellent mechanical properties. However, when GP and AgNWs try to combine with PEEK, the overall conductivity of the composite material is much lower than expected due to the poor interfacial compatibility between the two, which is particularly evident in the preparation of electro-induced shape memory polymers (SMPs).

[0004] Electro-shaped memory polymers are smart materials that can change their shape under the action of voltage. When driving the shape memory effect, this type of material usually requires a lower voltage and a shorter action time to meet the social needs of safety, energy saving, high efficiency and reliability. However, due to the compatibility issues between GP and AgNWs and PEEK, the prepared composite materials often require a higher voltage and a longer time to achieve the shape memory effect, which not only increases energy consumption, but also poses a safety hazard, which runs counter to the current society's pursuit of green energy saving and efficient materials.

[0005] Therefore, in order to overcome this technical difficulty, improve the compatibility of GP and AgNWs with PEEK, and build a complete and continuous conductive path, it has become an important direction of current material science research. The success of this research and development direction will pave the way for the commercial application of electro-shaped memory polymers, promote the advancement of smart material technology, and meet the society's demand for high-performance, environmentally friendly and energy-saving materials. Summary of the invention

[0006] In order to solve the compatibility problem between conductive fillers and PEEK and construct a complete and continuous conductive path to obtain an electro-shaped memory composite material, an electro-shaped memory composite material and its preparation method and application are provided. The present invention uses GP-m-AgNWs as a conductive filler to fill the PEEK matrix, and the obtained electro-shaped memory composite material has a low driving voltage lower than the human body safety voltage, and a fast shape memory effect, with a recovery time of less than 60s, and a shape fixation rate and a recovery rate of more than 90%.

[0007] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:

[0008] The first aspect of the present invention provides an electro-shaped memory composite material, comprising the following materials in weight percentage: GP-m-AgNWs as a conductive filler and PEEK as a matrix;

[0009] The dosage of GP-m-AgNWs is 5 to 30% of the weight of PEEK;

[0010] The GP-m-AgNWs are obtained by grafting GP and AgNWs using a mercapto-containing silane coupling agent, wherein the mass ratio of AgNWs to GP is 1:1-2.

[0011] Furthermore, the graphene is a single-layer flake with a flake diameter of 5 to 10 mm; the diameter of the AgNWs is 30 nm to 40 nm and the length is 20 to 50 μm.

[0012] Furthermore, the mercapto-containing silane coupling agent is selected from one or more of mercaptopropyl trimethoxysilane, γ-mercaptopropyl triethoxysilane, mercaptopropyl methyl dimethoxysilane, 2-mercaptoethyl triethoxysilane, (mercapto) methyl siloxane-dimethyl siloxane copolymer (CAS No. 102783-03-9), and mercaptopropyl terminated polydimethylsiloxane (CAS No. 308072-58-4). When the mercapto-containing silane coupling agent is used for grafting, the mercapto group (-SH) can react with AgNWs, the sulfur atom can form a coordination with silver, and the two can chelate to form a stable complex.

[0013] Furthermore, the method for obtaining the GP-m-AgNWs is as follows: AgNWs and a mercapto-containing silane coupling agent are formed into a uniform dispersion in an organic solvent under stirring, light-proof, anhydrous conditions and a protective atmosphere, an amine catalyst is added, heated and condensed and refluxed, and then GP is added, and condensation and reflux are continued. After the reaction is completed, the material system after the reaction is filtered to obtain a solid product, which is washed with alcohol and dried to obtain GP-m-AgNWs.

[0014] Furthermore, the usage ratio of AgNWs, mercapto-containing silane coupling agent, amide organic solvent and amine catalyst is 1g:200-250g:700-800mL:1g.

[0015] Furthermore, the organic solvent is selected from one or more of DMF, DMAc, acetone, and tetrahydrofuran; the amine catalyst is dicyclohexylcarbodiimide (DCC); and the condensation reflux temperature is such that the organic solvent reaches a boiling point and generates reflux, and the reflux temperature is usually 1 to 20° C. higher than the boiling point of the solvent.

[0016] Furthermore, the condensation reflux time before adding GP is 1 to 3 hours, and the condensation reflux time after adding GP is 4 to 6 hours.

[0017] The second aspect of the present invention provides a method for preparing an electro-shaped memory composite material, comprising the following steps: uniformly mixing GP-m-AgNWs as a conductive filler and PEEK as a matrix according to a ratio, and then performing melt blending, extrusion and molding, or injection molding, to obtain an electro-shaped memory composite material. The molding method includes injection molding, extrusion molding, 3D printing molding, or 4D printing molding.

[0018] The last aspect of the present invention provides an application of an electro-shaped memory composite material in the preparation of interventional or implantable medical device materials, including the preparation of cardiovascular stents, orthopedic implants, dental braces and other materials and devices.

[0019] Beneficial technical effects:

[0020] The present invention grafts GP and AgNWs through a mercapto-containing silane coupling agent to obtain GP-m-AgNWs, which are used as conductive fillers and PEEK as a substrate to form an electro-shaped memory composite material. The composite material of the present invention has a low driving voltage (30V), which is lower than the human safety voltage (36V), has a fast shape memory recovery effect at a lower driving voltage, a shape fixation rate of more than 95%, a recovery time of no more than 60s, and a shape recovery rate of more than 95%; by adjusting the mass ratio of GP-m-AgNWs to PEEK, the performance of the composite material can be optimized; the electro-shaped memory composite material of the present invention has a wide range of application potentials in the biomedical field, such as cardiovascular and cerebrovascular stents, orthopedic implants, dental braces, and 3D and 4D printing, etc.; the preparation method of the present invention is simple, low-cost, easy to industrialize, and meets the needs of different application fields; it brings new solutions to the biomedical field;

[0021] The present invention adopts a mercapto-containing silane coupling agent to graft GP and AgNWs, which can improve the interface compatibility between the two high-conductivity fillers and the PEEK matrix; by forming a stable chemical bond, the mercapto-containing silane coupling agent enhances the interaction between the filler and the matrix, can effectively disperse the conductive filler, reduce filler aggregation, and ensure the formation of a complete and continuous conductive path in the PEEK matrix, thereby improving the conductivity of the composite material, and at the same time can reduce the driving voltage and time required for the shape recovery of the electro-shaped memory polymer, showing a rapid shape memory effect, with a recovery time of no more than 60s, and achieving a driving voltage lower than the human safety voltage (36V), which is only 30V, which not only improves the safety of use, but also meets the social demand for energy saving and low-voltage applications. At the same time, this rapid response capability is particularly important for application scenarios that require instant shape changes, such as stents and correctors in medical equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A shape memory test model. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.

[0025] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods.

[0026] Example 1

[0027] An electro-shaped memory composite material, comprising the following materials: GP-m-AgNWs as a conductive filler, and PEEK as a matrix;

[0028] Among them, the method for obtaining GP-m-AgNWs is:

[0029] In a 250 mL three-necked round-bottom flask, 200.0 mg of AgNWs and 42 g of mercaptopropyltrimethoxysilane were dissolved in 150 mL of dimethylformamide (DMF) solution under stirring, light protection and nitrogen flow to form a uniform dispersion, and then 200.0 mg of catalyst dicyclohexylcarbodiimide (DCC) was added thereto, and the system was heated to 155 °C to boil and condense under reflux for 2 h;

[0030] Then add 100.0 mg GP, stir and condense under reflux for 5 hours. The experiment is carried out in a strict anhydrous environment to prevent hydrolysis of 3-mercaptopropyltrimethoxysilane. After the reaction is completed, the reacted material system is vacuum filtered through a 0.45 μm polytetrafluoroethylene membrane to obtain a solid product, which is washed with anhydrous ethanol three times and dried in a vacuum drying oven at 60 ° C for 10 hours to constant weight to obtain GP-m-AgNWs.

[0031] The preparation method of the above-mentioned electro-shaped memory composite material includes the following steps: putting GP-m-AgNWs and PEEK powder in a mass ratio of 1:10, 1.5:10, and 2:10 into a high-speed mixer and mixing them evenly, and then directly performing injection molding to obtain the electro-shaped memory composite material.

[0032] Example 2

[0033] An electro-shaped memory composite material, comprising the following materials: GP-m-AgNWs as a conductive filler, and PEEK as a matrix;

[0034] Among them, the method for obtaining GP-m-AgNWs is:

[0035] In a 250 mL three-necked round-bottom flask, 200.0 mg of AgNWs and 45 g of γ-mercaptopropyltriethoxysilane were dissolved in 160 mL of acetone solution under stirring, light protection and nitrogen flow to form a uniform dispersion, and then 200.0 mg of catalyst dicyclohexylcarbodiimide (DCC) was added thereto, and the system was heated to 70 °C in a water bath to boil and condense under reflux for 1.5 h;

[0036] Then add 150.0 mg GP, stir and condense reflux for 4.5 hours. The experiment is carried out in a strict anhydrous environment to prevent hydrolysis of γ-mercaptopropyltriethoxysilane. After the reaction is completed, the reacted material system is vacuum filtered through a 0.45 μm polytetrafluoroethylene membrane to obtain a solid product, which is washed with anhydrous ethanol three times and dried in a vacuum drying oven at 60 ° C for 10 hours to constant weight to obtain GP-m-AgNWs.

[0037] The preparation method of the above-mentioned electro-shaped memory composite material comprises the following steps: putting GP-m-AgNWs and PEEK powder in a mass ratio of 0.5:10 into a high-speed mixer and mixing them thoroughly and evenly, and then directly performing injection molding to obtain the electro-shaped memory composite material.

[0038] Example 3

[0039] An electro-shaped memory composite material, comprising the following materials: GP-m-AgNWs as a conductive filler, and PEEK as a matrix;

[0040] Among them, the method for obtaining GP-m-AgNWs is:

[0041] In a 250 mL three-necked round-bottom flask, 200.0 mg of AgNWs and 48 g of 2-mercaptoethyltriethoxysilane were dissolved in 160 mL of tetrahydrofuran solution under stirring, light protection and nitrogen flow to form a uniform dispersion, and then 200.0 mg of catalyst dicyclohexylcarbodiimide (DCC) was added thereto, and the system was heated to 70 °C in a water bath to boil and reflux for 2.5 h;

[0042] Then add 200.0 mg GP, stir and condense reflux for 5.5 h. The experiment was carried out in a strict anhydrous environment to prevent hydrolysis of 2-mercaptoethyltriethoxysilane. After the reaction was completed, the reacted material system was vacuum filtered through a 0.45 μm polytetrafluoroethylene membrane to obtain a solid product, which was washed with anhydrous ethanol three times and dried in a vacuum drying oven at 60 ° C for 10 h to constant weight to obtain GP-m-AgNWs.

[0043] The preparation method of the above-mentioned electro-shaped memory composite material comprises the following steps: putting GP-m-AgNWs and PEEK powder in a mass ratio of 3:10 into a high-speed mixer and mixing them thoroughly and evenly, and then directly performing injection molding to obtain the electro-shaped memory composite material.

[0044] Comparative Example 1

[0045] In this case, surface modified GP (m-GP) is used as a filler and blended with PEEK. The blending ratio and preparation method are the same as those in Example 1.

[0046] Preparation of m-GP: In a 250mL three-necked round-bottom flask, 200.0mg GP and 20mL 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were dissolved in 120mL dimethylformamide (DMF) solution, and 200.0mg dicyclohexylcarbodiimide (DCC) was added as a catalyst; stirred to a reflux temperature of 155°C for condensation reflux for 5 hours. After the reaction was completed, vacuum filtered through a 0.45μm polytetrafluoroethylene membrane, the sample was washed 3 times with anhydrous ethanol, and the solid black powder obtained by filtration was placed in a vacuum drying oven and dried at 50°C for 10h to obtain m-GP.

[0047] Comparative Example 2

[0048] In this case, surface modified AgNWs (m-AgNWs) were used as fillers and blended with PEEK. The blending ratio and preparation method were the same as those in Example 1.

[0049] Preparation of m-AgNWs: In a 250 mL three-necked round-bottom flask, protected from light and passed with nitrogen, 200.0 mg of AgNWs and 40 mL of dodecanethiol were fully mixed and stirred to reach the reflux temperature for condensation and reflux for 2 hours. After completion, it was filtered through a 0.45 μm polytetrafluoroethylene membrane and washed three times with anhydrous ethanol. The solid silver powder obtained by filtration was placed in a vacuum drying oven and dried at 50 ° C for 10 h to obtain m-AgNWs.

[0050] test

[0051] Shape memory test method: Figure 1 The U-bending model is used to evaluate the electro-shaped memory process of the composite material, where θ is the angle between the electro-shaped recovery and the horizontal plane, and θ1 is the bending angle measured after cooling and shaping. First, the sample is heated to the melting temperature T g At 10°C above, a rectangular sample (100×10×2mm) was bent into a U shape, the stress was maintained and the sample was rapidly cooled to fix the deformation. Then a voltage of 30V was applied to the sample, and the change of the sample recovery angle (θ1-θ) over time (t) was recorded. The shape fixation rate is (θ1 / 180°) and the deformation recovery rate is (θ1-θ) / θ1.

[0052] The performance data of the above embodiments and comparative examples are shown in Table 1 below.

[0053] Table 1 Properties of electro-shaped memory composites

[0054]

[0055] As shown in Table 1, only using graphene or silver nanowires is not enough to form a good conductive network. The recovery time of Comparative Examples 1 and 2 is more than 60s, and the shape recovery rate is less than 90%. The present invention uses a mercapto-containing silane coupling agent to graft GP and AgNWs, which can improve the interface compatibility between the two high-conductivity fillers and the PEEK matrix; by forming a stable chemical bond, the mercapto-containing silane coupling agent enhances the interaction between the filler and the matrix, can effectively disperse the conductive filler, reduce filler aggregation, and ensure that a complete and continuous conductive path is formed in the PEEK matrix, thereby improving the conductivity of the composite material, and at the same time can reduce the driving voltage and time required for the shape recovery of the electro-induced shape memory polymer, showing a rapid shape memory effect, the recovery time is less than 60s at a driving voltage (only 30V) lower than the human safety voltage (36V), and the shape recovery rate exceeds 90%, which not only improves the safety of use, but also meets the social demand for energy saving and low-voltage applications.

[0056] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An electro-shaped memory composite material, characterized in that: The materials include the following weight percentages: GP-m-AgNWs as a conductive filler and PEEK as a matrix; The dosage of GP-m-AgNWs was 5–30% of the weight of PEEK; The GP-m-AgNWs are obtained by grafting GP and AgNWs using a mercapto-containing silane coupling agent, wherein the mass ratio of AgNWs to GP is 1:1-2; The method for obtaining the GP-m-AgNWs is as follows: AgNWs and a mercapto-containing silane coupling agent are mixed in an organic solvent under stirring, light-proof, anhydrous conditions and a protective atmosphere to form a uniform dispersion, an amine catalyst is added, heated and condensed under reflux, and then GP is added, and condensation and reflux are continued. After the reaction is completed, the material system after the reaction is filtered to obtain a solid product, and the solid product is washed with alcohol and dried to obtain the GP-m-AgNWs.

2. The electro-shaped memory composite material according to claim 1, characterized in that: GP is a single layer of flakes with a flake size of 5~10mm; the diameter of AgNWs is 30nm~40nm and the length is 20~50μm; The mercapto-containing silane coupling agent is selected from one or more of mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, mercaptopropylmethyldimethoxysilane, 2-mercaptoethyltriethoxysilane, (mercapto)methylsiloxane-dimethylsiloxane copolymer, and mercaptopropyl-terminated polydimethylsiloxane.

3. The electro-shaped memory composite material according to claim 2, characterized in that: The dosage ratio of AgNWs, mercapto-containing silane coupling agent, amide organic solvent and amine catalyst is 1g:200~250g:700~800mL:1g.

4. The electro-shaped memory composite material according to claim 1, characterized in that: The organic solvent is selected from one or more of DMF, DMAc, acetone, and tetrahydrofuran; the amine catalyst is dicyclohexylcarbodiimide; and the condensation reflux temperature is such that the organic solvent reaches a boiling point and can generate reflux.

5. The electro-shaped memory composite material according to claim 1, characterized in that: The condensation reflux time before adding GP is 1-3 hours, and the condensation reflux time after adding GP is 4-6 hours.

6. The method for preparing an electro-shaped memory composite material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: uniformly mixing GP-m-AgNWs as a conductive filler and PEEK as a matrix according to a proportion, and then performing melt blending, extrusion and molding, or injection molding to obtain an electro-shaped memory composite material.

7. Use of an electro-shaped memory composite material according to any one of claims 1 to 5 in the preparation of interventional and implantable medical device materials.