Positive electrode binder, positive electrode sheet and lithium ion battery
By designing a polymer structure containing cyano groups and ester groups, the solubility and lithium ion diffusion rate of the polyimide cathode binder are improved, solving the problems of poor solubility and high electrode impedance in the existing technology, and improving the lithium Cycling performance and thermal stability of ion batteries.
Patent Information
- Application Number
- CN202410842978.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The existing polyimide has poor solubility and high electrode impedance, which affects the cycle stability and overcharge safety of lithium-ion batteries.
Design a cathode binder, which includes a polymer. The polymer contains polyamideimide segments and side chain segments. The side chain segments contain repeating units containing cyano groups and optionally ester groups. By adjusting the molar Ratio and monomer selection to improve solubility and lithium ion diffusion rate in polar aprotic solvents.
It improves the solubility and lithium ion diffusion rate of the cathode binder in polar aprotic solvents, reduces electrode impedance, and improves the cycle performance and thermal stability of lithium-ion batteries.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a positive electrode binder, a positive electrode sheet and a lithium ion battery. Background Art
[0002] Lithium-ion batteries are widely used in various portable electronic devices, electric vehicles, energy storage systems and other fields due to their high energy density, long cycle life and environmental protection characteristics. Among them, electrode materials are one of the key factors affecting battery performance. As an important component of electrode materials, the performance of binders has an important influence on the electrochemical performance of batteries. Currently, the main commercial positive electrode binder is polyvinylidene fluoride (PVDF). PVDF has excellent performance in electrochemical stability, adhesion, lithium ion migration ability, etc., and can basically meet the needs of lithium-ion battery positive electrode binders. In addition, the high temperature performance of the PVDF system still needs to be improved.
[0003] Polyimide is a high-performance polymer material with excellent thermal stability, chemical stability and mechanical strength. Rationally designing the structure of polyimide adhesive as a binder in the positive electrode of lithium-ion batteries is of great significance for the development of polyimide batteries with high capacity, stable cycle performance and good safety performance. Chinese patent application CN114773599A discloses a block polyimide precursor adhesive as a lithium-ion battery adhesive, which takes into account both tensile strength and high temperature resistance. The battery prepared by the adhesive has better capacity retention and high temperature safety performance.
[0004] Traditional aromatic polyimide has poor solubility and usually exists as a product in the form of its precursor (polyamic acid, PAA). Its preparation process for pole pieces requires the addition of a high-temperature imidization step, which is incompatible with the existing pole piece manufacturing process. For soluble polyimide, fluorinated monomers are often used, which are expensive and not environmentally friendly, and have high electrode impedance. Therefore, how to enhance the solubility of polyimide lithium-based battery positive electrode binder in organic solvents, while enhancing ion transfer ability, reducing electrode impedance, maintaining thermal stability, and ensuring the cycle stability and overcharge safety of lithium-ion batteries is still a problem that needs to be solved urgently. Summary of the invention
[0005] The technical problem to be solved by the present invention is the poor solubility of existing polyimide and the high electrode impedance. The present invention provides a positive electrode binder, a positive electrode sheet and a lithium ion battery.
[0006] In order to solve the above technical problems, on the one hand, the present invention provides a positive electrode binder, which includes a polymer, the polymer includes a polyamideimide segment and a side chain segment connected to the polyamideimide segment as a side chain, the side chain segment is a polymer segment including a cyano-containing repeating unit, and the side chain segment also selectively includes an ester-containing repeating unit.
[0007] Preferably, the molar ratio of the cyano group-containing repeating unit to the ester group-containing repeating unit is (10-1):(0-9).
[0008] Preferably, the cyano group-containing repeating unit is selected from (meth)acrylonitrile monomer units; and the ester group-containing repeating unit is selected from (meth)acrylate monomer units.
[0009] Preferably, the polymer is formed by polymerization of a diacid monomer, an anhydride monomer and a diisocyanate monomer; the diacid monomer is a polymer monomer having at least one terminal diacid group; the polymer monomer includes a cyano group-containing repeating unit and optionally includes an ester group-containing repeating unit.
[0010] Preferably, the diacid monomer is formed by polymerizing a mercapto-containing dicarboxylic acid with a (meth)acrylonitrile monomer and a selectively added (meth)acrylate monomer.
[0011] Preferably, the molar ratio of the (meth)acrylonitrile monomer to the (meth)acrylate monomer is (10-1):(0-9); the ratio of the total molar number of the (meth)acrylonitrile monomer and the (meth)acrylate monomer to the molar number of the mercapto-containing dicarboxylic acid is 100:(1-10).
[0012] Preferably, the molar ratio of the diacid monomer to the anhydride monomer is (10-50):(50-90); the ratio of the total molar number of the diacid monomer and the anhydride monomer to the molar number of the diisocyanate monomer is (95-105):100.
[0013] Preferably, the (meth) acrylic acid ester monomers include one or more of methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-hexyl methacrylate, isooctyl methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, and isooctyl acrylate;
[0014] And / or, the acid anhydride monomer includes one or more of pyromellitic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropyldiphenyldiphenoxy)diphthalic anhydride, butanetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, p-phenylene di(trimellitic acid ester) dianhydride, and trimellitic acid anhydride;
[0015] And / or, the diisocyanate monomer includes one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate.
[0016] In a second aspect, the present application provides a positive electrode sheet, comprising a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode binder, and the positive electrode binder is the positive electrode binder described above or prepared by the preparation method of the positive electrode binder described above.
[0017] In a third aspect, the present application provides a lithium-ion battery, comprising a negative electrode sheet, a separator and the positive electrode sheet described above.
[0018] The positive electrode binder provided by the present application includes a polymer, the polymer includes a polyamide-imide segment and a side chain segment connected to the polyamide-imide segment as a side chain, the side chain segment is a polymer segment including a repeating unit containing a cyano group, and the side chain segment also selectively includes a repeating unit containing an ester group. The positive electrode binder with this structure has good solubility in polar aprotic solvents, and the polymer with this structure can generate a dipole interaction force with lithium ions, increase the lithium ion diffusion rate, reduce the electrode impedance, and improve its battery cycle performance; at the same time, the polymer has good thermal stability. DETAILED DESCRIPTION
[0019] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0020] On the one hand, an embodiment of the present application provides a positive electrode binder, which includes a polymer, wherein the polymer includes a polyamideimide segment and a side chain segment connected to the polyamideimide segment as a side chain, wherein the side chain segment is a polymer segment including a cyano-containing repeating unit, and the side chain segment also selectively includes an ester-containing repeating unit.
[0021] The positive electrode binder provided by the present application includes a polymer, the polymer includes a polyamide-imide segment and a side chain segment connected to the polyamide-imide segment as a side chain, the side chain segment is a polymer segment including a repeating unit containing a cyano group, and the side chain segment also selectively includes a repeating unit containing an ester group. The positive electrode binder with this structure has good solubility in polar aprotic solvents, and the polymer with this structure can generate a dipole interaction force with lithium ions, increase the lithium ion diffusion rate, reduce the electrode impedance, and improve its battery cycle performance; at the same time, the polymer has good thermal stability.
[0022] Specifically, the molar ratio of the cyano-containing repeating unit to the ester-containing repeating unit is (10-1): (0-9). The molar amount of the ester-containing repeating unit can be 0. The molar ratio of the cyano-containing repeating unit to the ester-containing repeating unit can be in the following ranges: (10-6): (0-4), (10-8): (0-2), (10-4): (0-6), (10-2): (0-8), etc. Preferably, the side chain segment contains both cyano-containing repeating units and ester-containing repeating units, wherein the molar number of the cyano-containing repeating unit is higher than the molar number of the ester-containing repeating unit. More preferably, the molar ratio of the cyano-containing repeating unit to the ester-containing repeating unit can be (9-6): (1-4), (8-7): (2-3). At this time, it is more beneficial to further reduce the electrode impedance.
[0023] Preferably, the cyano-containing repeating unit is selected from (meth)acrylonitrile monomer units, such as acrylonitrile monomer units.
[0024] The ester group-containing repeating unit is selected from (meth)acrylic acid ester monomer units.
[0025] It should be noted that the (meth)acrylonitrile monomer unit includes at least one of an acrylonitrile monomer unit and a methacrylonitrile monomer unit; and the (meth)acrylate monomer unit includes at least one of a methacrylate monomer unit and an acrylate monomer unit.
[0026] In some embodiments, the (meth)acrylate monomer units include one or more of methyl methacrylate monomer units, ethyl methacrylate monomer units, propyl methacrylate monomer units, isopropyl methacrylate monomer units, butyl methacrylate monomer units, isobutyl methacrylate monomer units, n-pentyl methacrylate monomer units, isopentyl methacrylate monomer units, n-hexyl methacrylate monomer units, isooctyl methacrylate monomer units, methyl acrylate monomer units, ethyl acrylate monomer units, propyl acrylate monomer units, butyl acrylate monomer units, pentyl acrylate monomer units, and isooctyl acrylate monomer units.
[0027] In some preferred embodiments, the (meth)acrylic acid ester monomer unit includes at least one of a butyl methacrylate monomer unit and an isobutyl methacrylate monomer unit.
[0028] Preferably, the polymer is formed by polymerization of a diacid monomer, an anhydride monomer and a diisocyanate monomer; the diacid monomer is a polymer monomer having at least one terminal diacid group; the polymer monomer includes a cyano group-containing repeating unit and optionally includes an ester group-containing repeating unit.
[0029] According to the present invention, preferably, the diacid monomer is formed by polymerizing a dicarboxylic acid containing a mercapto group with a (meth)acrylonitrile monomer and a selectively added (meth)acrylate monomer. The mercapto group in the dicarboxylic acid undergoes a mercaptoene addition reaction with the (meth)acrylonitrile monomer and / or the (meth)acrylate monomer, thereby obtaining a long-chain polymer monomer having at least one diacid group at its end.
[0030] The molar ratio of the (meth)acrylonitrile monomer to the (meth)acrylate monomer is (10-1): (0-9). As mentioned above, the molar amount of the (meth)acrylate monomer can be 0. The molar ratio of the (meth)acrylonitrile monomer to the (meth)acrylate monomer can be in the following ranges: (10-6): (0-4), (10-8): (0-2), (10-4): (0-6), (10-2): (0-8), etc. Preferably, the molar number of the (meth)acrylonitrile monomer is higher than the molar number of the (meth)acrylate monomer. More preferably, the molar ratio of the (meth)acrylonitrile monomer to the (meth)acrylate monomer can be (9-6): (1-4), (8-7): (2-3). At this time, it is more beneficial to further reduce the electrode impedance.
[0031] The ratio of the total mole number of the (meth)acrylonitrile monomer and the (meth)acrylate monomer to the mole number of the dicarboxylic acid containing a mercapto group is 100:(1-10). That is, the total mole number of the (meth)acrylonitrile monomer and the (meth)acrylate monomer is n1, the mole number of the dicarboxylic acid is n2, and n1:n2=100:(1-10).
[0032] When the ratio of the total molar number of the (meth) acrylonitrile monomer and the (meth) acrylic acid ester monomer to the molar number of the mercapto-containing dicarboxylic acid is 100: (1-10), the obtained diacid monomer has a suitable chain length. After the polymer provided by the present invention is prepared by the diacid monomer, the solubility of the positive electrode binder in a polar aprotic solvent can be effectively improved. If n1: n2 is lower than 100: (1-10), the chain segment of the diacid monomer is short, the effect of improving solubility decreases, and the effect of reducing electrode impedance also decreases. If n1: n2 is higher than 100: (1-10), the heat resistance and stability of the positive electrode binder deteriorate, the swelling of the positive electrode binder increases, and the cycle stability of the battery is affected. Preferably, the value of n1: n2 can be in the following range 100: (4-10), more preferably 100: (5-10), and further preferably 100: (6-9).
[0033] In the present invention, the mercapto-containing dicarboxylic acid may be a conventional substance known to those skilled in the art, for example, mercaptosuccinic acid. The (meth)acrylonitrile monomer may be acrylonitrile. The (meth)acrylic ester monomer includes one or more of methyl methacrylate monomer, ethyl methacrylate monomer, propyl methacrylate monomer, isopropyl methacrylate monomer, butyl methacrylate monomer, isobutyl methacrylate monomer, n-pentyl methacrylate monomer, isopentyl methacrylate monomer, n-hexyl methacrylate monomer, isooctyl methacrylate monomer, methyl acrylate monomer, ethyl acrylate monomer, propyl acrylate monomer, butyl acrylate monomer, pentyl acrylate monomer, and isooctyl acrylate monomer.
[0034] In some preferred embodiments, the (meth)acrylate monomer includes at least one of butyl methacrylate monomer and isobutyl methacrylate monomer.
[0035] Preferably, the molar ratio of the diacid monomer to the anhydride monomer is (10-50):(50-90); the ratio of the total molar number of the diacid monomer and the anhydride monomer to the molar number of the diisocyanate monomer is (95-105):100.
[0036] In some embodiments, the anhydride monomer includes one or more of pyromellitic acid dianhydride, 3,3',4,4'-diphenyl ether dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 4,4'-(4,4'-isopropyldiphenyldiphenoxy)diphthalic anhydride, butanetetracarboxylic acid dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic acid dianhydride, p-phenylene di(trimellitic acid ester) dianhydride, and trimellitic acid anhydride.
[0037] In some preferred embodiments, the anhydride monomer includes one or more of pyromellitic anhydride, 3,3',4,4'-diphenyl ketone tetracarboxylic anhydride, 4,4'-biphenyl ether dianhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, 4,4'-(4,4'-isopropyldiphenyldiphenoxy) diphthalic anhydride, and trimellitic anhydride.
[0038] In some embodiments, the diisocyanate monomer includes one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate.
[0039] In some preferred embodiments, the diisocyanate monomer includes one or more of toluene diisocyanate and diphenylmethane diisocyanate.
[0040] Specifically, the molar ratio of the diacid monomer to the anhydride monomer is in the range of (10-50): (50-90), which helps to improve the solubility of the positive electrode binder in aprotic polar solvents and improve the heat resistance, stability and mechanical properties of the positive electrode binder. If the added anhydride monomer is too low, the swelling of the prepared positive electrode binder increases, and the heat resistance, stability and mechanical properties deteriorate. If the added anhydride monomer is too high, the solubility of the positive electrode binder in aprotic polar solvents decreases.
[0041] The molar ratio of the total mole of the diacid monomer and the acid anhydride monomer to the diisocyanate monomer is (95-105):100. The diacid monomer with a long side chain is introduced, and the carboxyl group reacts with the isocyanate group to form an amide group, so that it has good solubility in polar aprotic solvents; at the same time, the positive electrode binder prepared by it can generate a dipole interaction force with lithium ions, thereby increasing the lithium ion diffusion rate, reducing the electrode impedance, and improving its battery cycle performance; it also makes the battery have good thermal stability.
[0042] The closer the molar ratio of the total molar amount of the diacid monomer and the anhydride monomer to the diisocyanate monomer is to 1:1, the longer the molecular chain is, the better the heat resistance, stability and mechanical properties of the prepared positive electrode binder are, the higher the solubility in non-protonic polar solvents is, and when used in lithium-ion batteries, the lithium ion diffusion rate is higher, reducing the electrode impedance.
[0043] If the molar ratio of the total mole of the diacid monomer and the acid anhydride monomer to the diisocyanate monomer is lower than (95-105):100, the content of the added diisocyanate monomer is too much, and the mixed solution formed by the diacid monomer, the acid anhydride monomer, the diisocyanate, and the second organic solvent produces gel, and the positive electrode binder cannot be prepared. If the molar ratio of the total mole of the diacid monomer and the acid anhydride monomer to the diisocyanate monomer is higher than (95-105):100, the content of the added diisocyanate monomer is too little, the viscosity of the prepared positive electrode binder is low, the generated main chain is short, and the positive electrode sheet obtained by coating the positive electrode slurry on the surface of the positive electrode collector is relatively brittle and easy to break.
[0044] Specifically, the molar ratio of the total molar ratio of the diacid monomer and the acid anhydride monomer to the diisocyanate monomer may be 95:100, 96:100, 97:100, 98:100, 99:100, 10:100, 101:100, 102:100, 103:100, 104:100 or 105:100, etc. As long as the molar ratio of the total molar ratio of the acid monomer and the acid anhydride monomer to the diisocyanate monomer is within the range of (95-105):100, it is acceptable.
[0045] In a second aspect, the present application provides a method for preparing the positive electrode binder described above, comprising the following steps:
[0046] Adding a dicarboxylic acid containing a mercapto group, a first monomer and an initiator into a first organic solvent to perform a telomerization reaction to obtain a diacid monomer containing a side chain;
[0047] The diacid monomer, the anhydride monomer and the diisocyanate monomer are subjected to a polycondensation reaction in a second organic solvent to obtain the positive electrode binder;
[0048] Specifically, the first monomer includes a (meth)acrylonitrile monomer and a selectively added (meth)acrylate monomer.
[0049] The method for preparing the positive electrode binder provided in the present application comprises adding the first monomer mentioned above to generate the diacid monomer when preparing the diacid monomer, and then reacting the diacid monomer with anhydride and diisocyanate monomer to prepare the positive electrode binder.
[0050] In some embodiments, the initiator includes at least one of azobisisobutyronitrile, azobisisoheptanenitrile, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, di-tert-butyl peroxide, and diisopropylbenzene peroxide.
[0051] In some preferred embodiments, the initiator includes at least one of azobisisobutyronitrile and azobisisoheptanenitrile; further preferably, the initiator is azobisisobutyronitrile.
[0052] In some embodiments, the first organic solvent includes one or more of tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, toluene, xylene, and dioxane.
[0053] In some embodiments, the second organic solvent includes one or more of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, toluene, and xylene.
[0054] In some preferred embodiments, the second organic solvent includes N-methylpyrrolidone.
[0055] In some embodiments, based on the total mass of the thiol-containing dicarboxylic acid and the first monomer being 100%, the mass proportion of the initiator is 0.1-0.5%.
[0056] Specifically, the initiator plays a role in initiating polymerization. If the amount of initiator added is too high, the preparation cost will increase, the chain will become shorter, and the by-products will increase. If the amount of initiator added is too little, the rate of initiation polymerization will decrease. The mass proportion of the initiator is in the range of 0.1~0.5%, which can play a role in initiating polymerization and generate diacid monomers containing long side chains, which helps to destroy the symmetry of polyimide and make the positive electrode binder have good solubility in polar aprotic solvents. The mass proportion of the initiator can be, for example, in the following ranges: 0.1~0.2%, 0.2~0.3%, 0.3~0.4%, and 0.4~0.5%.
[0057] In some embodiments, the diacid monomer, the anhydride monomer and the diisocyanate monomer are subjected to a condensation polymerization reaction in a second organic solvent, and the positive electrode binder is obtained after the reaction is completed, which comprises the following steps: dissolving the diacid monomer, the anhydride monomer and the diisocyanate monomer in the second organic solvent for a condensation polymerization reaction, and obtaining the positive electrode binder after the reaction is completed;
[0058] Adding the binder into the second organic solvent to dilute to form a positive electrode binder glue solution, wherein the solid content of the positive electrode binder glue solution is 8% to 40%;
[0059] Specifically, the solid content of the positive electrode binder paste is in the range of 8% to 40%, which refers to the solid content in the positive electrode binder; when the solid content is within the above range, a uniform and stable positive electrode binder paste can be obtained.
[0060] The solid content of the positive electrode binder glue can be 8%, 10%, 12%, 15%, 18%, 20%, 23%, 26%, 29%, 30%, 34%, 38%, 40%, etc., as long as the solid content is within the range of 8% to 40%.
[0061] In some preferred embodiments, the solid content of the positive electrode binder paste is 10% to 20%.
[0062] In some embodiments, the reaction temperature of the telomerization reaction is 40-100° C., and the reaction time of the telomerization reaction is 4-24 h;
[0063] And / or, the reaction temperature of the polycondensation reaction is 40-150° C., and the reaction time of the polycondensation reaction is 8-72 hours.
[0064] In a third aspect, the present application provides a positive electrode sheet, comprising a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode binder, and the positive electrode binder is the positive electrode binder described above or prepared by the preparation method of the positive electrode binder described above.
[0065] Specifically, the positive electrode sheet includes a positive electrode active material layer and a positive electrode current collector, the positive electrode current collector includes aluminum foil, carbon-coated aluminum foil, etc., and the positive electrode current collector is preferably aluminum foil. The positive electrode active material layer is obtained by coating the positive electrode slurry on the surface of the positive electrode current collector and drying it. The positive electrode slurry includes a positive electrode active material, a positive electrode conductive agent, a positive electrode binder and a third organic solvent. The positive electrode active material includes lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, etc. The positive electrode conductive agent includes conductive carbon black, carbon nanotubes, conductive graphite, carbon fiber, graphene, etc. The positive electrode binder is the positive electrode binder provided in this application, and the third organic solvent includes NMP.
[0066] The positive electrode sheet provided in the present application includes the positive electrode binder provided in the present application. During the preparation of the positive electrode slurry, the positive electrode binder can be well dissolved in the organic solvent NMP, the uniformity and stability of the prepared positive electrode slurry are increased, and the adhesion of the positive electrode sheet prepared by coating the positive electrode slurry on the surface of the positive electrode collector is enhanced.
[0067] In a fourth aspect, the present application provides a lithium-ion battery, comprising a negative electrode sheet, a separator and the positive electrode sheet described above.
[0068] Specifically, the lithium-ion battery includes a negative electrode sheet, a positive electrode sheet and a separator, and the separator is arranged between the positive electrode sheet and the negative electrode sheet. The positive electrode sheet is the positive electrode sheet described above, and the negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes graphite, silicon-based negative electrode, etc.
[0069] The lithium-ion battery provided by the present application includes the positive electrode binder provided by the present application, which contains cyano groups and can generate dipole interaction forces with lithium ions, thereby increasing the diffusion rate of lithium ions, reducing electrode impedance, and improving the battery cycle performance. At the same time, the positive electrode binder provided by the present application has good heat resistance, stability and mechanical properties, and can make the battery have good thermal stability.
[0070] The present invention is further described below by way of examples.
[0071] The positive electrode binder, positive electrode sheet and lithium ion battery disclosed in the present invention are specifically described.
[0072] Example 1
[0073] 1) Preparation of positive electrode binder
[0074] S1: 10 g of mercaptosuccinic acid, 50 g of acrylonitrile and 0.18 g of initiator azobisisobutyronitrile were dissolved in 140 g of the first organic solvent tetrahydrofuran, and a polyol reaction was carried out under a nitrogen atmosphere. The polyol reaction temperature was 60°C and the polyol reaction time was 24 hours. After the polyol reaction was completed, part of the first organic solvent tetrahydrofuran was removed by rotary evaporation, and then precipitated in methanol and vacuum dried at 40°C for 24 hours to obtain a diacid monomer containing a side chain, with a yield of 96.0%.
[0075] S2: 0.8 mol (257.8 g) of 3,3',4,4'-dibenzophenone tetraacid dianhydride (BTDA), 0.2 mol (180.2 g) of the diacid monomer containing a side chain obtained in step S1, 0.5 mol (87.1 g) of toluene diisocyanate (TDI), 0.5 mol (125.1 g) of diphenylmethane diisocyanate (MDI), and 2600 g of N-methylpyrrolidone (NMP) were added into a 10 L reactor for polycondensation reaction. The reaction was carried out at 40 ° C for 1 hour, and then the temperature was gradually increased to 120 ° C at a heating rate of 10 ° C per hour, and then the polycondensation reaction was carried out at 120 ° C for 8 hours. After the reaction, a positive electrode binder was obtained, and then NMP was added to the positive electrode binder to dilute it to a positive electrode binder glue with a solid content of 10%.
[0076] 2) Preparation of positive electrode:
[0077] Prepare positive electrode slurry: wherein the mass ratio of lithium nickel cobalt manganese oxide, conductive carbon black, conductive graphite, and the positive electrode binder prepared above is 97.8:0.3:0.7:1.2, wherein the positive electrode binder is added according to the solid content.
[0078] Conductive carbon black (Super .P) and conductive graphite (KS 6) are dispersed in NMP according to the above ratio, and then the above lithium-ion battery positive electrode binder and lithium nickel cobalt manganate are added, stirred and dispersed to obtain the positive electrode slurry.
[0079] The positive electrode slurry is coated on the positive electrode current collector carbon-coated aluminum foil, dried at 100° C., rolled, and cut into strips of 20 mm×100 mm to obtain the positive electrode sheet.
[0080] 3) Lithium-ion battery preparation:
[0081] A negative electrode sheet is obtained, wherein the negative electrode active material in the negative electrode sheet is graphite; a positive electrode sheet, a negative electrode sheet and a separator are stacked to obtain a winding core, the winding core, an aluminum-plastic film and a commercially available lithium-ion battery electrolyte are assembled, and aging, formation and other processes are performed to prepare a lithium-ion battery.
[0082] Example 2
[0083] Most of the steps of this embodiment are the same as those of Embodiment 1, except that in step S1 of preparing the positive electrode binder, 15 g of butyl methacrylate, an acrylic acid ester monomer, is added.
[0084] The molar ratio of acrylonitrile to acrylate monomers is 9.4:1.1; and the molar ratio of the total molar ratio of acrylonitrile and acrylate monomers to mercaptosuccinic acid is 15.77:1.
[0085] Example 3
[0086] Most of the steps of this embodiment are the same as those of Embodiment 2, except that in step S1 of the preparation of the positive electrode binder, 32 g of acrylonitrile and 60 g of butyl methacrylate, an acrylic acid ester monomer, are added.
[0087] The molar ratio of acrylonitrile to acrylate monomers is 6.0:4.2; and the molar ratio of the total molar ratio of acrylonitrile and acrylate monomers to mercaptosuccinic acid is 15.43:1.
[0088] Example 4
[0089] Most of the steps of this embodiment are the same as those of Embodiment 2, except that in step S1 of the preparation of the positive electrode binder, 6 g of acrylonitrile and 130 g of butyl methacrylate, an acrylic acid ester monomer, are added.
[0090] The molar ratio of acrylonitrile to acrylate monomers is 1.1:9.1; and the molar ratio of the total molar ratio of acrylonitrile and acrylate monomers to mercaptosuccinic acid is 15.43:1.
[0091] Example 5
[0092] Most of the steps of this embodiment are the same as those of Embodiment 2, except that in step S1 of the preparation of the positive electrode binder, 45 g of acrylonitrile and 40 g of butyl methacrylate, an acrylic acid ester monomer, are added.
[0093] The molar ratio of acrylonitrile to acrylate monomers is 8.5:2.8; the molar ratio of the total molar ratio of acrylonitrile and acrylate monomers to mercaptosuccinic acid is 15.43:1.
[0094] Example 6
[0095] Most of the steps of this embodiment are the same as those of Embodiment 1, except that in step S1 of the preparation of the positive electrode binder, 20 g of acrylonitrile and 20 g of butyl methacrylate, an acrylic acid ester monomer, are added.
[0096] The molar ratio of acrylonitrile to acrylate monomers is 3.7:1.4; the molar ratio of the total molar ratio of acrylonitrile and acrylate monomers to mercaptosuccinic acid is 7.79:1.
[0097] Example 7
[0098] Most of the steps of this embodiment are the same as those of Embodiment 1, except that 1 g of mercaptosuccinic acid is added in step S1 of the preparation of the positive electrode binder.
[0099] Wherein, the molar ratio of acrylonitrile to mercaptosuccinic acid is 141.85:1.
[0100] Example 8
[0101] Most of the steps of this embodiment are the same as those of embodiment 1, except that in step S2 of the preparation of the positive electrode binder, the diacid monomer is 0.1 mol, the 3,3',4,4'-dibenzophenone tetraacid dianhydride is 0.9 mol, and the toluene diisocyanate is 1.0 mol.
[0102] The molar ratio of the diacid monomer to the anhydride monomer is 10:90; and the molar ratio of the total molar ratio of the diacid monomer and the anhydride monomer to the diisocyanate monomer is 1:1.
[0103] Example 9
[0104] Most of the steps of this embodiment are the same as those of embodiment 1, except that in step S2 of the preparation of the positive electrode binder, the diacid monomer is 0.45 mol, the 3,3',4,4'-dibenzophenone tetraacid dianhydride is 0.5 mol, and the toluene diisocyanate is 1.0 mol.
[0105] The molar ratio of the diacid monomer to the anhydride monomer is 45:50; and the molar ratio of the total molar ratio of the diacid monomer and the anhydride monomer to the diisocyanate monomer is 0.95:1.
[0106] Example 10
[0107] Most of the steps of this embodiment are the same as those of embodiment 1, except that in step S2 of the preparation of the positive electrode binder, the diacid monomer is 0.5 mol, the 3,3',4,4'-dibenzophenone tetraacid dianhydride is 0.8 mol, and the toluene diisocyanate is 1.0 mol.
[0108] The molar ratio of the diacid monomer to the anhydride monomer is 50:80; and the molar ratio of the total molar ratio of the diacid monomer and the anhydride monomer to the diisocyanate monomer is 1.3:1.
[0109] Embodiment 11
[0110] Most of the steps of this embodiment are the same as those of embodiment 1, except that in step S2 of the preparation of the positive electrode binder, the diacid monomer is 0.5 mol, the 3,3',4,4'-dibenzophenone tetraacid dianhydride is 0.4 mol, and the toluene diisocyanate is 1.0 mol.
[0111] The molar ratio of the diacid monomer to the anhydride monomer is 50:40; and the molar ratio of the total molar ratio of the diacid monomer and the anhydride monomer to the diisocyanate monomer is 0.9:1.
[0112] Example 12
[0113] Most of the steps of this embodiment are the same as those of Embodiment 2, except that the types of acrylic acid ester monomers added in step S1 are different, and the acrylic acid ester monomers in Embodiment 12 are ethyl methacrylate and methyl acrylate.
[0114] The types of anhydride monomers in step S2 are different. The anhydride monomers in Example 12 are 4,4'-(4,4'-isopropyldiphenyldiphenoxy)diphthalic anhydride and cyclobutanetetracarboxylic dianhydride;
[0115] The types of diisocyanate monomers in step S2 are different. The diisocyanate monomer in Example 12 is toluene diisocyanate.
[0116] It should be noted that the total mole of the anhydride monomer in Example 12 is still 0.8 mol, the total mole of the diacid monomer is still 0.2 mol; the total mole of the diisocyanate is still 1 mol; and the total mole of the acrylate monomer is the same as that in Example 2.
[0117] Comparative Example 1
[0118] The positive electrode binder of this comparative example adopts commercially available PVDF, and the preparation method of the battery is the same as that of Example 1.
[0119] Comparative Example 2
[0120] This comparative example is the same as the large step of Example 1, except that: in the positive electrode binder preparation step, there is no S1 step, and in the S2 step, 0.2 mol (30 g) of mercaptosuccinic acid, 0.8 mol (322.2 g) of 3,3',4,4'-dibenzophenone tetraacid dianhydride (BTDA), 0.5 mol (87.1 g) of toluene diisocyanate (TDI), and 0.5 mol (125.1 g) of diphenylmethane diisocyanate (MDI) are directly subjected to polycondensation reaction, and the reaction conditions are the same as S2. In the late stage of the reaction, the polymerization solution is turbid, insoluble matter is precipitated, and the electrode cannot be prepared.
[0121] Comparative Example 3
[0122] This comparative example has the same major steps as Example 1, except that: this comparative example has the same major steps as Example 1, except that: in step S1 of the preparation of the positive electrode binder, acrylonitrile monomer is not added.
[0123] The molar ratio of the total mole of the acrylic acid ester monomer to the mercaptosuccinic acid is 15.77:1.
[0124] Performance Testing:
[0125] The positive electrode sheets and lithium-ion batteries prepared in the above examples and comparative examples were subjected to the following tests.
[0126] 1) Steel needle winding flexibility test
[0127] The positive electrode sheets prepared in the above embodiments and comparative examples were tested for flexibility according to the method of GB / T 1731-2020.
[0128] 2) Cycle capacity retention test
[0129] The batteries prepared in the above embodiments and comparative examples were tested for capacity of the soft-pack battery at a temperature of 25°C ± 2°C, recorded as the capacity before storage, and the soft-pack battery was discharged at a constant current of 0.5C to a voltage of 2.7V. Then, it was charged at a constant current of 1C to a voltage of 4.3V, and then charged at a constant voltage to a cut-off current of 0.05C. After charging, it was discharged at a constant current of 1C to 2.75V; the discharge capacity C1 and internal resistance R1 of the first week were recorded; this method was repeated for 500 cycles, and the discharge capacity C1 of the 500th week was recorded. 500 , internal resistance R 500。
[0130] Cycle capacity retention rate = C 500 / C1×100%.
[0131] The cycle capacity retention rate of the battery at 45°C was tested using the same test method.
[0132] Fill in the results of the above tests in Table 1.
[0133] Table 1
[0134]
[0135] It can be seen from the experimental results in Table 1 that the positive electrode binder of the present application has good solubility in polar aprotic solvents; the positive electrode sheet prepared using the positive electrode binder of the present application has good mechanical properties; when the above-mentioned positive electrode sheet is used to prepare a battery, the polymer contained in the positive electrode binder can generate a dipole interaction force with lithium ions, thereby increasing the lithium ion diffusion rate, reducing the electrode impedance, and improving the battery cycle performance; at the same time, the polymer has good thermal stability, so that the battery prepared using it has good cycle stability.
[0136] Comparison of Examples 1-5 and Comparative Example 3 shows that the molar ratio of the repeating unit containing a cyano group to the repeating unit containing an ester group affects the cycle capacity retention rate of the battery, and the molar ratio of the repeating unit containing a cyano group to the repeating unit containing an ester group affects the electrode impedance, thereby improving the cycle capacity retention rate of the battery, and from the comparison of Examples 1-3, 5 and Example 4, it can be seen that when the molar number of the repeating unit containing a cyano group is higher than the molar number of the repeating unit containing an ester group, it is more beneficial to further reduce the electrode impedance, so that the battery has a better cycle capacity retention rate. At the same time, from the comparison of Example 1 and Examples 2-5, it can be seen that the introduction of the ester unit improves the flexibility of the pole piece.
[0137] It can be seen from Examples 6-7 that the ratio of n1 to n2 will affect the solubility, heat resistance, stability and mechanical properties of the positive electrode binder. In Example 6, n1:n2 is lower than 100:(1~10), and the positive electrode binder is a turbid colloid in NMP and is difficult to dissolve. This is because when n1:n2 is lower than 100:(1~10), the chain segment of the diacid monomer is short and the effect of improving solubility decreases; in Example 7, n1:n2 is higher than 100:(1~10), and its cycle capacity retention rate and stability become poor.
[0138] The mechanical properties of the electrode sheet in Example 10 are poor, and the cycle performance of the battery is poor. This is because when the molar ratio of the total mole of the diacid monomer and the anhydride monomer to the diisocyanate monomer is higher than (95-105):100, the content of the added diisocyanate monomer is too little, the viscosity of the prepared positive electrode binder is low, the main chain generated is short, and the positive electrode sheet obtained by coating the positive electrode slurry on the surface of the positive electrode collector is relatively brittle and easy to break. The positive electrode binder in Example 11 is a gel in NMP and is difficult to dissolve. When the molar ratio of the total mole of the diacid monomer and the anhydride monomer to the diisocyanate monomer is lower than (95-105):100, the content of the added diisocyanate monomer is too much, and the mixed solution formed by the diacid monomer, the anhydride monomer, the diisocyanate, and the second organic solvent produces a gel, and the positive electrode binder cannot be prepared.
[0139] It can be seen from Comparative Example 2 that if the diacid monomer does not have a side chain, the polymerization solution will be turbid and insoluble matter will precipitate in the later stage of the reaction, making it impossible to prepare the electrode.
[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A positive electrode binder, characterized in that: The positive electrode binder comprises a polymer, the polymer comprises a polyamideimide segment and a side chain segment connected to the polyamideimide segment as a side chain, the side chain segment comprises a repeating unit containing a cyano group and a repeating unit containing an ester group; the polymer is formed by polymerizing a diacid monomer, an acid anhydride monomer and a diisocyanate monomer; the diacid monomer is a polymer monomer having at least one terminal containing a diacid group; the polymer monomer comprises a repeating unit containing a cyano group and a repeating unit containing an ester group; The diacid monomer is formed by polymerizing a dicarboxylic acid containing a mercapto group with a (meth)acrylonitrile monomer and a (meth)acrylate monomer; The molar ratio of the cyano group-containing repeating unit to the ester group-containing repeating unit is (9-6): (1-4); The ratio of the total mole number of the (meth)acrylonitrile monomer and the (meth)acrylate monomer to the mole number of the mercapto group-containing dicarboxylic acid is 100:(1-10); The molar ratio of the diacid monomer to the anhydride monomer is (10-50): (50-90); The ratio of the total mole number of the diacid monomer and the acid anhydride monomer to the mole number of the diisocyanate monomer is (95-105):
100.
2. The positive electrode binder according to claim 1, characterized in that The repeating unit containing a cyano group is selected from (meth)acrylonitrile monomer units; and the repeating unit containing an ester group is selected from (meth)acrylate monomer units.
3. The positive electrode binder according to claim 1, characterized in that The molar ratio of the (meth)acrylonitrile monomer to the (meth)acrylate monomer is (9-6):(1-4).
4. The positive electrode binder according to claim 1, characterized in that The (meth) acrylic acid ester monomers include one or more of methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-hexyl methacrylate, isooctyl methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, and isooctyl acrylate; And / or, the acid anhydride monomer includes one or more of pyromellitic dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(4,4'-isopropyldiphenyldiphenoxy)diphthalic anhydride, butanetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, p-phenylene di(trimellitic acid ester) dianhydride, and trimellitic acid anhydride; And / or, the diisocyanate monomer includes one or more of toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate.
5. A positive electrode sheet, characterized in that: The invention comprises a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode binder, and the positive electrode binder is the positive electrode binder according to any one of claims 1 to 4.
6. A lithium ion battery, characterized in that: The invention comprises a negative electrode sheet, a separator and the positive electrode sheet as claimed in claim 5.