Overhead weld laser welding method and butt joint of sheet metal parts
The overhead welding laser welding method solves the problem of weld defects during the welding process by positioning the workpiece side by side and setting up protective gas nozzles, adjusting the laser and gas parameters, achieving the flatness and stability of the weld, and improving the welding quality and efficiency. .
Patent Information
- Application Number
- CN202410879784.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-02
AI Technical Summary
Existing laser welding technology can easily cause weld defects such as humps, collapses and pores during the welding process of butt sheet metal parts, and existing solutions have problems such as high cost, complex operation or low efficiency.
Using the overhead welding laser welding method, by positioning the workpieces side by side, setting up the laser overhead welding device and protective gas nozzle, and adjusting the angle and parameters, the laser beam and protective gas are supported on the surface of the molten pool behind the small hole, slowing down the flow of the molten pool. and cooling process to achieve the smoothness of the weld.
It effectively reduces the hump and collapse of the weld root, improves the stability of the small hole, reduces the occurrence of welding spatter and pores, forms a smooth weld, and improves the welding quality and efficiency.
Smart Images

Figure CN118404201B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of laser welding technology, in particular, to an overhead weld laser welding method. In addition, the present invention also relates to a butt-jointed sheet metal part, which is manufactured by using the overhead weld laser welding method. Background Art
[0002] Laser welding is one of the most widely used advanced processes in laser processing technology. It has the advantages of fast heating and cooling, small welding deformation, and high processing flexibility. It is widely used in aerospace, automotive, precision instruments and other industries. Laser welding uses a high-energy-density laser beam as a heat source to radiate the surface of the material, causing the material to melt or even vaporize. Under the action of evaporation pressure, the surface of the molten pool sinks to form a "keyhole" (also called a small hole). The opening and closing of the small hole is directly affected by the pressure balance of the small hole wall. The small hole effect is the essential feature of laser penetration welding.
[0003] When the first workpiece 1 is arranged horizontally, the molten pool flows in the direction 10 as shown in FIG. Figure 1 As shown in FIG. 1 , the gravity G and the reaction force f of the steam in the hole on the molten pool are superimposed on the molten pool 14 in front of the small hole and the molten pools on the left and right sides (not marked in the figure). The molten pool 14 in front of the small hole and the molten pools on the left and right sides flow downward along the hole wall, resulting in a hump 12 at the root of the weld 9; the molten pool 8 behind the small hole is reversed along the hole wall under the superimposed action of the gravity G and the reaction force f of the steam in the hole on the molten pool, causing the top of the weld 9 to collapse 11. At the same time, the molten pool 8 behind the small hole will impact the "gas-liquid interface" to form wrinkles 16 during the process of flowing back to the root of the weld 9, resulting in reduced stability of the small hole and prone to defects such as spatter and welding pores; the cross-section of the weld 9 is shown in FIG. Figure 2 shown.
[0004] To address this problem, various solutions are provided in the prior art, but they all have their own limitations in practical applications.
[0005] For example, Chinese patent CN103506770A discloses an aluminum alloy laser welding auxiliary weld forming material and a preparation method thereof, which obtains a smooth-looking weld by attaching the prepared aluminum alloy laser welding auxiliary weld forming material to the back of the weld through forced forming, thereby preventing the weld from collapsing. However, the patent has the following problems: 1) the prepared aluminum alloy laser welding auxiliary weld forming material needs to be tightly fitted to the back of the weld. If the fit is not tight, there is a risk of welding wind collapse; 2) the manufacturing process of the aluminum alloy laser welding auxiliary weld forming material is complicated and the production cost is high.
[0006] For example, Chinese patent CN113634896A discloses a laser welding device and a laser welding method for improving the surface forming of the weld. The device provides an upward suction to the molten pool through a gas-electric exhauster, thereby realizing the overall upward movement of the molten pool during laser deep penetration welding of thick plates. The device can effectively improve defects such as upper surface collapse and bottom hump during laser deep penetration welding of thick plates. However, since the molten pool of laser welding is small, it is difficult to accurately apply the suction to the bottom of the molten pool, which is difficult to achieve in practical applications.
[0007] For example, Chinese patent CN111545906A discloses a mirror laser welding device and method for optimizing weld pool formation, which effectively prevents defects such as collapse during welding by tightly clamping high-laser-transmittance high-temperature-resistant glass on the lower side of the welded workpiece. However, this patent has the following problems: 1) The radiation temperature of the laser spot is very high, which may burn the high-laser-transmittance high-temperature-resistant glass, and the impurities generated enter the molten pool, affecting the quality of the weld; 2) Clamping the high-laser-transmittance high-temperature-resistant glass tightly on the lower side of the workpiece requires precision tooling to ensure, which is costly.
[0008] For example, Chinese patent CN114799527A discloses a thin plate laser arc composite high-speed vertical welding method and device. The workpiece is placed upright. When the laser is welded vertically upward, the welding direction is opposite to gravity. The MIG welding gun provides liquid metal to enter the molten pool from the front of the keyhole at the edge of the molten pool. The jet device is set to reduce the problem of weld defects caused by the liquid metal in the welding molten pool flowing downward due to the influence of gravity. However, the patent has the following problems: 1) Its structure is complex, requiring the MIG welding gun, low-energy laser beam, and high-energy laser beam to cooperate, which is difficult to operate and costly; 2) Because the workpiece is placed upright and the jet device also sprays protective gas toward the welding work surface, the molten metal is easy to flow down along the weld from the back of the welding work surface (the side away from the MIG welding gun), resulting in defects on the back of the weld.
[0009] In addition, Chinese patent CN111417485A discloses a manufacturing method and manufacturing device for a molded object, which is formed on the upper surface of the base plate by tilting the base plate and controlling the weld height BH and weld width BW corresponding to the base surface inclination angle θ and the track inclination angle to overcome the sagging of the weld bead caused by the influence of gravity. Since it uses molten metal wire for molding, it needs the upper surface of the base plate for support, and is not suitable for welding of butt-jointed sheet metal parts without support from the base plate. Summary of the invention
[0010] The invention provides an overhead weld laser welding method and butting sheet metal parts to solve the technical problem that laser welding in the prior art easily leads to weld defects.
[0011] According to one aspect of the present invention, there is provided an overhead weld laser welding method, comprising the following steps:
[0012] S1. Position two workpieces to be welded side by side, so that the workpieces form an angle α with the horizontal plane, and the angle α is greater than 90°;
[0013] S2. Arrange the laser overhead welding device and the shielding gas nozzle below the workpiece;
[0014] S3, start the laser overhead welding device, so that the center line of the laser beam forms an angle β with the normal line of the workpiece, and the shielding gas nozzle forms an angle γ with the center line of the laser beam; by setting the α angle, β angle, γ angle, welding power P, welding speed V, defocusing amount U, swing amplitude W and shielding gas pressure σ, the laser overhead welding device emits a laser beam to radiate the two workpieces to be welded, and the shielding gas nozzle moves with the laser overhead welding head and blows shielding gas to support the surface of the molten pool behind the keyhole;
[0015] S4. When the welding end point is reached, the laser overhead welding device is turned off, the shielding gas nozzle stops blowing shielding gas, and the welding process is completed.
[0016] In this embodiment, the protective gas nozzle includes a ventilation pipe, and the air outlet cross section of the ventilation pipe is arranged parallel to the workpiece.
[0017] In this embodiment, the distance from the nozzle tip to the welding point is 1-2 mm, and the diameter of the ventilation pipe is 2-5 mm.
[0018] In this embodiment, the protective gas pressure σ is 0.1-0.5 bar.
[0019] In this embodiment, the protective gas is argon.
[0020] In this embodiment, the angle α is 90° to 180°, the angle β is 5° to 45°, and the angle γ is 45° to 85°.
[0021] In this embodiment, the welding power P of the laser overhead welding device is 1-2 kW, the welding speed V is 1-2 m / min, the defocus amount U is 0-+5 mm, and the swing amplitude W is 0-2 mm.
[0022] In this embodiment, the thickness of the workpiece is 0.5-3 mm.
[0023] In this embodiment, the thickness of the workpiece is 1.2 mm.
[0024] According to another aspect of the present invention, there is also provided a butted sheet metal part, which is manufactured using the above-mentioned overhead weld laser welding method.
[0025] The present invention has the following beneficial effects:
[0026] In the overhead weld laser welding method of the present invention, the first workpiece and the second workpiece are fixed side by side, and the first workpiece is arranged at an angle α greater than 90° with the horizontal plane. On the one hand, during overhead welding, the steam reaction force f in the hole acts obliquely upward on the molten pool in front of the small hole and the molten pools on the left and right sides, and the gravity G of the molten pools in front of the small hole and on the left and right sides can be decomposed into a component force in the opposite direction to the steam reaction force f in the hole. When α and β become larger at the same time, the component force of gravity becomes larger, which can reduce the effect of the steam reaction force f in the hole on the molten pool in front of the small hole and the molten pools on the left and right sides. Compared with the flat weld butt joint of sheet metal In the welding method of alloy, the combined force acting on the molten pool in front of the small hole and the molten pools on the left and right sides is greatly reduced, so that the speed at which the molten pools in front of the small hole and the left and right sides flow downward along the hole wall is greatly slowed down, and the volume of the molten pool ejected from the bottom is reduced, which can avoid the formation of a hump at the root of the weld; on the other hand, the speed at which the molten pool in front of the small hole and the molten pools on the left and right sides flow downward along the hole wall is greatly slowed down, and the volume of molten metal flowing to the bottom of the molten pool is reduced. The reduced molten metal will flow to the molten pool behind the small hole. The molten pool behind the small hole flows in the direction of gravity under the action of gravity G, and the protective gas nozzle is sprayed to the molten pool. The shielding gas is injected, wherein the shielding gas is pressurized by an air compressor, so that the shielding gas ejected from the special shielding gas nozzle forms an air column, which supports the surface of the molten pool behind the small hole to slow down the tendency of the molten metal in the molten pool behind the small hole to flow in the direction of gravity; since gravity is opposite to the reflux direction of the molten metal at the rear side of the small hole, and the gas ejected from the shielding gas nozzle can accelerate the cooling and solidification of the molten metal, the molten metal at the rear side of the small hole will not flow back to the root of the weld, thereby avoiding disturbing the formation of wrinkles on the rear wall of the small hole, improving the stability of the small hole, and reducing welding spatter. Splashing can be prevented to prevent welding porosity; at the same time, since the molten pool behind the keyhole is affected by the surface tension of the molten pool interface, the supporting force of the solidified weld and the reaction force of the steam in the keyhole in addition to the gravity G and the shielding gas pressure, the welding power P, welding speed V, defocusing amount U and swing amplitude W of the laser overhead welding device are adjusted, and the shielding gas pressure σ, α angle, β angle and γ angle sprayed from the shielding gas nozzle are adjusted to achieve force balance in the molten pool. After the molten pool behind the keyhole is quickly cooled, a weld with relatively smooth front and back sides can be formed.
[0027] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0029] Figure 1 It is a schematic diagram of the prior art laser welding flat welding butt joint sheet metal;
[0030] Figure 2 It is a structural schematic diagram of the weld cross section of the prior art;
[0031] Figure 3 It is a schematic diagram of the layout of the overhead weld laser welding method of the preferred embodiment of the present invention;
[0032] Figure 4 It is a schematic diagram of the structure of the gas column supporting the molten pool behind the small hole in the preferred embodiment of the present invention;
[0033] Figure 5 is a schematic structural diagram of a protective gas nozzle of a preferred embodiment of the present invention;
[0034] Figure 6 is a structural schematic diagram of a weld cross section of a preferred embodiment of the present invention;
[0035] Figure 7 It is a physical schematic diagram of the weld cross section of the preferred embodiment of the present invention.
[0036] Legend:
[0037] 1. The first workpiece; 2. The second workpiece; 3. The normal line of the workpiece; 4. The laser beam; 5. The center line of the laser beam; 6. The base material; 7. The shielding gas nozzle; 8. The molten pool behind the keyhole; 9. The weld; 10. The flow direction of the molten pool; 11. The collapse; 12. The hump of the weld; 13. The keyhole; 14. The molten pool in front of the keyhole; 15. The gas column; 16. The wrinkles. DETAILED DESCRIPTION
[0038] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. However, the present invention can be implemented in many different ways as defined and covered below.
[0039] The overhead weld laser welding method of this embodiment includes the following steps:
[0040] S1, positioning the first workpiece 1 and the second workpiece 2 to be welded, the first workpiece 1 and the second workpiece 2 are arranged in parallel, the first workpiece 1 forms an angle α with the horizontal plane, and the angle α is greater than 90°;
[0041] S2, placing the laser overhead welding device and the shielding gas nozzle below the workpiece, that is, the angle between the welding working surface of the first workpiece 1 and the second workpiece 2 and the horizontal plane is 180°-α;
[0042] S3, start the laser overhead welding device, so that the laser beam center line 4 forms an angle β with the workpiece normal 3, and the shielding gas nozzle 7 forms an angle γ with the laser beam center line 4; by setting the α angle, β angle, γ angle, welding power P, welding speed V, defocusing amount U, swing amplitude W and shielding gas pressure σ, the laser overhead welding device emits a laser beam to radiate the first workpiece 1 and the second workpiece 2 to be welded, and the shielding gas nozzle 7 moves with the laser overhead welding head and blows shielding gas to support the surface of the molten pool 8 behind the keyhole;
[0043] S4. When the welding end point is reached, the laser overhead welding device is turned off, and the shielding gas nozzle 7 stops blowing shielding gas, and the welding process is completed.
[0044] The overhead weld laser welding method of this embodiment is as follows: Figure 3 and Figure 4 As shown, the first workpiece 1 and the second workpiece 2 are fixed side by side, and the first workpiece 1 forms an angle α greater than 90° with the horizontal plane, that is, the angle between the welding working surface of the first workpiece 1 and the horizontal plane is 180°-α, and the laser overhead welding device performs overhead welding on the weld of the first workpiece 1 and the second workpiece 2 from below the welding working surface. On the one hand, during overhead welding, the steam reaction force f in the hole acts obliquely upward on the molten pool 14 on the front side of the small hole and the molten pools on the left and right sides, and the gravity G of the molten pools on the front side 14 of the small hole and the left and right sides can be decomposed into a component force in the opposite direction to the steam reaction force f in the hole. When α and β increase at the same time, the component force of gravity increases, which can reduce the effect of the steam reaction force f in the hole on the molten pool 14 on the front side of the small hole and the molten pools on the left and right sides. Figure 1In the flat weld butt welding method shown, the resultant force acting on the molten pool 14 on the front side of the small hole and the molten pools on the left and right sides is greatly reduced, so that the speed at which the molten pools on the front side of the small hole 14 and the molten pools on the left and right sides flow downward along the hole wall is greatly slowed down, and the volume of the molten pool ejected from the bottom is reduced, which can avoid the formation of a hump 12 at the root of the weld 9; on the other hand, the speed at which the molten pool 14 on the front side of the small hole and the molten pools on the left and right sides flow downward along the hole wall is greatly slowed down, and the volume of molten metal flowing to the bottom of the molten pool is reduced, and the reduced molten metal will flow to the molten pool 8 behind the small hole. The molten pool 8 behind the small hole flows in the direction of gravity under the action of gravity G, and shielding gas is sprayed into the molten pool through the shielding gas nozzle 7, wherein the shielding gas is pressurized by an air compression pump, so that the shielding gas ejected from the special shielding gas nozzle 7 forms an air column 15, and the air column 15 supports the surface of the molten pool 8 behind the small hole to slow down the trend of the molten metal in the molten pool 8 behind the small hole to flow in the direction of gravity; due to gravity The molten metal at the rear side of the keyhole 8 has a reverse flow direction opposite to that of the molten metal at the rear side of the keyhole, and the gas ejected from the shielding gas nozzle 7 can accelerate the cooling and solidification of the molten metal. Therefore, the molten metal at the rear side of the keyhole 8 will not flow back to the root of the weld 9, thereby avoiding disturbing the formation of wrinkles 16 on the rear wall of the keyhole, improving the stability of the keyhole 13, reducing welding spatter, and preventing the occurrence of welding pores. At the same time, since the molten pool 8 at the rear side of the keyhole is affected by the gravity G and the shielding gas pressure, it is also affected by the surface tension of the molten pool interface, the supporting force of the solidified weld, and the reaction force of the steam in the keyhole. Therefore, the welding power P, welding speed V, defocusing amount U and swing amplitude W of the laser overhead welding device are adjusted, and the shielding gas pressure σ ejected from the shielding gas nozzle 7, as well as the angles α, β and γ, are adjusted to achieve force balance in the molten pool. After the molten pool 8 at the rear side of the keyhole is quickly cooled, a weld 9 with relatively flat front and back sides can be formed (the cross section of the weld is as shown in FIG. 1 ). Figure 6 as shown).
[0045] like Figure 5 As shown, in this embodiment, the shielding gas nozzle 7 includes a ventilation pipe 71, and the air outlet section 72 of the ventilation pipe 71 is arranged parallel to the first workpiece 1, that is, θ=α-90°, which can ensure that the shielding gas can be evenly sprayed onto the surface of the molten pool 8 behind the small hole, and effectively support the surface of the molten pool 8 behind the small hole.
[0046] In this embodiment, the distance from the nozzle tip to the welding point is 1 to 2 mm, and the diameter of the ventilation tube is 2 to 5 mm. When the distance from the nozzle tip to the welding point is less than 1 mm and the diameter of the ventilation tube is less than 2 mm, the air column 15 is difficult to cover the molten pool 8 behind the small hole; when the distance from the nozzle tip to the welding point is greater than 2 mm and the diameter of the ventilation tube is greater than 5 mm, the air column 15 will cover the molten pool 14 in front of the small hole and the molten pools on the left and right sides, causing molten metal to splash.
[0047] In this embodiment, the shielding gas pressure σ is 0.1 to 0.5 bar. When the shielding gas pressure σ is less than 0.1, the gas column 15 has a poor supporting effect on the molten pool 8 behind the small hole. When the shielding gas pressure σ is greater than 0.5 bar, the molten metal will splash.
[0048] In this embodiment, the protective gas is argon gas. Optionally, the purity of the argon gas is 99.999%.
[0049] In this embodiment, the angle value of α is 90° to 180°. If α is less than 90°, the reaction force of the steam in the hole on the molten pool in front of the small hole and the molten pools on the left and right sides cannot play a supporting role, and the root of the weld 9 is prone to form a hump 12; the angle value of β is 5° to 45°. At this time, the reaction force of the steam in the hole acts entirely on the molten pool in front of the small hole and the molten pools on the left and right sides, and the supporting effect on the molten pool is the best. If the angle of β is other angles, the reaction force of the steam in the hole on the molten pool in front of the small hole and the molten pools on the left and right sides is the component of f, and the supporting effect on the molten pool will be weakened; the angle of γ is 45° to 85°. Optionally, the angle value of α is 135° to 175°, so as to be suitable for workpieces with a thickness of 0.5 to 3 mm. Optionally, β=180°-α, γ=α-90°, at this time, the laser beam center line 4 is arranged in the vertical direction, and the shielding gas nozzle 7 is arranged in the vertical direction, which can avoid interference between the laser beam and the shielding gas nozzle 7 and ensure smooth overhead welding.
[0050] In this embodiment, the welding power P of the laser overhead welding device is 1-2 kW, the welding speed V is 1-2 m / min, the defocus amount U is 0-+5 mm, and the swing amplitude W is 0-2 mm.
[0051] In this embodiment, the thickness of the first workpiece 1 and the second workpiece 2 are both 0.5 to 3 mm. When the thickness of the first workpiece 1 and the second workpiece 2 is less than 0.5 mm, molten metal splashing may occur easily during welding. When the thickness of the first workpiece 1 and the second workpiece 2 is greater than 3 mm, it is difficult for the laser to penetrate the workpiece, resulting in poor welding effect.
[0052] like Figure 7 As shown, in this embodiment, the thickness of the first workpiece 1 and the second workpiece 2 are both 1.2 mm.
[0053] The overhead weld laser welding method of the present invention can reduce the combined force acting on the molten pool 14 on the front side of the small hole and the molten pools on the left and right sides, thereby slowing down the downward flow speed of the molten pool 14 on the front side of the small hole and the molten pools on the left and right sides. The volume of molten metal ejected from the bottom of the molten pool is greatly reduced, thereby avoiding the formation of a hump 12 at the root of the weld 9; the molten metal in the molten pool 8 on the rear side of the small hole will not flow back under the action of gravity, thereby avoiding disturbing the rear wall of the small hole, improving the stability of the small hole 13, avoiding the occurrence of molten metal splashing, and preventing the bottom of the weld 9 from collapsing 11. The weld is smooth as a whole and has good mechanical properties.
[0054] A butt-jointed sheet metal part is manufactured by utilizing the above-mentioned overhead weld laser welding method.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for laser welding an overhead weld, characterized in that: The following steps are involved: S1. Position two workpieces to be welded side by side, with the workpieces forming an angle α with the horizontal plane, and the angle value of α is 135° to 175°; S2. Arrange the laser overhead welding device and the shielding gas nozzle below the workpiece so that the angle between the welding working surface of the workpiece and the horizontal plane is 180°-α; S3, start the laser overhead welding device, so that the center line of the laser beam forms an angle β with the normal line of the workpiece, and the shielding gas nozzle forms an angle γ with the center line of the laser beam; by setting the α angle, β angle, γ angle, welding power P, welding speed V, defocusing amount U, swing amplitude W and shielding gas pressure σ, the laser overhead welding device emits a laser beam to radiate the two workpieces to be welded, and the shielding gas nozzle moves with the laser overhead welding head and blows shielding gas to support the surface of the molten pool behind the keyhole; S4. When the welding end point is reached, the laser overhead welding device is turned off, the shielding gas nozzle stops blowing shielding gas, and the welding process is completed.
2. The overhead weld laser welding method according to claim 1, characterized in that: The protective gas nozzle comprises a ventilation pipe, and the air outlet cross section of the ventilation pipe is arranged parallel to the workpiece.
3. The overhead weld laser welding method according to claim 2, characterized in that: The distance from the nozzle tip to the welding point is 1 to 2 mm, and the diameter of the ventilation pipe is 2 to 5 mm.
4. The overhead seam laser welding method according to any one of claims 1 to 3, characterized in that: The protective gas pressure σ is 0.1~0.5bar.
5. The overhead weld laser welding method according to claim 4, characterized in that: The shielding gas is argon.
6. The overhead weld laser welding method according to claim 1, characterized in that: The β angle value is 5° to 45°, and the γ angle value is 45° to 85°.
7. The overhead weld laser welding method according to claim 1, characterized in that: The welding power P of the laser overhead welding device is 1-2 kW, the welding speed V is 1-2 m / min, the defocus amount U is 0-+5 mm, and the swing amplitude W is 0-2 mm.
8. The overhead weld laser welding method according to claim 1, characterized in that: The thickness of the workpiece is 0.5 to 3 mm.
9. The overhead weld laser welding method according to claim 8, characterized in that: The thickness of the workpiece is 1.2 mm.
10. A butt-jointed sheet metal part, characterized in that: The method is manufactured by using the overhead weld laser welding method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Aluminum alloy sheet laser welding auxiliary weld-joint forming material and preparation method thereof
CN103506770A
Method and device for manufacturing shaped objects
CN111417485A
Mirror image laser welding device and method for optimizing weld joint forming of molten pool
CN111545906A
Laser welding device and laser welding method for improving weld surface forming
CN113634896A
Laser mirror welding method
CN111604593A