A diaphragm for alkaline hydrolysis tank and preparation method thereof

Through the porous metal oxide structure and organic filler conditioning technology, the problems of loose adhesion and large pollution of the alkaline water electrolyzer separator are solved, achieving high strength, low surface resistance and excellent gas barrier properties, and extending the service life. And improve the gas purity and corrosion resistance.

CN118390110BActive Publication Date: 2024-10-29NORTH CHINA ELECTRIC POWER UNIV

Patent Information

Application Number
CN202410514294.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-10-29
Estimated Expiration
2044-04-26

AI Technical Summary

Technical Problem

The existing alkaline water electrolyzer separators have problems such as insufficient adhesion, high pollution, and poor durability. In particular, the PPS separator is highly polluted during the sulfonation modification process, and the composite separator is not tightly adhered, making it difficult to meet the requirements. Demand for higher strength and lower surface resistance.

Method used

Using a porous metal oxide structure as the separator, through inorganic skeleton molding and organic filler infiltration phase transformation, a separator with zirconium oxide or titanium dioxide as the main component is prepared, which has high wet tensile strength and excellent gas barrier properties, and is passed Organic fillers adjust the pore structure to improve the performance of the separator.

Benefits of technology

It achieves high wet tensile strength, low surface resistance and excellent gas barrier properties of the diaphragm, prolongs the service life of the diaphragm, and improves the purity of gas production and corrosion resistance during alkaline hydrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118390110B_ABST
    Figure CN118390110B_ABST
Patent Text Reader

Abstract

The present invention discloses a diaphragm for an alkaline hydrolysis tank and a preparation method thereof, wherein the diaphragm is a porous metal oxide structure, wherein the porosity is 30-38%, the average pore size of the pores is 1-5 μm, the thickness of the diaphragm is 300-350 μm, and the metal oxide structure comprises at least one of zirconium oxide and titanium dioxide. In the preparation method, an inorganic skeleton is first obtained by molding and sintering a mixture containing an inorganic raw material, and then an organic filler is infiltrated into the inorganic skeleton, and then a diaphragm of an alkaline hydrolysis tank is obtained by phase conversion. The diaphragm for an alkaline hydrolysis tank provided by the present invention has high wet tensile strength, adopts an organic filler to adjust the pore structure, has excellent gas barrier properties, and has high erosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen production by hydrolysis, and particularly relates to a diaphragm for an alkaline hydrolysis tank and a preparation method thereof. Background Art

[0002] At present, the mainstream methods of hydrogen production include proton exchange membrane water electrolysis, anion exchange membrane water electrolysis, solar photolysis water electrolysis and alkaline water electrolysis. After long-term development and practical verification, alkaline water electrolysis hydrogen production technology has taken a dominant position and has become a mature method. When alkaline water electrolysis hydrogen production is coupled with renewable energy (such as solar energy, wind energy, etc.), zero carbon emissions can be achieved in the hydrogen production process.

[0003] When alkaline water electrolysis hydrogen production technology is used to electrolyze alkaline solution, oxygen is produced at the anode and hydrogen is produced at the cathode. The function of the diaphragm is to prevent gas cross-talk, ensure the safety of the electrolysis process and improve the purity of the gas produced. Most existing alkaline water electrolyzers use PPS fabric as the diaphragm for water electrolysis, but the traditional PPS fabric diaphragm has poor hydrophilicity, large surface resistance and high bubble point pressure. In order to improve the safety and efficiency of water electrolysis, the current measures mainly include: sulfonation modification of PPS, composite of PPS with organic and inorganic materials, etc.

[0004] For example, patent CN111733602A provides a method for preparing a PPS / MOFs micro-nano fiber alkaline water electrolyzer diaphragm, 1) preparing a PPS melt-blown cloth through a melt-blown device for dried PPS resin; 2) modifying the PPS melt-blown cloth to be hydrophilic; 3) modifying the hydrophilic modified PPS melt-blown cloth with alkali-resistant hydrophilic MOFs; 4) hot-pressing the MOFs-modified PPS melt-blown cloth, and rapidly cooling it to obtain a PPS / MOFs micro-nano fiber alkaline water electrolyzer diaphragm. This scheme adopts the method of modifying the hydrophilic ZIF-90, which not only improves its hydrophilicity and alkali absorption rate, but also because the three-dimensional pore structure of the MOFs materials possessed by ZIF-90 can effectively prevent the penetration of gas molecules, ensuring that the gases generated by the two electrodes during the electrolysis of water will not penetrate and mix with each other, thereby ensuring the purity of the gas.

[0005] For example, patent CN116770362A provides a composite diaphragm and its preparation method and electrochemical energy device. The preparation method includes: S1. Dissolving a binder and a pore former in an organic solvent to obtain a homogeneous solution; S2. Adding a filler to the homogeneous solution in step S1 to obtain a precursor slurry; S3. Applying the precursor slurry in step S2 on a support fabric, and then vertically placing it in a coagulation bath for phase inversion treatment to obtain a composite diaphragm. This preparation method uses a simple casting method and can be prepared at room temperature. It is low-cost, easy to make, and easy to scale up. In addition, the phase inversion diaphragm is prepared by vertical immersion in a coagulation bath. The surface of the obtained diaphragm does not require additional polymer layer modification, thereby increasing the hydrophilicity of the diaphragm and reducing the surface resistance. The diaphragm has excellent gas barrier properties and low surface resistance.

[0006] However, the sulfonation modification of PPS is more polluting, and the PPS composite diaphragm is not tightly bonded. Therefore, it is necessary to explore a more durable alkaline water electrolysis diaphragm with less pollution in the production process.

[0007] Therefore, exploring and developing alkaline water electrolyzer diaphragms with higher strength, lower surface resistance and simpler process is an urgent problem to be solved by technicians in this field. Summary of the invention

[0008] In view of the defects existing in the above-mentioned prior art, the present invention provides a diaphragm for an alkaline hydrolysis tank and a preparation method thereof. The diaphragm is a porous metal oxide structure, the average pore size of the pores is 1-5 μm, the thickness of the diaphragm is 300-350 μm, and the metal oxide structure contains at least one of zirconium oxide and titanium dioxide. In the preparation method, a mixture containing inorganic raw materials is first formed and sintered to obtain an inorganic skeleton, and then an organic filler is infiltrated into the inorganic skeleton, and then a phase transformation is performed to obtain a diaphragm for an alkaline hydrolysis tank. The diaphragm for an alkaline hydrolysis tank provided by the present invention has high wet tensile strength, adopts organic fillers to adjust the pore structure, has excellent gas barrier properties, and has high erosion resistance.

[0009] In a first aspect, the present invention provides a diaphragm for an alkaline hydrolysis cell, wherein the diaphragm is a porous metal oxide structure with a porosity of 30-38%, an average pore size of 1-5 μm, a diaphragm thickness of 300-350 μm, and the metal oxide structure comprises at least one of zirconium oxide and titanium dioxide.

[0010] Furthermore, the wet tensile strength of the separator is not less than 30 MPa.

[0011] Furthermore, the bubble point pressure of the diaphragm is not less than 0.4Mpa, and the surface resistance is not greater than 0.4Ω·cm 2 .

[0012] In a second aspect, the present invention further provides a method for preparing the above-mentioned diaphragm for an alkaline hydrolysis tank, comprising the following steps:

[0013] S1: dry pressing or tape casting a mixture containing inorganic raw materials to obtain a sheet, and sintering the sheet to prepare a porous inorganic skeleton;

[0014] S2: adding a binder and a pore-forming agent to an organic solvent, stirring at a constant temperature, and preparing an organic filler solution;

[0015] S3: In a vacuum dry environment, the organic filler is infiltrated into the inorganic skeleton, and then undergoes phase transformation to obtain a diaphragm for an alkaline hydrolysis cell.

[0016] Furthermore, step S1 specifically includes the following steps:

[0017] S11: mixing the inorganic raw material, graphite and ethanol to form a first mixture;

[0018] S12: ball milling the first mixture for a ball milling time of not less than 10 hours, and drying the mixture after ball milling to obtain a ball milling product;

[0019] S13: adding polyvinyl butyral and ethanol to the ball-milled product, grinding until the ethanol is completely volatilized to obtain fine powder;

[0020] S14: The fine powder is placed in a mold, and cold pressed into a sheet at a pressure of 10-15 MPa. The sheet is sintered, and then wet-milled to obtain an inorganic skeleton.

[0021] Furthermore, step S1 specifically includes the following steps:

[0022] S11: mixing the inorganic raw material with graphite, ethanol, xylene, fish oil, butyl benzyl phthalate, aqueous polyalkylene glycol, and polyvinyl butyral to form a second mixture;

[0023] S12: putting the second mixture into a pot mill for pot milling to obtain a uniformly mixed slurry, wherein the rotation speed of the pot mill is 350-400 r / min, and the pot milling time is not less than 24 hours;

[0024] S13: pouring the slurry onto the film-casting belt of the film-casting machine to cast the raw material, wherein the film-casting belt has a running speed of 0.2-0.4 r / s and a knife height of 350-400 μm;

[0025] S14: peeling the raw material and cutting it into pieces to obtain a sheet;

[0026] S15: Sintering the flakes and then wet grinding them to obtain an inorganic skeleton.

[0027] Further, in step S1, the inorganic raw material is at least one of YSZ or titanium dioxide;

[0028] The sheet is sintered, specifically comprising: firstly heating to 400-450°C and keeping the temperature for 4-6 hours, then heating to 1400-1600°C and keeping the temperature for 2-3 hours, and the thickness of the sheet after sintering is 300-350 μm.

[0029] Further, in step S2, the adhesive is polysulfone, the pore-forming agent is polyvinyl pyrrolidone, the organic solvent is N-methyl-2-pyrrolidone, and the mass ratio of the adhesive, the pore-forming agent and the organic solvent is 1:(0.2-0.5):(5-10);

[0030] Constant temperature stirring specifically includes: temperature of 40-45°C, stirring speed of 2500-2800r / min, and stirring time of not less than 3h.

[0031] Further, step S3 specifically includes the following steps:

[0032] S31: placing the inorganic framework obtained in step S1 into a culture dish, and pouring the organic filler solution obtained in step S2 into the dish, so that the inorganic framework is completely immersed in the organic filler solution;

[0033] S32: placing the culture dish in a vacuum drying oven for vacuum drying to obtain an inorganic skeleton infiltrated with an organic filler, wherein the vacuum degree is not greater than 0.02 MPa, the vacuum drying temperature is 40-50° C., and the time is 30-40 min;

[0034] S33: taking out the inorganic skeleton infiltrated with the organic filler, immersing it in deionized water, performing a phase conversion between water and the organic solvent, and then putting it in an oven for drying to obtain a diaphragm for an alkaline hydrolysis tank.

[0035] Furthermore, in step S33, the phase conversion time between water and organic solvent is 10 minutes, and the temperature of oven drying is 80° C. and the time is 30 minutes.

[0036] The present invention provides a diaphragm for an alkaline hydrolysis tank and a preparation method thereof, which at least have the following beneficial effects:

[0037] (1) The diaphragm for alkaline hydrolysis tank provided by the present invention has high wet tensile strength, adopts organic filler to adjust the pore structure, has excellent gas barrier property, has high erosion resistance, and has a longer service life.

[0038] (2) The present invention improves the overall bubble point pressure of the diaphragm through the pore structure after conditioning with organic fillers, which can inhibit gas crosstalk during the use of the diaphragm and improve the purity of gas produced during alkaline hydrolysis.

[0039] (3) The diaphragm provided by the present invention is a metal oxide structure. Compared with the PPS mesh composite diaphragm, it has better mechanical properties and can prevent damage caused by stress during use. It also has better corrosion resistance, especially improving the corrosion resistance of the diaphragm when it contacts the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A surface microscopic morphology image of the diaphragm of the alkaline hydrolysis tank of Example 1 provided by the present invention;

[0041] Figure 2 This is a cross-sectional microscopic morphology diagram of the diaphragm of the alkaline hydrolysis tank of Example 1 provided by the present invention. DETAILED DESCRIPTION

[0042] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings, and "multiple" generally includes at least two.

[0044] It should also be noted that the term "includes", "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, so that a commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprising a ..." do not exclude the existence of other identical elements in the commodity or device including the elements.

[0045] The current composite diaphragms made of PPS fabric generally have problems such as insufficient adhesion and low durability. Others, such as Zirfon membrane, have porous structural characteristics, and their pore morphology is similar to that of pure polysulfone membrane. In terms of microstructure, its surface presents a dense epidermis layer, and a unique finger-like pore network is constructed inside, which makes it have good ion conductivity and can operate stably for a long time in alkaline water electrolyzers. However, one of the shortcomings of this membrane is that its strength needs to be improved.

[0046] To this end, the present invention explores and develops an alkaline water electrolyzer diaphragm with higher strength, lower surface resistance and simpler process, and provides a diaphragm with a porous metal oxide structure. Specifically:

[0047] In a first aspect, the present invention provides a diaphragm for an alkaline hydrolysis cell, wherein the diaphragm is a porous metal oxide structure with a porosity of 30-38%, an average pore size of 1-5 μm, a diaphragm thickness of 300-350 μm, and the metal oxide structure comprises at least one of zirconium oxide and titanium dioxide.

[0048] Furthermore, the wet tensile strength of the separator is not less than 30 MPa.

[0049] Furthermore, the bubble point pressure of the diaphragm is not less than 0.4Mpa, and the surface resistance is not greater than 0.4Ω·cm 2 .

[0050] In a second aspect, the present invention further provides a method for preparing the above-mentioned diaphragm for an alkaline hydrolysis tank, comprising the following steps:

[0051] S1: dry pressing or tape casting a mixture containing inorganic raw materials to obtain a sheet, and sintering the sheet to prepare a porous inorganic skeleton;

[0052] S2: adding a binder and a pore-forming agent to an organic solvent, stirring at a constant temperature, and preparing an organic filler solution;

[0053] S3: In a vacuum dry environment, the organic filler is infiltrated into the inorganic skeleton, and then undergoes phase transformation to obtain a diaphragm for an alkaline hydrolysis cell.

[0054] Furthermore, step S1 specifically includes the following steps:

[0055] S11: mixing the inorganic raw material, graphite and ethanol to form a first mixture;

[0056] S12: ball milling the first mixture for a ball milling time of not less than 10 hours, and drying the mixture after ball milling to obtain a ball milling product;

[0057] S13: adding PVB (polyvinyl butyral) and ethanol to the ball-milled product, grinding until the ethanol is completely volatilized to obtain fine powder;

[0058] S14: The fine powder is placed in a mold, and cold pressed into a sheet at a pressure of 10-15 MPa. The sheet is sintered, and then wet-milled to obtain an inorganic skeleton.

[0059] Furthermore, step S1 specifically includes the following steps:

[0060] S11: mixing the inorganic raw material with graphite, ethanol, xylene, fish oil, BBP (butyl benzyl phthalate), PAG (aqueous polyalkylene glycol), and PVB (polyvinyl butyral) to form a second mixture;

[0061] S12: putting the second mixture into a pot mill for pot milling to obtain a uniformly mixed slurry, wherein the rotation speed of the pot mill is 350-400 r / min, and the pot milling time is not less than 24 hours;

[0062] S13: pouring the slurry onto the film-casting belt of the film-casting machine to cast the raw material, wherein the film-casting belt has a running speed of 0.2-0.4 r / s and a knife height of 350-400 μm;

[0063] S14: peeling the raw material and cutting it into pieces to obtain a sheet;

[0064] S15: Sintering the flakes and then wet grinding them to obtain an inorganic skeleton.

[0065] Further, in step S1, the inorganic raw material is at least one of YSZ or titanium dioxide;

[0066] The sheet is sintered, specifically comprising: firstly heating to 400-450°C and keeping the temperature for 4-6 hours, then heating to 1400-1600°C and keeping the temperature for 2-3 hours, and the thickness of the sheet after sintering is 300-350 μm.

[0067] Further, in step S2, the adhesive is PSU (polysulfone), the pore-forming agent is PVP (polyvinyl pyrrolidone), the organic solvent is NMP (N-methyl-2-pyrrolidone), and the mass ratio of the adhesive, the pore-forming agent and the organic solvent is 1: (0.2-0.5): (5-10);

[0068] Constant temperature stirring specifically includes: temperature of 40-45°C, stirring speed of 2500-2800r / min, and stirring time of not less than 3h.

[0069] Further, step S3 specifically includes the following steps:

[0070] S31: placing the inorganic framework obtained in step S1 into a culture dish, and pouring the organic filler solution obtained in step S2 into the dish, so that the inorganic framework is completely immersed in the organic filler solution;

[0071] S32: placing the culture dish in a vacuum drying oven for vacuum drying to obtain an inorganic skeleton infiltrated with an organic filler, wherein the vacuum degree is not greater than 0.02 MPa, the vacuum drying temperature is 40-50° C., and the time is 30-40 min;

[0072] S33: taking out the inorganic skeleton infiltrated with the organic filler, immersing it in deionized water, performing a phase conversion between water and the organic solvent, and then putting it in an oven for drying to obtain a diaphragm for an alkaline hydrolysis tank.

[0073] Furthermore, in step S33, the phase conversion time between water and organic solvent is not less than 10 minutes, and the temperature of oven drying is 80-100° C., and the time is not less than 30 minutes.

[0074] Example 1

[0075] Example 1: Preparation of a diaphragm for an alkaline hydrolysis tank with zirconium oxide as the skeleton.

[0076] In Example 1, the specific steps for preparing the diaphragm for the alkaline hydrolysis tank are as follows:

[0077] S1: dry-press or tape-cast the mixture containing inorganic raw materials to obtain a sheet, sinter the sheet, and prepare a porous inorganic skeleton. S11: mix YSZ (yttria-stabilized zirconia) with graphite and ethanol to form a first mixture; S12: ball-mill the first mixture for no less than 10 hours, dry it after ball-milling, and obtain a ball-milled product; S13: add PVB and ethanol to the ball-milled product, grind it until the ethanol is completely volatilized, and obtain a fine powder; S14: put the fine powder into a mold, cold-press it into a sheet at a pressure of 10MPa, sinter the sheet, and then wet-mill it to obtain an inorganic skeleton. When sintering the sheet, first heat it to 400℃ and keep it for 5 hours, then heat it to 1400℃ and keep it for 3 hours, and the thickness of the sheet after sintering is 300μm.

[0078] S2: Adding a binder and a pore former into an organic solvent and stirring at a constant temperature to prepare an organic filler solution. The binder is PSU, the pore former is PVP, the organic solvent is NMP, and the mass ratio of the binder, the pore former and the organic solvent is 1:0.26:7.06; stirring at a constant temperature, specifically including: a temperature of 40°C, a stirring speed of 2500r / min, and a stirring time of 3h.

[0079] S3: In a vacuum drying environment, the organic filler is infiltrated into the inorganic skeleton, and then phase conversion is performed to obtain a diaphragm for an alkaline hydrolysis tank. S31: The inorganic skeleton obtained in step S1 is placed in a culture dish, and the organic filler solution obtained in step S2 is poured in, so that the inorganic skeleton is completely immersed in the organic filler solution; S32: The culture dish is placed in a vacuum drying oven for vacuum drying to obtain an inorganic skeleton infiltrated with organic fillers, wherein the vacuum degree is 0.02MPa, the vacuum drying temperature is 40°C, and the time is 30min; S33: Take out the inorganic skeleton infiltrated with organic fillers, immerse it in deionized water, perform a phase conversion between water and organic solvent, and then place it in an oven for drying to obtain a diaphragm for an alkaline hydrolysis tank. The phase conversion time between water and organic solvent is 10min, and the oven drying temperature is 80°C for 30min.

[0080] The diaphragm of the alkaline hydrolysis tank prepared in this embodiment has a porous zirconium oxide structure (such as Figure 1-2 As shown), the porosity is about 35%, the average pore size is about 3 μm, and the membrane thickness is about 300 μm.

[0081] The wet tensile strength of the diaphragm is 43.24MPa, the bubble point pressure is 0.53MPa, and the surface resistance is 0.25Ω·cm 2 .

[0082] Example 2

[0083] Example 2 Preparation of a diaphragm for an alkaline hydrolysis tank with titanium dioxide as the skeleton.

[0084] Based on Example 1, Example 2 adjusts the following parameters.

[0085] Compared with the preparation process of Example 1, S11 in this embodiment:

[0086] Titanium dioxide is mixed with graphite and ethanol to form a first mixture.

[0087] The diaphragm of the alkaline hydrolysis tank prepared in this embodiment has a structure of porous titanium dioxide, a porosity of about 35%, an average pore diameter of about 2 μm, and a diaphragm thickness of about 330 μm.

[0088] The wet tensile strength of the diaphragm is 37.81MPa, the bubble point pressure is 0.47MPa, and the surface resistance is 0.36Ω·cm 2 .

[0089] Example 3

[0090] Example 3: Preparation of a diaphragm for an alkaline hydrolysis tank with zirconium oxide as the skeleton.

[0091] Based on Example 1, Example 3 adjusts the following parameters.

[0092] Compared with the preparation process of Example 1, S2 in this example:

[0093] S2: Adding a binder and a pore former into an organic solvent and stirring at a constant temperature to prepare an organic filler solution. The binder is PSU, the pore former is PVP, the organic solvent is NMP, and the mass ratio of the binder, the pore former to the organic solvent is 1:0.5:10;

[0094] The constant temperature stirring specifically includes: the temperature is 40° C., the stirring speed is 2500 r / min, and the stirring time is 3 h.

[0095] The diaphragm of the alkaline hydrolysis cell prepared in this embodiment has a structure of porous zirconium oxide, an average pore diameter of about 5 μm, and a thickness of about 350 μm.

[0096] The wet tensile strength of the diaphragm is 39.56MPa, the bubble point pressure is 0.43MPa, and the surface resistance is 0.31Ω·cm 2 .

[0097] Example 4

[0098] Example 4: Preparation of a diaphragm for an alkaline hydrolysis tank with zirconium oxide as the skeleton.

[0099] Based on Example 1, Example 4 adjusts the following parameters.

[0100] Compared with the preparation process of Example 1, S1 in this example:

[0101] Step S1 specifically includes the following steps:

[0102] S11: mixing an inorganic raw material with graphite, ethanol, xylene, fish oil, butyl benzyl phthalate, aqueous polyalkylene glycol, and polyvinyl butyral to form a second mixture; the inorganic raw material is YSZ;

[0103] S12: putting the second mixture into a pot mill for pot milling to obtain a uniformly mixed slurry, wherein the rotation speed of the pot mill is 350 r / min, and the pot milling time is not less than 24 hours;

[0104] S13: pouring the slurry onto the film-casting belt of the film-casting machine to cast the raw material, wherein the film-casting belt has a running speed of 0.3 r / s and a knife height of 350 μm;

[0105] S14: peeling the raw material and cutting it into pieces to obtain a sheet;

[0106] S15: Sintering the sheet, and then wet grinding to obtain an inorganic skeleton. When sintering the sheet, first heat it to 400°C and keep it for 5 hours, then heat it to 1400°C and keep it for 3 hours. The thickness of the sheet after sintering is 300 μm.

[0107] The diaphragm of the alkaline hydrolysis tank prepared in this embodiment has a porous zirconium oxide structure, a porosity of about 35%, an average pore diameter of about 3 μm, and a diaphragm thickness of about 300 μm.

[0108] The wet tensile strength of the diaphragm is 42.12MPa, the bubble point pressure is 0.51MPa, and the surface resistance is 0.27Ω·cm 2 .

[0109] Example 5

[0110] Example 5: Preparation of a diaphragm for an alkaline hydrolysis tank with zirconium oxide as the skeleton.

[0111] Based on Example 1, Example 5 adjusts the following parameters.

[0112] Compared with the preparation process of Example 1, in S1 of this embodiment:

[0113] The sheet is sintered, specifically including: first heating to 450° C. and keeping the temperature for 4 hours, then heating to 1600° C. and keeping the temperature for 2 hours. The thickness of the sheet after sintering is 300 μm.

[0114] The diaphragm of the alkaline hydrolysis cell prepared in this embodiment has a porous zirconium oxide structure, an average pore diameter of about 3 μm, and a diaphragm thickness of about 300 μm.

[0115] The wet tensile strength of the diaphragm is 37.61MPa, the bubble point pressure is 0.49MPa, and the surface resistance is 0.29Ω·cm 2 .

[0116] Comparative Example 1

[0117] Comparative Example 1 A composite diaphragm is prepared. The preparation method is as follows:

[0118] Step 1: PVP and PSU (molecular weight 80,000) in a mass ratio of 1:2 were weighed and dissolved in 20 mL of NMP solvent, and mechanically stirred at 300 rpm for 12 h at room temperature to form a homogeneous solution.

[0119] Step 2: Weigh a certain amount of nano ZrO with a particle size of 100 nm 2 The powder is added to the homogeneous solution obtained in step 1, and the PSU and nano ZrO 2The mass ratio was 1:4, and mechanical stirring was performed at 150 rpm at room temperature for 12 h, and then the mixture was allowed to stand for degassing to form a milky white precursor slurry.

[0120] Step 3: Pour the slurry onto a homemade slit coater with a slit width of 500 μm, use a 60-mesh PPS fabric to pass through the slit and evenly coat a layer of slurry, then place it vertically in an anhydrous ethanol coagulation bath for 30 minutes.

[0121] Step 4: Take the PPS mesh out of the coagulation bath and dry it under natural conditions to obtain a porous composite diaphragm.

[0122] The composite diaphragm prepared in this comparative example is a PPS mesh with ZrO 2 The structure of the coating, the average pore size of the coating is 136nm, and the surface resistance is 0.2456Ω·cm 2 .

[0123] Comparative Example 2

[0124] Comparative Example 2: Preparation of an inorganic framework of zirconium oxide.

[0125] Based on Example 1, the following parameters were adjusted in Comparative Example 2.

[0126] Compared with the preparation process of Example 1, steps S2 and S3 are omitted in this comparative example.

[0127] In this comparative example, an inorganic framework of zirconium oxide was prepared, and the porosity was greater than 40%.

[0128] The wet tensile strength of the inorganic skeleton of zirconia is 20.17MPa, the bubble point pressure is 0.27MPa, and the surface resistance is 0.26Ω·cm 2 .

[0129] Comparative Example 3

[0130] Comparative Example 3: A diaphragm for an alkaline hydrolysis tank with zirconium oxide as a skeleton is prepared.

[0131] Based on Example 1, the following parameters were adjusted in Comparative Example 3.

[0132] Compared with the preparation process of Example 1, S2 in this comparative example:

[0133] S2: Adding a binder and a pore former into an organic solvent and stirring at a constant temperature to prepare an organic filler solution. The binder is PSU, the pore former is PVP, the organic solvent is NMP, and the mass ratio of the binder, the pore former and the organic solvent is 1:0.15:4.5; stirring at a constant temperature, specifically including: a temperature of 40°C, a stirring speed of 2500r / min, and a stirring time of 3h.

[0134] The diaphragm of the alkaline hydrolysis tank prepared in this embodiment has a porous zirconium oxide structure, a porosity slightly greater than 40%, an average pore diameter of about 3 μm, and a diaphragm thickness of about 300 μm.

[0135] The wet tensile strength of the diaphragm is 43.24MPa, the bubble point pressure is 0.53MPa, and the surface resistance is 0.25Ω·cm 2 .

[0136] Comparative Example 4

[0137] Comparative Example 4: A diaphragm for an alkaline hydrolysis tank with zirconium oxide as a skeleton is prepared.

[0138] Based on Example 1, the following parameters were adjusted in Comparative Example 4.

[0139] Compared with the preparation process of Example 1, S32 in this comparative example:

[0140] The culture dish was placed in a vacuum drying oven for vacuum drying to obtain an inorganic skeleton infiltrated with organic fillers, wherein the vacuum degree was no greater than 0.02 MPa, the vacuum drying temperature was 30° C., and the time was 20 min.

[0141] The diaphragm of the alkaline hydrolysis cell prepared in this embodiment has a porous zirconium oxide structure, an average pore diameter of about 1 μm, and a diaphragm thickness of about 300 μm.

[0142] The wet tensile strength of the diaphragm is 28.87MPa, the bubble point pressure is 0.41MPa, and the surface resistance is 0.38Ω·cm 2 .

[0143] Performance Test:

[0144] The samples obtained in the above examples and comparative examples were tested for bubble point pressure, surface resistance and wet tensile strength. The specific test conditions and steps are as follows:

[0145] Bubble point pressure: The test of bubble point pressure refers to GB / T 32361-2015 "Test method for pore size of separation membranes - Bubble point and average flow method".

[0146] Surface resistance and wet tensile strength: The tests of surface resistance and wet tensile strength refer to SJ / T 10171-2016 "General test method for basic properties of alkaline battery separators", and the tests are carried out according to the test items of wet tensile strength in Chapter 4.7 and area resistance (surface resistance) in Chapter 4.8 respectively.

[0147] Table 1 Performance comparison table of embodiments and comparative examples

[0148]

[0149]

[0150] The data in Table 1 include the test results of bubble point pressure, wet tensile strength and surface resistance of the diaphragms for alkaline hydrolysis tanks prepared in various embodiments and comparative examples of the present invention.

[0151] Among them, from the perspective of bubble point pressure, the bubble point pressures of the membranes of Examples 1 to 5 are all greater than 0.4 MPa, and the bubble point pressure of the composite membrane of Comparative Example 1 is also greater than 0.4 MPa, but the bubble point pressures of the membranes / inorganic skeletons of Comparative Examples 2 to 4, which are adjusted on the basis of Example 1, are all less than 0.4 MPa. Among them, the bubble point pressure of the inorganic skeleton is the smallest.

[0152] In the process of producing hydrogen by electrolysis of water, the higher the bubble point pressure of the diaphragm, the stronger its ability to block gas, so that it can better prevent the mixing of hydrogen and oxygen, avoid the generation of explosive gas, and ensure the safe operation of the electrolyzer. By comparing the embodiment with the comparative example, the diaphragm with a porous metal oxide structure provided by the present invention has a higher bubble point pressure, which can better prevent the mixing of hydrogen and oxygen and ensure the safe operation of the electrolyzer.

[0153] The mechanical properties of the membranes obtained in various embodiments and comparative examples were evaluated mainly by testing the wet tensile strength. The wet tensile strength of the membranes of Examples 1-5 was greater than 30 MPa, especially the wet tensile strength of the membrane of Example 1 was the highest, reaching 43.24 MPa. The wet tensile strength of the membranes / inorganic skeletons of Comparative Examples 2-4 was less than 30 MPa, especially the wet tensile strength of the inorganic skeleton in Comparative Example 2 was the lowest.

[0154] In general, a diaphragm with a higher porosity may have a lower tensile strength because the presence of pores reduces the actual bearing area of ​​the material. Through the tests of the above embodiments and comparative diaphragms, it can be shown that the wet tensile strength can be significantly improved by conditioning the pore structure of the inorganic skeleton by infiltration of organic fillers. The diaphragms provided in each embodiment of the present invention can meet the practical application requirements of the electrolytic cell in terms of wet tensile strength.

[0155] The lower the surface resistance of the diaphragm, the smaller the barrier to ion conduction, and the lower the internal resistance of the electrolyzer, which helps to improve the power density of hydrogen production by hydrolysis. From the various embodiments and comparative examples, the diaphragm with a porous metal oxide structure provided by the present invention is equivalent to the composite diaphragm. By comparing Example 1 and Comparative Examples 2-3, it can also be concluded that the ratio of the organic filler and the penetration of the organic filler on the inorganic skeleton will reduce the surface resistance of the diaphragm finally obtained.

[0156] The above test results show that the diaphragm for the alkaline hydrolysis tank prepared in each embodiment has excellent mechanical properties, excellent gas barrier properties, and better erosion resistance than the composite diaphragm.

[0157] The present invention provides a diaphragm for an alkaline hydrolysis tank and a preparation method thereof, which at least have the following beneficial effects:

[0158] (1) The diaphragm for alkaline hydrolysis tank provided by the present invention has high wet tensile strength, adopts organic filler to adjust the pore structure, has excellent gas barrier property, has high erosion resistance, and has a longer service life.

[0159] (2) The present invention improves the overall bubble point pressure of the diaphragm through the pore structure after conditioning with organic fillers, which can inhibit gas crosstalk during the use of the diaphragm and improve the purity of gas produced during alkaline hydrolysis.

[0160] (3) The diaphragm provided by the present invention is a metal oxide structure. Compared with the PPS mesh composite diaphragm, it has better mechanical properties and can prevent damage caused by stress during use. It also has better corrosion resistance, especially improving the corrosion resistance of the diaphragm when it contacts the electrolyte.

[0161] Although preferred embodiments of the present invention have been described, additional changes and modifications may be made to these embodiments by those skilled in the art once the basic inventive concepts are known. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a diaphragm for an alkaline hydrolysis tank, characterized in that: The diaphragm is a porous metal oxide structure with a porosity of 30-38%, an average pore size of 1-5 μm, a diaphragm thickness of 300-350 μm, and the metal oxide structure comprises at least one of zirconium oxide and titanium dioxide; The method comprises the following steps: S1: dry pressing or tape casting a mixture containing inorganic raw materials to obtain a sheet, and sintering the sheet to prepare a porous inorganic skeleton; S2: adding a binder and a pore-forming agent to an organic solvent, stirring at a constant temperature, and preparing an organic filler solution; S3: In a vacuum dry environment, the organic filler is infiltrated into the inorganic skeleton, and then undergoes phase transformation to obtain a diaphragm for an alkaline hydrolysis cell.

2. The method for preparing a diaphragm for an alkaline hydrolysis tank according to claim 1, characterized in that: The wet tensile strength of the diaphragm is not less than 30MPa.

3. The method for preparing a diaphragm for an alkaline hydrolysis tank according to claim 1, characterized in that: The bubble point pressure of the diaphragm is not less than 0.4MPa, and the surface resistance is not more than 0.4Ω·cm 2 .

4. The method for preparing a diaphragm for an alkaline hydrolysis tank according to claim 1, characterized in that: Step S1 specifically includes the following steps: S11: mixing the inorganic raw material, graphite and ethanol to form a first mixture; S12: ball milling the first mixture for a ball milling time of not less than 10 hours, and drying the mixture after ball milling to obtain a ball milling product; S13: adding polyvinyl butyral and ethanol to the ball-milled product, grinding until the ethanol is completely volatilized to obtain fine powder; S14: The fine powder is placed in a mold, and cold pressed into a sheet at a pressure of 10-15 MPa. The sheet is sintered, and then wet-grinded to obtain an inorganic skeleton.

5. The method for preparing a diaphragm for an alkaline hydrolysis tank according to claim 1, characterized in that: Step S1 specifically includes the following steps: S11: mixing the inorganic raw material with graphite, ethanol, xylene, fish oil, butyl benzyl phthalate, water-based polyalkylene glycol, and polyvinyl butyral to form a second mixture; S12: putting the second mixture into a pot mill for pot milling to obtain a uniformly mixed slurry, wherein the rotation speed of the pot mill is 350-400 r / min, and the pot milling time is not less than 24 hours; S13: pouring the slurry onto the film-casting belt of the film-casting machine to cast the raw material, wherein the film-casting belt has a running speed of 0.2-0.4 r / s and a knife height of 350-400 μm; S14: peeling the raw material and cutting it into pieces to obtain a sheet; S15: Sintering the flakes and then wet grinding them to obtain an inorganic skeleton.

6. The method for preparing a diaphragm for an alkaline hydrolysis tank according to claim 1, characterized in that: In step S1, the inorganic raw material is at least one of YSZ or titanium dioxide; The sheet is sintered, specifically comprising: firstly heating to 400-450°C and keeping the temperature for 4-6 hours, then heating to 1400-1600°C and keeping the temperature for 2-3 hours, and the thickness of the sheet after sintering is 300-350 μm.

7. The method for preparing a diaphragm for an alkaline hydrolysis tank according to claim 1, characterized in that: In step S2, the adhesive is polysulfone, the pore-forming agent is polyvinyl pyrrolidone, the organic solvent is N-methyl-2-pyrrolidone, and the mass ratio of the adhesive, the pore-forming agent and the organic solvent is 1:(0.2-0.5):(5-10); Constant temperature stirring specifically includes: temperature of 40-45°C, stirring speed of 2500-2800r / min, and stirring time of not less than 3h.

8. The method for preparing a diaphragm for an alkaline hydrolysis tank according to claim 1, characterized in that: Step S3 specifically includes the following steps: S31: placing the inorganic framework obtained in step S1 into a culture dish, and pouring the organic filler solution obtained in step S2 into the dish, so that the inorganic framework is completely immersed in the organic filler solution; S32: placing the culture dish in a vacuum drying oven for vacuum drying to obtain an inorganic skeleton infiltrated with an organic filler, wherein the vacuum degree is not greater than 0.02 MPa, the vacuum drying temperature is 40-50° C., and the time is 30-40 min; S33: taking out the inorganic skeleton infiltrated with the organic filler, immersing it in deionized water, performing a phase conversion between water and the organic solvent, and then putting it in an oven for drying to obtain a diaphragm for an alkaline hydrolysis tank.

9. The method for preparing a diaphragm for an alkaline hydrolysis tank according to claim 8, characterized in that: In step S33, the phase conversion time between water and organic solvent is not less than 10 minutes, and the oven drying temperature is 80-100° C. and the time is not less than 30 minutes.

Citation Information

Patent Citations

  • Diaphragm slurry, preparation method thereof and diaphragm for alkaline water electrolysis

    CN115693017A

Cited By

  • High-toughness composite diaphragm for hydrogen production from alkaline electrolyzed water and preparation method of high-toughness composite diaphragm

    CN121675018A