A rare earth modified aluminum alloy and preparation method thereof

Through high-entropy alloy modification and rare earth ytterbium ultrasonic treatment technology, combined with sodium hydroxide aqueous solution and silane hydrolysate, the shortcomings of aluminum alloy materials in terms of corrosion performance and processing flow performance are solved, and its mechanical and corrosion resistance are improved. It is suitable for Forming of complex thin-walled parts.

CN118389912BActive Publication Date: 2024-11-12BEIJING JUJIA MASCH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410488215.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2024-11-12
Estimated Expiration
2044-04-23

AI Technical Summary

Technical Problem

The existing aluminum alloy materials have shortcomings in corrosion performance and processing flow performance, which limits their application in automotive electronics and other fields.

Method used

High-entropy alloy powder and aluminum powder are used to make high-entropy alloy modified aluminum alloy through pressure permeation process, and rare earth ytterbium and aluminum blocks are used to make aluminum rare earth binary intermediate alloy through high-energy ultrasonic method, combining sodium hydroxide aqueous solution and silane hydrolysate The reaction solution was sonicated with the 8-hydroxyquinoline solution to form a rare earth doped aluminum alloy.

Benefits of technology

Improve the mechanical properties, processing fluidity and corrosion resistance of rare earth modified aluminum alloys, avoid the problem of differences in interface brittle phase and thermal expansion between traditional ceramic particles and metal matrix, and enhance its flow performance in the molding of complex thin-walled parts. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004804418980000101
    Figure BDA0004804418980000101
  • Figure BDA0004804418980000111
    Figure BDA0004804418980000111
  • Figure BDA0004804418980000112
    Figure BDA0004804418980000112
Patent Text Reader

Abstract

The invention discloses a rare earth modified aluminum alloy and a preparation method thereof, and relates to the technical field of alloy materials. When preparing the rare earth modified aluminum alloy, the present invention uses aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder, and copper powder as raw materials, and adopts a wet grinding method to prepare a high entropy alloy powder; the high entropy alloy powder and aluminum powder are subjected to a pressure infiltration process to prepare a high entropy alloy modified aluminum alloy; rare earth ytterbium and aluminum blocks are subjected to a high-energy ultrasonic method to prepare an aluminum rare earth binary master alloy; aluminum rare earth binary master alloy and high entropy alloy modified aluminum alloy are cast and molded to prepare a rare earth doped aluminum alloy; the modified aluminum alloy is sequentially immersed in a sodium hydroxide aqueous solution, a silane hydrolyzate, and an 8-hydroxyquinoline reaction solution for ultrasonic treatment to prepare a rare earth modified aluminum alloy. The rare earth modified aluminum alloy prepared by the present invention has excellent processing fluidity, corrosion resistance, and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy materials, in particular to a rare earth modified aluminum alloy and a preparation method thereof. Background Art

[0002] Aluminum alloy is one of the most commonly used lightweight materials. It is widely used in the fields of automobile, electronics, aviation, construction, etc. due to its excellent properties such as low density, high specific strength and good plasticity. With the rapid development of the automotive electronics industry in recent years, the market has put forward higher requirements on the performance of aluminum alloy materials. In addition to requiring aluminum alloy materials to have higher mechanical properties, corrosion performance is also an important property that cannot be ignored. Poor corrosion performance will greatly limit the application range of the alloy. In addition, among the casting properties of the alloy, flowability is a very important parameter, which is especially important for the forming of complex thin-walled parts. Therefore, improving the corrosion resistance and processing flowability of aluminum alloys has very important practical significance and theoretical value. Summary of the invention

[0003] The purpose of the present invention is to provide a rare earth modified aluminum alloy and a preparation method thereof, so as to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] A rare earth modified aluminum alloy is prepared by subjecting high entropy alloy powder and aluminum powder to a pressure infiltration process to obtain a high entropy alloy modified aluminum alloy; casting an aluminum-rare earth binary master alloy and a high entropy alloy modified aluminum alloy to obtain a rare earth doped aluminum alloy; and immersing the modified aluminum alloy in a sodium hydroxide aqueous solution, a silane hydrolyzate, and an 8-hydroxyquinoline reaction solution in sequence for ultrasonic treatment to obtain the rare earth modified aluminum alloy.

[0006] As an optimization, the high entropy alloy powder is prepared by wet grinding using aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder and copper powder as raw materials.

[0007] As an optimization, the aluminum-rare earth binary master alloy is prepared by using a high-energy ultrasonic method to prepare rare earth ytterbium and aluminum blocks.

[0008] As an optimization, the mass fraction of the sodium hydroxide aqueous solution is 20-24%.

[0009] A method for preparing a rare earth modified aluminum alloy comprises the following preparation steps:

[0010] (1) Aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder and copper powder are mixed uniformly in a mass ratio of 1:1:(1.6-1.8):2:(2.1-2.3):(2.2-2.4), placed in a powder mixer, stirred and mixed at 300-500 r / min for 14-16 hours to obtain a mixed powder; the mixed powder is placed in a stainless steel ball mill at a ball-to-material ratio of (10-12):1, a process control agent 2-2.2 times the mass of the mixed powder is added, and the mixed powder is ball milled for 40-42 hours at 3-5 Pa and 100-120°C. Drying for 20 to 24 hours, passing through a 500-mesh sieve to obtain a high-entropy alloy powder; mixing the high-entropy alloy powder and aluminum powder in a volume ratio of 1: (2 to 2.2) and placing in a powder mixer, stirring and mixing at 300 to 500 r / min for 14 to 16 hours to obtain a mixed alloy powder; cold-pressing the mixed alloy powder at 10 to 20 MPa, placing in a high-temperature electric furnace, keeping the temperature at 600 to 700° C. for 4 to 6 hours, pouring at 700 to 800° C., keeping the pressure for 10 to 20 minutes, and demolding to obtain a high-entropy alloy modified aluminum alloy;

[0011] (2) Preheating a graphite crucible to 380-420°C in a pit-type resistance furnace, placing a dried aluminum block in the crucible, raising the temperature until the aluminum block is completely melted, raising the temperature to 730-750°C, removing slag and degassing, crushing rare earth ytterbium 0.03-0.05 times the mass of the aluminum block into small particles with a particle size of 0.1-0.2 mm and wrapping them in aluminum foil, pressing them into the melt with a bell jar, stirring them fully and keeping them warm for 50-60 minutes after they are completely melted, performing high-energy intermittent ultrasonic treatment, reducing the melt temperature to 690-710°C, refining the melt, removing slag, and pouring them into a metal mold to obtain aluminum rare earth Binary master alloy; preheating a graphite crucible to 380-420° C. in a pit-type resistance furnace, placing a high-entropy alloy particle-modified aluminum alloy in the crucible and heating it until it is completely melted, crushing an aluminum-rare earth binary master alloy of 0.10-0.12 times the mass of the high-entropy alloy particle-modified aluminum alloy into small particles with a particle size of 0.1-0.2 mm and wrapping them in aluminum foil, pressing them into the alloy melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 50-60 minutes to ensure that they are fully metamorphosed, lowering the melt temperature to 690-710° C., refining and deslagging the melt, and pouring them into a metal mold to obtain a rare earth-doped aluminum alloy;

[0012] (3) The rare earth doped aluminum alloy is immersed in a sodium hydroxide aqueous solution with a mass fraction of 20 to 24%, ultrasonically treated for 5 to 7 minutes, taken out, washed with deionized water for 3 to 5 times, immersed in a silane hydrolyzate solution, ultrasonically treated for 3 to 4 hours, taken out, and kept warm at 140 to 150° C. for 2 to 3 hours to obtain a silane surface treated aluminum alloy; the silane surface treated aluminum alloy is immersed in an 8-hydroxyquinoline reaction solution, ultrasonically treated at 50 to 60° C. for 3 to 4 hours, taken out, washed with anhydrous ethanol and deionized water for 3 to 5 times respectively, and dried at 5 to 7 Pa and 50 to 60° C. for 4 to 6 hours to obtain a rare earth modified aluminum alloy.

[0013] As an optimization, the process control agent in step (1) is one of anhydrous ethanol, cyclohexane, n-hexane, n-heptane, and toluene.

[0014] As an optimization, the specific operation process of the high-energy intermittent ultrasonic treatment in step (2) is: the ultrasonic output frequency is 1.5KHz, the ultrasonic time is 20 to 30 minutes, the high-energy ultrasonic application time is 70 to 80 seconds each time, and the intermittent time is 70 to 80 seconds.

[0015] As an optimization, the silane hydrolyzate in step (3) is prepared by uniformly mixing 3-aminopropyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, anhydrous ethanol and deionized water in a mass ratio of 1:(1.3-1.5):(2.2-2.5):(8-10), and adjusting the pH to 4.8-5.0 with a hydrochloric acid aqueous solution with a mass fraction of 10-12%.

[0016] As an optimization, the 8-hydroxyquinoline reaction solution in step (3) is prepared by uniformly mixing 5-chloromethyl-8-hydroxyquinoline hydrochloride, triethylamine, and N-methylpyrrolidone in a mass ratio of 1:(0.01-0.03):(8-10).

[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0018] The invention uses aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder and copper powder as raw materials to prepare high entropy alloy powder by wet grinding; uses pressure infiltration process to prepare high entropy alloy modified aluminum alloy by using high-energy ultrasonic method to prepare aluminum rare earth binary master alloy with rare earth ytterbium and aluminum block; casts aluminum rare earth binary master alloy and high entropy alloy modified aluminum alloy to prepare rare earth doped aluminum alloy; prepares silane hydrolyzate by 3-aminopropyltriethoxysilane and heptadecafluorodecyltrimethoxysilane; prepares reaction solution by 5-chloromethyl-8-hydroxyquinoline hydrochloride; and sequentially immerses the modified aluminum alloy in sodium hydroxide aqueous solution, silane hydrolyzate and reaction solution for ultrasonic treatment to prepare rare earth modified aluminum alloy.

[0019] Firstly, aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder and copper powder are used as raw materials and high entropy alloy powder is prepared by wet grinding; high entropy alloy modified aluminum alloy is prepared by pressure infiltration process by combining high entropy alloy powder and aluminum powder; in traditional aluminum alloy preparation process, ceramic particles and metal particles are often used as reinforcing materials, but the wettability between ceramic particles and metal matrix is ​​poor, and brittle phase is easily generated at the interface, resulting in low interface bonding strength, and large difference in thermal expansion coefficient between metal and ceramic, resulting in stress concentration in composite materials; metal particles have good wettability with the group, but the reinforcing performance of metal particles is not as good as that of ceramic particles; high entropy alloy powder and matrix not only have excellent wettability, but also have the characteristics of high strength and wear resistance, which well combines the respective advantages of ceramic particles and metal particles, giving rare earth modified aluminum alloy excellent mechanical properties without reducing the plasticity of rare earth modified aluminum alloy.

[0020] Secondly, rare earth ytterbium and aluminum block are prepared into aluminum rare earth binary master alloy through high energy ultrasonic method; aluminum rare earth binary master alloy and high entropy alloy modified aluminum alloy are cast to prepare rare earth doped aluminum alloy; rare earth ytterbium is a substance with high activity and surface activity, which makes the surface tension of the melt and the critical radius of nucleation smaller, and the addition of rare earth ytterbium forms a layer of surface active film between the grains and the melt, and this active film inhibits the growth of grains, thereby refining the grains and increasing the processing fluidity of the rare earth modified aluminum alloy.

[0021] Finally, 3-aminopropyltriethoxysilane and heptadecafluorodecyltrimethoxysilane are prepared into a silane hydrolyzate; 5-chloromethyl-8-hydroxyquinoline hydrochloride is prepared into a reaction solution; the modified aluminum alloy is immersed in a sodium hydroxide aqueous solution, a silane hydrolyzate, and a reaction solution in sequence and subjected to ultrasonic treatment to obtain a rare earth modified aluminum alloy; the modified aluminum alloy is treated with a sodium hydroxide aqueous solution to generate a large number of hydroxyl groups on the surface of the modified aluminum alloy, 3-aminopropyltriethoxysilane and heptadecafluorodecyltrimethoxysilane are hydrolyzed to generate active silanols, and the hydroxyl groups on the surface of the modified aluminum alloy and the active silanols on 3-aminopropyltriethoxysilane and heptadecafluorodecyltrimethoxysilane are adsorbed on the metal surface through hydrogen bonds, and the hydrogen bonds are dehydrated and condensed to form covalent bonds, thereby finally forming a silicon-containing alloy. The alkane film is attached to the surface of the modified aluminum alloy. The large number of fluorine atoms on the heptadecafluorodecyltrimethoxysilane have low reactivity and hydrophobicity, which can give the rare earth modified aluminum alloy excellent corrosion resistance. The chlorine atoms on 5-chloromethyl-8-hydroxyquinoline hydrochloride react with the amino groups on 3-aminopropyltriethoxysilane to introduce a large number of 8-hydroxyquinoline structures on the surface of the rare earth modified aluminum alloy. The 8-hydroxyquinoline structure can form a complex with the metal ions copper, aluminum, nickel, etc. escaped from the rare earth modified aluminum alloy, which can inhibit the occurrence of local corrosion of active points on the surface of the rare earth modified aluminum alloy. The 8-hydroxyquinoline structure can form an insoluble chelate with aluminum ions and copper ions and adsorb on the surface of the rare earth modified aluminum alloy to block the corrosion from continuing. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] A method for preparing a rare earth modified aluminum alloy, the method comprising the following preparation steps:

[0025] (1) Aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder, and copper powder were mixed in a mass ratio of 1:1:1.6:2:2.1:2.2, placed in a powder mixer, and stirred at 300 r / min for 14 hours to obtain a mixed powder; the mixed powder was placed in a stainless steel ball mill at a ball-to-material ratio of 10:1, cyclohexane twice the mass of the mixed powder was added, ball milled for 40 hours, dried at 3Pa, 100°C for 24 hours, and passed through a 500-mesh sieve to obtain a high-entropy alloy powder; the high-entropy alloy powder and aluminum powder were mixed in a volume ratio of 1:2, placed in a powder mixer, and stirred at 300 r / min for 14 hours to obtain a mixed alloy powder; the mixed alloy powder was cold-pressed at 10 MPa, placed in a high-temperature electric furnace, kept at 600°C for 6 hours, poured at 700°C, kept at pressure for 10 minutes, and demolded to obtain a high-entropy alloy modified aluminum alloy;

[0026] (2) Preheating a graphite crucible to 380°C in a pit-type resistance furnace, placing a dried aluminum block in the crucible, raising the temperature until the aluminum block is completely melted, raising the temperature to 730°C, removing slag and degassing, crushing 0.03 times the mass of the aluminum block into small particles with a particle size of 0.1 mm and wrapping them in aluminum foil, pressing them into the melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 50 minutes, and performing high-energy intermittent ultrasonic treatment, with an ultrasonic output frequency of 1.5 KHz, an ultrasonic time of 20 minutes, and a high-energy ultrasonic application time of 70 seconds each time, with an interval time of 70 seconds, to reduce the melt temperature to 690°C and refine the melt , slag removal, pouring in a metal mold to obtain an aluminum-rare earth binary master alloy; preheating a graphite crucible to 380°C in a pit-type resistance furnace, placing the high-entropy alloy particle-modified aluminum alloy in the crucible and heating it to complete melting, crushing the aluminum-rare earth binary master alloy with a mass of 0.10 times that of the high-entropy alloy particle-modified aluminum alloy into small particles with a particle size of 0.1 mm and wrapping them in aluminum foil, pressing them into the alloy melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 50 minutes to ensure that they are fully metamorphosed, lowering the melt temperature to 690°C, refining and slag removal of the melt, and pouring them in a metal mold to obtain a rare earth-doped aluminum alloy;

[0027] (3) 3-aminopropyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, anhydrous ethanol, and deionized water were mixed uniformly in a mass ratio of 1:1.3:2.2:8, and the pH value was adjusted to 4.8 with a 10% by mass aqueous solution of hydrochloric acid to prepare a silane hydrolyzate; the rare earth-doped aluminum alloy was immersed in a 20% by mass aqueous solution of sodium hydroxide, ultrasonically treated for 5 minutes, taken out, washed with deionized water for 3 times, and then immersed in the silane hydrolyzate, and ultrasonically treated for 5 minutes. The aluminum alloy was treated for 3 hours, taken out, and kept at 140°C for 3 hours to obtain a silane surface-treated aluminum alloy; 5-chloromethyl-8-hydroxyquinoline hydrochloride, triethylamine, and N-methylpyrrolidone were mixed uniformly at a mass ratio of 1:0.01:8 to prepare a reaction solution; the aluminum alloy treated with the silane surface was immersed in the reaction solution, ultrasonically treated at 50°C for 3 hours, taken out, washed with anhydrous ethanol and deionized water for 3 times each, and dried at 5Pa and 50°C for 6 hours to obtain a rare earth modified aluminum alloy.

[0028] Example 2

[0029] A method for preparing a rare earth modified aluminum alloy, the method comprising the following preparation steps:

[0030] (1) Aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder and copper powder were mixed in a mass ratio of 1:1:1.7:2:2.2:2.3, placed in a powder mixer, and stirred at 400 r / min for 15 hours to obtain a mixed powder; the mixed powder was placed in a stainless steel ball mill at a ball-to-material ratio of 11:1, cyclohexane 2.1 times the mass of the mixed powder was added, ball milled for 41 hours, dried at 4Pa, 110°C for 22 hours, and passed through a 500-mesh sieve to obtain a high-entropy alloy powder; the high-entropy alloy powder and aluminum powder were mixed in a volume ratio of 1:2.1, placed in a powder mixer, and stirred at 400 r / min for 15 hours to obtain a mixed alloy powder; the mixed alloy powder was cold-pressed at 15 MPa, placed in a high-temperature electric furnace, kept at 650°C for 5 hours, poured at 750°C, kept at pressure for 15 minutes, and demolded to obtain a high-entropy alloy modified aluminum alloy;

[0031] (2) Preheating a graphite crucible to 400°C in a pit-type resistance furnace, placing a dried aluminum block in the crucible, raising the temperature until the aluminum block is completely melted, raising the temperature to 740°C, removing slag and degassing, crushing 0.04 times the mass of the aluminum block into small particles with a particle size of 0.15 mm and wrapping them in aluminum foil, pressing them into the melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 55 minutes, and performing high-energy intermittent ultrasonic treatment, with an ultrasonic output frequency of 1.5 KHz, an ultrasonic time of 25 minutes, and a high-energy ultrasonic application time of 75 seconds each time, with an interval time of 75 seconds, to reduce the melt temperature to 700°C and refine the melt , slag removal, pouring in a metal mold to obtain an aluminum-rare earth binary master alloy; preheating a graphite crucible to 400°C in a pit-type resistance furnace, placing an aluminum alloy modified with high-entropy alloy particles in a crucible and heating it to complete melting, crushing an aluminum-rare earth binary master alloy with a mass of 0.11 times that of the aluminum alloy modified with high-entropy alloy particles into small particles with a particle size of 0.15 mm and wrapping them in aluminum foil, pressing them into the alloy melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 55 minutes to ensure that they are fully metamorphosed, lowering the melt temperature to 700°C, refining and slag removal of the melt, and pouring them in a metal mold to obtain a rare earth-doped aluminum alloy;

[0032] (3) 3-aminopropyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, anhydrous ethanol, and deionized water were mixed uniformly in a mass ratio of 1:1.4:2.35:9, and the pH value was adjusted to 4.9 with a 11% mass fraction hydrochloric acid aqueous solution to prepare a silane hydrolyzate; the rare earth-doped aluminum alloy was immersed in a 22% mass fraction sodium hydroxide aqueous solution, ultrasonically treated for 6 minutes, taken out, washed with deionized water for 4 times, and then immersed in the silane hydrolyzate and ultrasonically treated. 3.5h, take it out, keep it at 145℃ for 2.5h to obtain silane surface treated aluminum alloy; 5-chloromethyl-8-hydroxyquinoline hydrochloride, triethylamine and N-methylpyrrolidone are evenly mixed in a mass ratio of 1:0.02:9 to prepare a reaction solution; immerse the silane surface treated aluminum alloy in the reaction solution, ultrasonically treat it at 55℃ for 3.5h, take it out, wash it with anhydrous ethanol and deionized water for 4 times respectively, and dry it at 6Pa, 55℃ for 5h to obtain a rare earth modified aluminum alloy.

[0033] Example 3

[0034] A method for preparing a rare earth modified aluminum alloy, the method comprising the following preparation steps:

[0035] (1) Aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder, and copper powder were mixed in a mass ratio of 1:1:1.8:2:2.3:2.4, placed in a powder mixer, and stirred at 500 r / min for 16 hours to obtain a mixed powder; the mixed powder was placed in a stainless steel ball mill at a ball-to-material ratio of 12:1, cyclohexane 2.2 times the mass of the mixed powder was added, ball milled for 42 hours, dried at 5 Pa, 120°C for 20 hours, and passed through a 500-mesh sieve to obtain a high-entropy alloy powder; the high-entropy alloy powder and aluminum powder were mixed in a volume ratio of 1:2.2, placed in a powder mixer, and stirred at 500 r / min for 16 hours to obtain a mixed alloy powder; the mixed alloy powder was cold-pressed at 20 MPa, placed in a high-temperature electric furnace, kept at 700°C for 4 hours, poured at 800°C, kept at pressure for 20 minutes, and demolded to obtain a high-entropy alloy modified aluminum alloy;

[0036] (2) Preheating a graphite crucible to 420°C in a pit-type resistance furnace, placing a dried aluminum block in the crucible, raising the temperature until the aluminum block is completely melted, raising the temperature to 750°C, removing slag and degassing, crushing 0.05 times the mass of the aluminum block into small particles with a particle size of 0.2 mm and wrapping them in aluminum foil, pressing them into the melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 60 minutes, and performing high-energy intermittent ultrasonic treatment, with an ultrasonic output frequency of 1.5 KHz, an ultrasonic time of 30 minutes, and a high-energy ultrasonic application time of 80 seconds each time, with an interval time of 80 seconds, to reduce the melt temperature to 710°C and refine the melt , slag removal, pouring in a metal mold to obtain an aluminum-rare earth binary master alloy; preheating a graphite crucible to 420°C in a pit-type resistance furnace, placing the high-entropy alloy particle-modified aluminum alloy in the crucible and heating it to complete melting, crushing the aluminum-rare earth binary master alloy with a mass of 0.12 times that of the high-entropy alloy particle-modified aluminum alloy into small particles with a particle size of 0.2 mm and wrapping them in aluminum foil, pressing them into the alloy melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 60 minutes to ensure that they are fully metamorphosed, lowering the melt temperature to 710°C, refining and slag removal of the melt, and pouring them in a metal mold to obtain a rare earth-doped aluminum alloy;

[0037] (3) 3-aminopropyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, anhydrous ethanol, and deionized water were mixed uniformly in a mass ratio of 1:1.5:2.5:10, and the pH value was adjusted to 5.0 with a 12% by mass aqueous solution of hydrochloric acid to prepare a silane hydrolyzate; the rare earth-doped aluminum alloy was immersed in a 24% by mass aqueous solution of sodium hydroxide, ultrasonically treated for 7 minutes, taken out, washed with deionized water for 5 times, and then immersed in the silane hydrolyzate, and ultrasonically treated for 7 minutes. The aluminum alloy was treated for 4 hours, taken out, and kept at 150°C for 2 hours to obtain a silane surface-treated aluminum alloy; 5-chloromethyl-8-hydroxyquinoline hydrochloride, triethylamine, and N-methylpyrrolidone were mixed uniformly at a mass ratio of 1:0.03:10 to prepare a reaction solution; the aluminum alloy treated with the silane surface was immersed in the reaction solution, ultrasonically treated at 60°C for 4 hours, taken out, washed with anhydrous ethanol and deionized water for 5 times each, and dried at 7Pa and 60°C for 4 hours to obtain a rare earth modified aluminum alloy.

[0038] Comparative Example 1

[0039] The preparation method of the rare earth modified aluminum alloy of Comparative Example 1 is different from that of Example 2 in that step (1) is not performed, and step (2) is modified as follows: a graphite crucible is preheated to 400° C. in a pit-type resistance furnace, a dried aluminum block is placed in the crucible, and the temperature is increased until the aluminum block is completely melted, the temperature is increased to 740° C., and after slag removal and degassing, rare earth ytterbium with a mass of 0.04 times the mass of the aluminum block is crushed into small particles with a particle size of 0.15 mm and wrapped in aluminum foil, and pressed into the melt with a bell jar, and after it is completely melted, it is fully stirred and kept warm for 55 minutes, and high-energy intermittent ultrasonic treatment is performed, the ultrasonic output frequency is 1.5 KHz, the ultrasonic time is 25 minutes, and the high-energy ultrasonic application time is 7 5s, rest time 75s, lower the melt temperature to 700°C, refine and remove slag from the melt, and pour it into a metal mold to obtain an aluminum-rare earth binary master alloy; preheat a graphite crucible to 400°C in a pit-type resistance furnace, put an aluminum block into the crucible and heat it until it is completely melted, crush the aluminum-rare earth binary master alloy with a mass of 0.11 times the mass of the aluminum block into small particles with a particle size of 0.15mm and wrap them in aluminum foil, press them into the alloy melt with a bell jar, stir them fully and keep them warm for 55min to ensure that they are fully metamorphosed, lower the melt temperature to 700°C, refine and remove slag from the melt, and pour it into a metal mold to obtain a rare earth-doped aluminum alloy. The remaining steps are the same as in Example 2.

[0040] Comparative Example 2

[0041] The preparation method of the rare earth modified aluminum alloy of Comparative Example 2 is different from that of Example 2 in that step (2) is not performed, and step (3) is modified as follows: 3-aminopropyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, anhydrous ethanol, and deionized water are mixed uniformly in a mass ratio of 1:1.4:2.35:9, and the pH value is adjusted to 4.9 with a 11% mass fraction hydrochloric acid aqueous solution to obtain a silane hydrolyzate; the high entropy alloy modified aluminum alloy is immersed in a 22% mass fraction sodium hydroxide aqueous solution, ultrasonically treated for 6 minutes, taken out, and deionized water is removed. The aluminum alloy surface treated with silane was washed with water for 4 times, immersed in silane hydrolyzate, ultrasonically treated for 3.5 hours, taken out, and kept at 145°C for 2.5 hours to obtain the aluminum alloy surface treated with silane; 5-chloromethyl-8-hydroxyquinoline hydrochloride, triethylamine, and N-methylpyrrolidone were mixed uniformly in a mass ratio of 1:0.02:9 to prepare a reaction solution; the aluminum alloy surface treated with silane was immersed in the reaction solution, ultrasonically treated at 55°C for 3.5 hours, taken out, washed with anhydrous ethanol and deionized water 4 times each, and dried at 6Pa, 55°C for 5 hours to obtain the rare earth modified aluminum alloy. The remaining steps are the same as those in Example 2.

[0042] Comparative Example 3

[0043] The preparation method of the rare earth modified aluminum alloy of Comparative Example 3 is different from that of Example 2 only in step (3). Step (3) is modified as follows: 3-aminopropyltriethoxysilane, anhydrous ethanol, and deionized water are mixed uniformly in a mass ratio of 1:2.35:9, and the pH value is adjusted to 4.9 with a 11% mass fraction hydrochloric acid aqueous solution to obtain a silane hydrolyzate; the rare earth doped aluminum alloy is immersed in a 22% mass fraction sodium hydroxide aqueous solution, ultrasonically treated for 6 minutes, taken out, washed 4 times with deionized water, and then Immerse in silane hydrolysis solution, ultrasonically treat for 3.5 hours, take out, keep warm at 145°C for 2.5 hours, and obtain silane surface treated aluminum alloy; 5-chloromethyl-8-hydroxyquinoline hydrochloride, triethylamine, and N-methylpyrrolidone are mixed uniformly in a mass ratio of 1:0.02:9 to prepare a reaction solution; immerse the silane surface treated aluminum alloy in the reaction solution, ultrasonically treat at 55°C for 3.5 hours, take out, wash with anhydrous ethanol and deionized water 4 times each, and dry at 6Pa, 55°C for 5 hours to obtain a rare earth modified aluminum alloy. The remaining steps are the same as in Example 2.

[0044] Comparative Example 4

[0045] The preparation method of the rare earth modified aluminum alloy of Comparative Example 4 is different from that of Example 2 only in step (3), and step (3) is modified as follows: 17-fluorodecyltrimethoxysilane, anhydrous ethanol, and deionized water are mixed uniformly in a mass ratio of 1:2.35:9, and the pH is adjusted to 4.9 with a 11% mass fraction hydrochloric acid aqueous solution to obtain a silane hydrolyzate; the rare earth doped aluminum alloy is immersed in a 22% mass fraction sodium hydroxide aqueous solution, ultrasonically treated for 6 minutes, taken out, washed with deionized water 4 times, immersed in the silane hydrolyzate again, ultrasonically treated for 3.5 hours, taken out, and kept warm at 145° C. for 2.5 hours to obtain a rare earth modified aluminum alloy. The remaining steps are the same as those of Example 2.

[0046] Comparative Example 5

[0047] The preparation method of the rare earth modified aluminum alloy of Comparative Example 5 is different from that of Example 2 in that step (3) is not performed, and step (2) is modified as follows: a graphite crucible is preheated to 400° C. in a pit-type resistance furnace, a dried aluminum block is placed in the crucible, and the temperature is increased until the aluminum block is completely melted, the temperature is increased to 740° C., and after slag removal and degassing, rare earth ytterbium with a mass of 0.04 times the mass of the aluminum block is crushed into small particles with a particle size of 0.15 mm and wrapped in aluminum foil, and pressed into the melt with a bell jar, and after it is completely melted, it is fully stirred and kept warm for 55 minutes, and high-energy intermittent ultrasonic treatment is performed, the ultrasonic output frequency is 1.5 KHz, the ultrasonic time is 25 minutes, the high-energy ultrasonic application time is 75 seconds each time, and the intermittent time is 75 seconds. s, the melt temperature is reduced to 700 ° C, the melt is refined and deslagging, and poured in a metal mold to obtain an aluminum rare earth binary master alloy; the graphite crucible is preheated to 400 ° C in a pit resistance furnace, the high entropy alloy particle modified aluminum alloy is placed in the crucible and heated to completely melted, the aluminum rare earth binary master alloy with a mass of 0.11 times the high entropy alloy particle modified aluminum alloy is crushed into small particles with a particle size of 0.15 mm and wrapped in aluminum foil, and pressed into the alloy melt with a bell jar, and after it is completely melted, it is fully stirred and kept warm for 55 minutes to ensure that it is fully metamorphosed, the melt temperature is reduced to 700 ° C, the melt is refined and deslagging, and poured in a metal mold to obtain a rare earth modified aluminum alloy. The remaining steps are the same as in Example 2.

[0048] Test Example 1

[0049] Mechanical properties test method: The examples and comparative examples were prepared into standard specimens according to GB / T228, and the tensile strength of the examples and comparative examples was tested using a universal electronic tensile testing machine, with the tensile rate set to 0.05 mm / min. The results are shown in Table 1.

[0050] Table 1

[0051]

[0052]

[0053] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 1, it can be found that the rare earth modified aluminum alloy prepared in the present invention has good mechanical properties.

[0054] By comparison, the tensile strength of Examples 1 to 3 is greater than that of Comparative Example 1, indicating that high entropy alloy powder is prepared by wet grinding using aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder, and copper powder as raw materials; high entropy alloy-modified aluminum alloy is prepared by pressure infiltration process using high entropy alloy powder and aluminum powder; in traditional aluminum alloy preparation processes, ceramic particles and metal particles are often used as reinforcing materials, but the wettability of ceramic particles and metal matrix is ​​poor, and brittle phases are easily generated at the interface, resulting in low interface bonding strength, and a large difference in thermal expansion coefficients between metal and ceramic, resulting in stress concentration in the composite material; metal particles have good wettability with the group, but the reinforcement performance of metal particles is not as good as that of ceramic particles; high entropy alloy powder and matrix not only have excellent wettability, but also have the characteristics of high strength and wear resistance, which well combines the respective advantages of ceramic particles and metal particles, and gives rare earth modified aluminum alloy excellent mechanical properties.

[0055] Test Example 2

[0056] Processing fluidity performance test

[0057] Test method: The spiral method is adopted to test the fluidity of the alloy melt. The length of the spiral cavity of the spiral flow channel mold made of H13 mold steel is 1200mm, the flow channel cross-section is 10mm wide and 4mm high, the mass of the alloy tested each time is 500g, the pouring temperature is 760℃, the temperature-stable alloy melts of the embodiment and the comparative example are refined, degassed and slag-stripped, and then poured into the fluidity mold preheated to 200℃. After the alloy solidifies and cools, the mold is opened to measure the flow length. The results are shown in Table 2.

[0058] Table 2

[0059]

[0060]

[0061] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 2, it can be found that the rare earth modified aluminum alloy prepared in the present invention has good processing flowability.

[0062] By comparison, the flow lengths of Examples 1 to 3 are greater than the flow length of Comparative Example 2, which indicates that the aluminum-rare-earth binary master alloy is prepared by high-energy ultrasonic method using rare earth ytterbium and aluminum block; the aluminum-rare-earth binary master alloy and the high-entropy alloy modified aluminum alloy are cast to prepare the rare earth-doped aluminum alloy; rare earth ytterbium is a highly active and surface-active substance, which reduces the surface tension of the melt and the critical radius of nucleation, and the addition of rare earth ytterbium forms a surface-active film between the grains and the melt, and this active film inhibits the growth of the grains, thereby refining the grains and increasing the processing fluidity of the rare earth modified aluminum alloy.

[0063] Test Example 3

[0064] Corrosion resistance test

[0065] Test method: Weigh the mass of the embodiment and the comparative example as m1, immerse the weighed embodiment and the comparative example in a 10% hydrochloric acid aqueous solution, let stand for 48 hours, take out, dry at 5Pa, 100°C for 5 hours, weigh the mass of the embodiment and the comparative example after hydrochloric acid treatment as m2, calculate the corrosion rate of the embodiment and the comparative example, corrosion rate = (m1-m2) / m1×100%. The results are shown in Table 3.

[0066] Table 3

[0067]

[0068]

[0069] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 3, it can be found that the rare earth modified aluminum alloy prepared in the present invention has good corrosion resistance.

[0070] By comparison, the corrosion rates of Examples 1 to 3 are lower than those of Comparative Examples 3 to 5, indicating that 3-aminopropyltriethoxysilane and heptadecafluorodecyltrimethoxysilane are prepared into a silane hydrolyzate; 5-chloromethyl-8-hydroxyquinoline hydrochloride is prepared into a reaction solution; the modified aluminum alloy is sequentially immersed in a sodium hydroxide aqueous solution, a silane hydrolyzate, and a reaction solution for ultrasonic treatment to obtain a rare earth modified aluminum alloy; the modified aluminum alloy is treated with a sodium hydroxide aqueous solution to generate a large number of hydroxyl groups on the surface of the modified aluminum alloy, 3-aminopropyltriethoxysilane and heptadecafluorodecyltrimethoxysilane are hydrolyzed to generate active silanols, and the hydroxyl groups on the surface of the modified aluminum alloy are adsorbed on the metal surface through hydrogen bonds with the active silanols on 3-aminopropyltriethoxysilane and heptadecafluorodecyltrimethoxysilane, and the hydrogen bonds are desorbed. Water condenses to form a covalent bond, and finally forms a silane film attached to the surface of the modified aluminum alloy. The large number of fluorine atoms on the heptadecafluorodecyltrimethoxysilane have low reactivity and hydrophobicity, which can give the rare earth modified aluminum alloy excellent corrosion resistance. The chlorine atoms on the 5-chloromethyl-8-hydroxyquinoline hydrochloride react with the amino groups on the 3-aminopropyltriethoxysilane to introduce a large number of 8-hydroxyquinoline structures on the surface of the rare earth modified aluminum alloy. The 8-hydroxyquinoline structure can form a complex with the metal ions copper, aluminum, nickel, etc. that escape from the rare earth modified aluminum alloy, which can inhibit the occurrence of local corrosion of active points on the surface of the rare earth modified aluminum alloy. The 8-hydroxyquinoline structure can form an insoluble chelate with aluminum ions and copper ions and adsorb on the surface of the rare earth modified aluminum alloy to block the corrosion from continuing.

[0071] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a rare earth modified aluminum alloy, characterized in that: The method comprises the following preparation steps: (1) Mix aluminum powder, silicon powder, titanium powder, chromium powder, nickel powder and copper powder in a mass ratio of 1:1:(1.6~1.8):2:(2.1~2.3):(2.2~2.4), place in a powder mixer, stir and mix at 300~500r / min for 14~16h to obtain a mixed powder; place the mixed powder in a stainless steel ball mill at a ball-to-material ratio of (10~12):1, add a process control agent 2~2.2 times the mass of the mixed powder, ball mill for 40~42h, and heat at 3~5Pa, 100~120℃ Dry for 20-24 hours, pass through a 500-mesh sieve to obtain a high-entropy alloy powder; mix the high-entropy alloy powder and aluminum powder in a volume ratio of 1: (2-2.2) and place in a powder mixer, stir and mix at 300-500 r / min for 14-16 hours to obtain a mixed alloy powder; cold-press the mixed alloy powder at 10-20 MPa, place in a high-temperature electric furnace, keep warm at 600-700°C for 4-6 hours, pour at 700-800°C, keep the pressure for 10-20 minutes, and demold to obtain a high-entropy alloy modified aluminum alloy; (2) Preheating a graphite crucible to 380-420°C in a pit-type resistance furnace, placing a dry aluminum block in the crucible, raising the temperature until the aluminum block is completely melted, raising the temperature to 730-750°C, removing slag and degassing, crushing rare earth ytterbium with a particle size of 0.1-0.2 mm with a mass of 0.03-0.05 times the mass of the aluminum block into small particles and wrapping them in aluminum foil, pressing them into the melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 50-60 minutes, performing high-energy intermittent ultrasonic treatment, reducing the melt temperature to 690-710°C, refining the melt, removing slag, and pouring them into a metal mold to obtain aluminum rare earth Binary master alloy; preheating a graphite crucible to 380-420° C. in a pit-type resistance furnace, placing a high-entropy alloy particle-modified aluminum alloy in the crucible and heating it until it is completely melted, crushing an aluminum-rare earth binary master alloy of 0.10-0.12 times the mass of the high-entropy alloy particle-modified aluminum alloy into small particles with a particle size of 0.1-0.2 mm and wrapping them in aluminum foil, pressing them into the alloy melt with a bell jar, stirring them fully after they are completely melted and keeping them warm for 50-60 minutes to ensure that they are fully metamorphosed, lowering the melt temperature to 690-710° C., refining and deslagging the melt, and pouring them into a metal mold to obtain a rare earth-doped aluminum alloy; (3) The rare earth doped aluminum alloy was immersed in a sodium hydroxide aqueous solution with a mass fraction of 20% to 24%, ultrasonically treated for 5 to 7 minutes, taken out, washed with deionized water for 3 to 5 times, immersed in a silane hydrolyzate solution, ultrasonically treated for 3 to 4 hours, taken out, and kept at 140 to 150°C for 2 to 3 hours to obtain a silane surface treated aluminum alloy; the silane surface treated aluminum alloy was immersed in an 8-hydroxyquinoline reaction solution, ultrasonically treated at 50 to 60°C for 3 to 4 hours, taken out, washed with anhydrous ethanol and deionized water for 3 to 5 times respectively, and dried at 5 to 7 Pa and 50 to 60°C for 4 to 6 hours to obtain a rare earth modified aluminum alloy.

2. The method for preparing a rare earth modified aluminum alloy according to claim 1, characterized in that: The process control agent in step (1) is one of anhydrous ethanol, cyclohexane, n-hexane, n-heptane and toluene.

3. The method for preparing a rare earth modified aluminum alloy according to claim 1, characterized in that: The specific operation process of the high-energy intermittent ultrasonic treatment in step (2) is as follows: the ultrasonic output frequency is 1.5 KHz, the ultrasonic time is 20 to 30 minutes, the high-energy ultrasonic application time is 70 to 80 seconds each time, and the intermittent time is 70 to 80 seconds.

4. The method for preparing a rare earth modified aluminum alloy according to claim 1, characterized in that: The silane hydrolyzate in step (3) is prepared by uniformly mixing 3-aminopropyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, anhydrous ethanol and deionized water in a mass ratio of 1:(1.3-1.5):(2.2-2.5):(8-10), and adjusting the pH to 4.8-5.0 with a 10%-12% mass fraction hydrochloric acid aqueous solution.

5. The method for preparing a rare earth modified aluminum alloy according to claim 1, characterized in that: The 8-hydroxyquinoline reaction solution in step (3) is prepared by uniformly mixing 5-chloromethyl-8-hydroxyquinoline hydrochloride, triethylamine, and N-methylpyrrolidone in a mass ratio of 1:(0.01-0.03):(8-10).