A new type of wear-resistant leather and its preparation process

The combination of TiO2-aminographene modified leather fiber and thermoplastic polyurethane foam layer solves the problem of insufficient wear resistance and wrinkle resistance of traditional leather, achieves higher wear resistance and environmental protection, and is suitable for high-end application scenarios .

CN118404876BActive Publication Date: 2024-10-22ZHEJIANG LIANQIAO NEW MATERIAL TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410492003.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2024-10-22
Estimated Expiration
2044-04-23

AI Technical Summary

Technical Problem

Traditional leather has insufficient wear resistance under high-intensity wear and harsh environments, is prone to scratches and abrasions, and has poor wrinkle resistance, affecting its service life and environmental protection.

Method used

TiO2-aminographene modified leather fiber is combined with the thermoplastic polyurethane foam layer to enhance the mechanical strength and toughness of the leather fiber through chemical modification and physical filling, and form a buffer layer through the foaming process to improve the wear resistance and comfort of the leather. Spend.

Benefits of technology

It significantly improves the wear resistance, crack resistance and tensile damage resistance of leather, extends its service life, reduces environmental risks, and is suitable for high-end application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004805696180000111
    Figure BDA0004805696180000111
Patent Text Reader

Abstract

The invention discloses a novel wear-resistant leather and a preparation process thereof, belonging to the technical field of leather materials, comprising a base fabric layer, a foaming layer and a wear-resistant leather layer arranged on the base fabric layer; the wear-resistant leather layer comprises the following components in parts by weight: 15-20 parts of TiO2-amino graphene modified leather fibers, 40-60 parts of polypropylene, 16-28 parts of polyisobutylene, 1-5 parts of plasticizer, 0.1-0.3 parts of antioxidants and 0.2-0.5 parts of antibacterial agents; the foaming layer comprises the following components in parts by weight: 80-120 parts of thermoplastic polyurethane, 20-60 parts of propylene oxide, 16-30 parts of polyether polyols, 10-20 parts of dibutyl sebacate and 1-3 parts of foaming agents; the plasticizer is one or more of nano calcium carbonate, silicate, diisononyl sebacate and tributyl citrate. The problem of insufficient wear resistance and easy cracking of existing leather is solved. It has the advantages of good mechanical properties, economy and environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of leather materials, and in particular to a novel wear-resistant leather and a preparation process thereof. Background Art

[0002] As a material with a long history and wide application, leather is deeply favored by consumers for its unique texture, durability and aesthetics. However, traditional leather often shows insufficient wear resistance when facing high-intensity wear, harsh environment and frequent use, which limits its further application in high-end footwear, furniture decoration, automobile interior and other fields. However, as consumers' requirements for product performance and environmental protection continue to increase, traditional leather technology faces challenges in wear resistance and wrinkle resistance. (1) Wear resistance problem: Although existing leather is surface treated through tanning, coating and other processes, it is still prone to scratches and wear in areas with long-term use or frequent friction, such as uppers, soles, bottoms of handbags, etc., affecting the appearance and service life. (2) Wrinkle resistance bottleneck: Leather is prone to permanent wrinkles after bending, folding or being pressed, which not only affects the visual beauty, but also reduces the comfort of wearing or use.

[0003] Faced with the limitations of traditional leather technology, many composite leathers have come into being. Traditional composite leathers rely on anti-wrinkle treatment methods such as resin finishing and pre-shrinkage in terms of wear resistance and wrinkle resistance. These treatments may cause the leather to become hard, the breathability to decrease, and the anti-wrinkle effect to weaken over time; and traditional composite leathers may use more chemical additives in the production process, which has a certain impact on the environment and human health, and are not easy to degrade after being discarded, which does not meet the demand of modern consumers for environmentally friendly products.

[0004] Therefore, there is an urgent need for a new type of wear-resistant leather and its preparation process to improve the problems of insufficient wear resistance, easy cracking and poor environmental protection of leather in the prior art. Summary of the invention

[0005] To this end, the present invention provides a new type of wear-resistant leather and a preparation process thereof, so as to solve the problems of insufficient wear resistance, easy cracking and poor environmental protection of leather in the prior art.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] According to a first aspect of the present invention, there is provided a novel wear-resistant leather, comprising a base fabric layer, a foaming layer and a wear-resistant leather layer disposed on the base fabric layer;

[0008] The wear-resistant leather layer comprises the following components in parts by weight: 15-20 parts of TiO2-amino graphene modified leather fiber, 40-60 parts of polypropylene, 16-28 parts of polyisobutylene, 1-5 parts of plasticizer, 0.1-0.3 parts of antioxidant and 0.2-0.5 parts of antibacterial agent;

[0009] The foaming layer comprises the following components in parts by weight: 80-120 parts of thermoplastic polyurethane, 20-60 parts of propylene oxide, 16-30 parts of polyether polyol, 10-20 parts of dibutyl sebacate and 1-3 parts of foaming agent.

[0010] Furthermore, the plasticizer is one or more of nano calcium carbonate, silicate, diisononyl sebacate, and tributyl citrate.

[0011] Furthermore, the antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)]pentaerythritol, bis(3,5-di-tert-butyl-4-hydroxyphenyl) sulfide, tris(2,4-di-tert-butylphenyl) phosphite, and dilauryl thiodipropionate.

[0012] Furthermore, the antibacterial agent is a nano-silver antibacterial agent.

[0013] Furthermore, the foaming agent is one or more of azodicarbonamide, ammonium bicarbonate or sodium bicarbonate.

[0014] According to a second aspect of the present invention, there is provided a process for preparing a novel wear-resistant leather, comprising the following steps:

[0015] S1. The formula amount of TiO2-amino graphene modified leather fiber, polypropylene, polyisobutylene, plasticizer, antioxidant and antibacterial agent is mixed and calendered to obtain a wear-resistant leather layer;

[0016] S2. The amount of thermoplastic polyurethane, propylene oxide, polyether polyol, dibutyl sebacate, foaming agent and thickener is mixed uniformly, and then the resulting mixed slurry is applied to the lower surface of the wear-resistant leather layer obtained in S1, foaming, calendering, to obtain a foaming layer;

[0017] S3. Bond the lower surface of the foaming layer to the base fabric layer to obtain a new type of wear-resistant leather.

[0018] Furthermore, the preparation of the TiO2-amino graphene modified leather fiber comprises the following steps:

[0019] (1) dispersing graphene oxide-based nanoparticles in ethanol and heating them, then adding 3-aminopropyltrimethoxysilane APS, reflux reaction, centrifuging, washing with ethanol, and drying in an oven to obtain amino-modified graphene nanoparticles;

[0020] (2) dissolving tetrabutyl titanate in anhydrous ethanol, slowly dropping 30-60 mL of deionized water into the mixture under stirring conditions, and continuing the reaction for 1-3 hours after the mixture becomes a white emulsion to obtain nano-sized titanium dioxide powder, and then adding the nano-sized titanium dioxide powder into a peptizing agent to dissolve it to obtain a precursor solution;

[0021] (3) adding amino-modified graphene nanoparticles to a precursor solution, heating under reflux for reaction, filtering and washing a precipitate generated by the reaction, and finally sintering the precipitate at 300-600° C. in an inert atmosphere to obtain a TiO2-amino graphene composite material;

[0022] (4) The leather fiber was carboxylated by sodium chloroacetate, and the TiO2-amino graphene composite material was cross-linked with the carboxylated leather fiber using 3-glycidyloxypropyltrimethoxysilane as a cross-linking agent to obtain TiO2-amino graphene modified leather fiber.

[0023] Furthermore, the specific steps of performing carboxylation treatment on the leather fiber in step (4) are:

[0024] (1) Add 20-40 g of ammonium chloroacetate and 15-25 mL of water into a reaction kettle, stir to dissolve, and simultaneously dropwise add 20-60% potassium hydroxide solution to neutralize, to obtain sodium chloroacetate;

[0025] (2) 5-15 g of leather is immersed in 300-500 mL of deionized water for 10-12 h, and then placed in a water bath constant temperature oscillator for 5-7 h to obtain rewetted leather;

[0026] (3) adding the sodium chloroacetate obtained in step (1) to the rewetted leather obtained in step (2) to carry out a reaction at a temperature of 40-60° C. for 4-8 hours.

[0027] Furthermore, the cross-linking process of the TiO2-amino graphene composite material and the carboxylated leather fiber in step (4) is as follows:

[0028] The TiO2-amino graphene composite material and the 3-glycidyloxypropyltrimethoxysilane solution added to the modified leather fiber are stirred for reaction for 3-6 hours. After the reaction is completed, the mixture is filtered, washed with deionized water for 3-5 times, and dried.

[0029] Furthermore, in step (3), NaHCO3 is used to adjust the pH value of the system to maintain at 7-8.

[0030] The present invention has the following advantages:

[0031] 1. The TiO2-amino graphene modified leather fiber of the present application chemically modifies TiO2 so that it can be effectively combined with the leather fiber, and introduces amino graphene to improve the wear resistance of the leather fiber by utilizing its excellent mechanical strength; and the polyurethane foam foaming layer adopts thermoplastic polyurethane, propylene oxide, polyether polyol, dibutyl sebacate, foaming agent and thickener, which are evenly mixed and coated on the lower surface of the wear-resistant leather layer, and a foaming layer with good cushioning properties is formed through a foaming process, which not only increases the comfort of the leather, but also further improves the wear resistance.

[0032] 2. The TiO2-amino graphene composite material used in this application strengthens the connection between leather fibers through physical filling and chemical bonding, improves the overall strength and toughness of leather, and the two-dimensional planar structure of amino graphene can form effective bridges and supports between fibers, limiting the slippage and separation of fibers, and the introduction of amino graphene increases the crosslinking points between fibers, so that the fiber network can more effectively disperse stress when subjected to force and prevent the expansion of cracks. At the same time, the hardness and shear resistance of TiO2 nanoparticles also enhance the wear resistance and tear resistance of leather, and its filling effect increases the compactness of leather, reduces internal voids, and improves its ability to resist tensile damage. DETAILED DESCRIPTION

[0033] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The present invention provides a novel wear-resistant leather, comprising a base fabric layer, a foaming layer and a wear-resistant leather layer arranged on the base fabric layer;

[0035] The wear-resistant leather layer comprises the following components in parts by weight: 15-20 parts of TiO2-amino graphene modified leather fiber, 40-60 parts of polypropylene, 16-28 parts of polyisobutylene, 1-5 parts of plasticizer, 0.1-0.3 parts of antioxidant and 0.2-0.5 parts of antibacterial agent;

[0036] The foaming layer comprises the following components in parts by weight: 80-120 parts of thermoplastic polyurethane, 20-60 parts of propylene oxide, 16-30 parts of polyether polyol, 10-20 parts of dibutyl sebacate and 1-3 parts of foaming agent.

[0037] Specifically, the plasticizer is one or more of nano calcium carbonate, silicate, diisononyl sebacate, and tributyl citrate. Preferably, diisononyl sebacate is used in the present application.

[0038] Specifically, the antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)]pentaerythritol, bis(3,5-di-tert-butyl-4-hydroxyphenyl) sulfide, tris(2,4-di-tert-butylphenyl) phosphite, and dilauryl thiodipropionate. Preferably, dilauryl thiodipropionate is used in the present application.

[0039] Specifically, the antibacterial agent is a nano-silver antibacterial agent.

[0040] Specifically, the foaming agent is one or more of azodicarbonamide, ammonium bicarbonate or sodium bicarbonate; preferably, the present application uses azodicarbonamide.

[0041] The present invention provides a novel process for preparing wear-resistant leather, comprising the following steps:

[0042] S1. The formula amount of TiO2-amino graphene modified leather fiber, polypropylene, polyisobutylene, plasticizer, antioxidant and antibacterial agent is mixed and calendered to obtain a wear-resistant leather layer;

[0043] S2. The amount of thermoplastic polyurethane, propylene oxide, polyether polyol, dibutyl sebacate, foaming agent and thickener is mixed uniformly, and then the resulting mixed slurry is applied to the lower surface of the wear-resistant leather layer obtained in S1, foaming, calendering, to obtain a foaming layer;

[0044] S3. Bond the lower surface of the foaming layer to the base fabric layer to obtain a new type of wear-resistant leather.

[0045] Specifically, the preparation of TiO2-amino graphene modified leather fiber includes the following steps:

[0046] (1) dispersing graphene oxide-based nanoparticles in ethanol and heating them, then adding 3-aminopropyltrimethoxysilane APS, reflux reaction, centrifuging, washing with ethanol, and drying in an oven to obtain amino-modified graphene nanoparticles;

[0047] (2) dissolving tetrabutyl titanate in anhydrous ethanol, slowly dropping 30-60 mL of deionized water into the mixture under stirring conditions, and continuing the reaction for 1-3 hours after the mixture becomes a white emulsion to obtain nano-sized titanium dioxide powder, and then adding the nano-sized titanium dioxide powder into a peptizing agent to dissolve it to obtain a precursor solution;

[0048] (3) adding amino-modified graphene nanoparticles to a precursor solution, heating under reflux for reaction, filtering and washing a precipitate generated by the reaction, and finally sintering the precipitate at 300-600° C. in an inert atmosphere to obtain a TiO2-amino graphene composite material;

[0049] (4) The leather fiber was carboxylated by sodium chloroacetate, and the TiO2-amino graphene composite material was cross-linked with the carboxylated leather fiber using 3-glycidyloxypropyltrimethoxysilane as a cross-linking agent to obtain TiO2-amino graphene modified leather fiber.

[0050] Wherein, the specific steps of carboxylating the leather fiber in step (4) are:

[0051] (1) Add 20-40 g of ammonium chloroacetate and 15-25 mL of water into a reaction kettle, stir to dissolve, and simultaneously dropwise add 20-60% potassium hydroxide solution to neutralize, to obtain sodium chloroacetate;

[0052] (2) 5-15 g of leather is immersed in 300-500 mL of deionized water for 10-12 h, and then placed in a water bath constant temperature oscillator for 5-7 h to obtain rewetted leather;

[0053] (3) adding the sodium chloroacetate obtained in step (1) to the rewetted leather obtained in step (2) to carry out a reaction at a temperature of 40-60° C. for 4-8 hours.

[0054] Wherein, the cross-linking process of the TiO2-amino graphene composite material and the carboxylated leather fiber in step (4) is as follows:

[0055] The TiO2-amino graphene composite material and the 3-glycidyloxypropyltrimethoxysilane solution added to the modified leather fiber are stirred for reaction for 3-6 hours. After the reaction is completed, the mixture is filtered, washed with deionized water for 3-5 times, and dried.

[0056] Specifically, in step (3), NaHCO3 is used to adjust the pH value of the system to maintain at 7-8.

[0057] Example 1

[0058] This embodiment provides a preparation process of a novel wear-resistant leather, comprising the following steps:

[0059] S1. 20 g of TiO2-amino graphene-modified leather fiber, 60 g of polypropylene, 28 g of polyisobutylene, 5 g of diisononyl sebacate, 0.3 g of dilauryl thiodipropionate and 0.5 g of nano-silver antibacterial agent were mixed in an internal mixer at a mixing temperature of 150 ° C. After calendering, a wear-resistant leather layer was obtained;

[0060] S2. The formula amount of thermoplastic polyurethane 120g, propylene oxide 60g, polyether polyol 25g, dibutyl sebacate 20g, foaming agent 2.5g was mixed uniformly, and then the resulting mixed slurry was applied to the lower surface of the wear-resistant leather layer obtained in S1, foamed, calendered to obtain a foaming layer;

[0061] S3. Bond the lower surface of the foaming layer to the base fabric layer using acrylic glue to obtain a new type of wear-resistant leather.

[0062] Specifically, the preparation of TiO2-amino graphene modified leather fiber includes the following steps:

[0063] (1) 5 g of graphene oxide-based nanoparticles were dispersed in 30 g of ethanol, heated to 100° C., and then 1 wt % of 3-aminopropyltrimethoxysilane APS was added, refluxed for 3 h, centrifuged, washed with ethanol 3 times, and dried in an oven at 60° C. for 12 h to obtain amino-modified graphene nanoparticles;

[0064] (2) dissolving 10 mL of tetrabutyl titanate in 50 mL of anhydrous ethanol, slowly dropping 45 mL of deionized water into the mixture under stirring, stirring for 5 min and then continuing the reaction for 1 h to obtain nano-sized titanium dioxide powder, and then adding the nano-sized titanium dioxide powder into 30 mL of hydrogen peroxide solution to dissolve it, to obtain a precursor solution;

[0065] (3) adding 10 g of amino-modified graphene nanoparticles to 120 mL of the precursor solution, heating and refluxing for 10 h to react, filtering the generated precipitate and washing it with deionized water and ethanol, and finally sintering the precipitate at 600 ° C in an inert atmosphere to obtain a TiO2-amino graphene composite material;

[0066] (4) The leather fiber was carboxylated by sodium chloroacetate, and the TiO2-amino graphene composite material was cross-linked with the carboxylated leather fiber using 3-glycidyloxypropyltrimethoxysilane as a cross-linking agent to obtain TiO2-amino graphene modified leather fiber.

[0067] Specifically, the specific steps of carboxylating the leather fibers in step (4) are:

[0068] (1) adding 30 g of ammonium chloroacetate and 20 mL of water to a reaction kettle, stirring to dissolve, and slowly dropping a 30% potassium hydroxide solution for neutralization, stirring continuously during the dropping process and monitoring the pH value of the solution in real time until the pH value stabilizes in the range of 7-8, to obtain sodium chloroacetate;

[0069] (2) 15 g of leather was immersed in 500 mL of deionized water for 12 h to fully wet the leather and preliminarily remove possible impurities, and then placed in a water bath constant temperature oscillator set at 45° C. for 6 h to obtain rewetted leather;

[0070] (3) The sodium chloroacetate obtained in step (1) is added to the rewetted leather obtained in step (2) while stirring for reaction at a temperature of 50° C. The pH value of the system is adjusted to 7-8 with NaHCO3. NaHCO3 should be added slowly and stirred thoroughly. After reacting for 8 hours, carboxylated leather fibers are obtained.

[0071] Specifically, the cross-linking process of the TiO2-amino graphene composite material and the carboxylated leather fiber in step (4) is as follows:

[0072] The TiO2-amino graphene composite material and modified leather fiber were placed in a 100 mL beaker, and then 0.08 g / mL of 3-glycidyloxypropyltrimethoxysilane solution was added. The beaker was placed on a magnetic stirrer and stirred at 300 rpm for 6 hours. After the reaction, it was filtered using a Buchner funnel, washed with deionized water three times, and placed in a vacuum drying oven at 50°C until completely dried.

[0073] Example 2

[0074] This embodiment provides a preparation process of a novel wear-resistant leather, comprising the following steps:

[0075] S1. 17 g of TiO2-amino graphene-modified leather fiber, 60 g of polypropylene, 28 g of polyisobutylene, 5 g of diisononyl sebacate, 0.3 g of dilauryl thiodipropionate and 0.5 g of nano-silver antibacterial agent were mixed in an internal mixer at a mixing temperature of 150 ° C. After calendering, a wear-resistant leather layer was obtained;

[0076] S2. The formula amount of thermoplastic polyurethane 120g, propylene oxide 60g, polyether polyol 25g, dibutyl sebacate 20g, foaming agent 2.5g was mixed uniformly, and then the resulting mixed slurry was applied to the lower surface of the wear-resistant leather layer obtained in S1, foamed, calendered to obtain a foaming layer;

[0077] S3. Bond the lower surface of the foaming layer to the base fabric layer using acrylic glue to obtain a new type of wear-resistant leather.

[0078] Specifically, the preparation of TiO2-amino graphene modified leather fiber includes the following steps:

[0079] (1) 5 g of graphene oxide-based nanoparticles were dispersed in 30 g of ethanol, heated to 100° C., and then 1 wt % of 3-aminopropyltrimethoxysilane APS was added, refluxed for 3 h, centrifuged, washed with ethanol 3 times, and dried in an oven at 60° C. for 12 h to obtain amino-modified graphene nanoparticles;

[0080] (2) dissolving 10 mL of tetrabutyl titanate in 50 mL of anhydrous ethanol, slowly dropping 30 mL of deionized water into the mixture under stirring, stirring for 5 min and then continuing the reaction for 1 h to obtain nano-sized titanium dioxide powder, and then adding the nano-sized titanium dioxide powder into 30 mL of hydrogen peroxide solution to dissolve it, to obtain a precursor solution;

[0081] (3) adding 10 g of amino-modified graphene nanoparticles to 120 mL of the precursor solution, heating and refluxing for 10 h to react, filtering the generated precipitate and washing it with deionized water and ethanol, and finally sintering the precipitate at 600 ° C in an inert atmosphere to obtain a TiO2-amino graphene composite material;

[0082] (4) The leather fiber was carboxylated by sodium chloroacetate, and the TiO2-amino graphene composite material was cross-linked with the carboxylated leather fiber using 3-glycidyloxypropyltrimethoxysilane as a cross-linking agent to obtain TiO2-amino graphene modified leather fiber.

[0083] Specifically, the specific steps of carboxylating the leather fibers in step (4) are:

[0084] (1) adding 30 g of ammonium chloroacetate and 20 mL of water to a reaction kettle, stirring to dissolve, and slowly dropping a 30% potassium hydroxide solution for neutralization, stirring continuously during the dropping process and monitoring the pH value of the solution in real time until the pH value stabilizes in the range of 7-8, to obtain sodium chloroacetate;

[0085] (2) 15 g of leather was immersed in 500 mL of deionized water for 12 h to fully wet the leather and preliminarily remove possible impurities, and then placed in a water bath constant temperature oscillator set at 45° C. for 6 h to obtain rewetted leather;

[0086] (3) The sodium chloroacetate obtained in step (1) is added to the rewetted leather obtained in step (2) while stirring for reaction at a temperature of 50° C. The pH value of the system is adjusted to 7-8 with NaHCO3. NaHCO3 should be added slowly and stirred thoroughly. After reacting for 8 hours, carboxylated leather fibers are obtained.

[0087] Specifically, the cross-linking process of the TiO2-amino graphene composite material and the carboxylated leather fiber in step (4) is as follows:

[0088] The TiO2-amino graphene composite material and modified leather fiber were placed in a 100 mL beaker, and then 0.08 g / mL of 3-glycidyloxypropyltrimethoxysilane solution was added. The beaker was placed on a magnetic stirrer and stirred at 300 rpm for 6 hours. After the reaction, it was filtered using a Buchner funnel, washed with deionized water three times, and placed in a vacuum drying oven at 50°C until completely dried.

[0089] Example 3

[0090] This embodiment provides a preparation process of a novel wear-resistant leather, comprising the following steps:

[0091] S1. 15 g of TiO2-amino graphene-modified leather fiber, 60 g of polypropylene, 28 g of polyisobutylene, 5 g of diisononyl sebacate, 0.3 g of dilauryl thiodipropionate and 0.5 g of nano-silver antibacterial agent were mixed in an internal mixer at a mixing temperature of 150 ° C. After calendering, a wear-resistant leather layer was obtained;

[0092] S2. The formula amount of thermoplastic polyurethane 120g, propylene oxide 60g, polyether polyol 25g, dibutyl sebacate 20g, foaming agent 2.5g was mixed uniformly, and then the resulting mixed slurry was applied to the lower surface of the wear-resistant leather layer obtained in S1, foamed, calendered to obtain a foaming layer;

[0093] S3. Bond the lower surface of the foaming layer to the base fabric layer using acrylic glue to obtain a new type of wear-resistant leather.

[0094] Specifically, the preparation of TiO2-amino graphene modified leather fiber includes the following steps:

[0095] (1) 5 g of graphene oxide-based nanoparticles were dispersed in 30 g of ethanol, heated to 100° C., and then 1 wt % of 3-aminopropyltrimethoxysilane APS was added, refluxed for 3 h, centrifuged, washed with ethanol 3 times, and dried in an oven at 60° C. for 12 h to obtain amino-modified graphene nanoparticles;

[0096] (2) dissolving 10 mL of tetrabutyl titanate in 50 mL of anhydrous ethanol, slowly dropping 60 mL of deionized water into the mixture under stirring conditions, stirring for 5 min and then continuing the reaction for 1 h to obtain nano-sized titanium dioxide powder, and then adding the nano-sized titanium dioxide powder into 30 mL of hydrogen peroxide solution to dissolve it, to obtain a precursor solution;

[0097] (3) adding 10 g of amino-modified graphene nanoparticles to 120 mL of the precursor solution, heating and refluxing for 10 h to react, filtering the generated precipitate and washing it with deionized water and ethanol, and finally sintering the precipitate at 600 ° C in an inert atmosphere to obtain a TiO2-amino graphene composite material;

[0098] (4) The leather fiber was carboxylated by sodium chloroacetate, and the TiO2-amino graphene composite material was cross-linked with the carboxylated leather fiber using 3-glycidyloxypropyltrimethoxysilane as a cross-linking agent to obtain TiO2-amino graphene modified leather fiber.

[0099] Specifically, the specific steps of carboxylating the leather fibers in step (4) are:

[0100] (1) adding 30 g of ammonium chloroacetate and 20 mL of water to a reaction kettle, stirring to dissolve, and slowly dropping a 30% potassium hydroxide solution for neutralization, stirring continuously during the dropping process and monitoring the pH value of the solution in real time until the pH value stabilizes in the range of 7-8, to obtain sodium chloroacetate;

[0101] (2) 15 g of leather was immersed in 500 mL of deionized water for 12 h to fully wet the leather and preliminarily remove possible impurities, and then placed in a water bath constant temperature oscillator set at 45° C. for 6 h to obtain rewetted leather;

[0102] (3) The sodium chloroacetate obtained in step (1) is added to the rewetted leather obtained in step (2) while stirring for reaction at a temperature of 50° C. The pH value of the system is adjusted to 7-8 with NaHCO3. NaHCO3 should be added slowly and stirred thoroughly. After reacting for 8 hours, carboxylated leather fibers are obtained.

[0103] Specifically, the cross-linking process of the TiO2-amino graphene composite material and the carboxylated leather fiber in step (4) is as follows:

[0104] The TiO2-amino graphene composite material and modified leather fiber were placed in a 100 mL beaker, and then 0.08 g / mL of 3-glycidyloxypropyltrimethoxysilane solution was added. The beaker was placed on a magnetic stirrer and stirred at 300 rpm for 6 hours. After the reaction, it was filtered using a Buchner funnel, washed with deionized water three times, and placed in a vacuum drying oven at 50°C until completely dried.

[0105] Comparative Example 1: This example is used as a comparative example, and the TiO2-amino graphene modified leather fiber in Example 1 is replaced by leather fiber coated with polyurethane, and the other steps and parameters are the same as those in Example 1.

[0106] Comparative Example 2: This example is used as a comparative example, and the TiO2-amino graphene modified leather fiber in Example 1 is replaced by ordinary leather fiber, and the other steps and parameters are the same as those in Example 1.

[0107] Performance testing: Leather was tested for folding fastness (-20℃); Martindale abrasion resistance 200,000 times (10kPa); leather fabric tear strength was tested according to QB / T 2711-2005 "Determination of tear force in leather physical and mechanical tests: double-sided tearing"; and tensile strength was tested according to QB / T 2714 and QB / T 2726 physical and mechanical tests. The specific results are as follows:

[0108]

[0109] in conclusion:

[0110] 1. From the data of Examples 1-3 in the table, it can be seen that the wear-resistant leather prepared in Example 1 has the best performance. The detection performance of the samples obtained in Examples 2 and 3 decreases with the reduction of the amount of TiO2-amino graphene modified leather fiber used, proving that the introduction of TiO2-amino graphene composite material enhances the crosslinking and interaction between leather fibers, improves the stability and toughness of the overall structure, especially under low temperature (-20°C) conditions, its excellent thermal stability and cold brittleness resistance help to maintain the flexibility and resilience of the leather. The modification of leather fiber by TiO2-amino graphene composite material forms a protective layer on the surface of leather fiber, which improves the surface hardness and wear resistance. The introduction of TiO2 nanoparticles increases the surface roughness, reduces the friction coefficient, and makes the leather surface more difficult to be worn.

[0111] 2. From the data of Example 1 and Comparative Examples 1-2 in the table, it can be seen that the new wear-resistant leather prepared by the TiO2-amino graphene modified leather fiber in the present application has significantly improved the number of folding resistance at -20°C compared with the samples made from the unmodified ordinary leather fiber and the leather fiber coated with polyurethane, showing a stronger low-temperature bending resistance, reducing fatigue fracture and surface cracking caused by repeated folding, and extending the service life of leather products in low temperature environments. In the Martindale wear test, the new wear-resistant leather has significantly increased the number of abrasions under a pressure of 10kPa, showing a higher wear resistance. Even under long-term, high-intensity use conditions, its surface can still maintain good flatness and color, and is not prone to scratches and wear marks, which improves the appearance quality and durability of leather products.

[0112] The tear strength of the new wear-resistant leather is significantly improved, which means that under the same external force, its ability to resist crack expansion is enhanced, the crack width is reduced, and a greater force is required to tear it completely. In addition, its tensile strength is significantly improved, which means that under the same tensile rate, it can withstand greater tensile force without breaking.

[0113] In summary, the new wear-resistant leather exhibits excellent durability and functionality by significantly improving low-temperature folding resistance, abrasion resistance, tear strength and tensile strength, and is suitable for application scenarios with high standards for leather performance.

[0114] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.

Claims

1. A new type of wear-resistant leather, characterized in that: It comprises a base fabric layer, a foaming layer and a wear-resistant leather layer arranged on the base fabric layer; The wear-resistant leather layer comprises the following components in parts by weight: 15-20 parts of TiO2-amino graphene modified leather fiber, 40-60 parts of polypropylene, 16-28 parts of polyisobutylene, 1-5 parts of plasticizer, 0.1-0.3 parts of antioxidant and 0.2-0.5 parts of antibacterial agent; The foaming layer comprises the following components in parts by weight: 80-120 parts of thermoplastic polyurethane, 20-60 parts of propylene oxide, 16-30 parts of polyether polyol, 10-20 parts of dibutyl sebacate and 1-3 parts of foaming agent; The preparation of the TiO2-amino graphene modified leather fiber comprises the following steps: (1) dispersing graphene oxide-based nanoparticles in ethanol and heating them, then adding 3-aminopropyltrimethoxysilane APS, reflux reaction, centrifuging, washing with ethanol, and drying in an oven to obtain amino-modified graphene nanoparticles; (2) Dissolve tetrabutyl titanate in anhydrous ethanol, slowly add 30-60 mL of deionized water to the mixture under stirring, and continue to react for 1-3 hours after the mixture becomes a white emulsion to obtain nano-sized titanium dioxide powder, and then add the nano-sized titanium dioxide powder to a peptizing agent to dissolve it to obtain a precursor solution; (3) adding amino-modified graphene nanoparticles to a precursor solution, heating under reflux for reaction, filtering and washing a precipitate generated by the reaction, and finally sintering the precipitate at 300-600° C. in an inert atmosphere to obtain a TiO2-amino graphene composite material; (4) Carboxylating the leather fiber with sodium chloroacetate, and cross-linking the TiO2-amino graphene composite material with the carboxylated leather fiber using 3-glycidyloxypropyltrimethoxysilane as a cross-linking agent to obtain TiO2-amino graphene modified leather fiber; The specific steps of performing carboxylation treatment on leather fibers in (4) are as follows: A1. Add 20-40 g of ammonium chloroacetate and 15-25 mL of water to a reaction vessel, stir to dissolve, and then dropwise add 20-60% potassium hydroxide solution to neutralize to obtain sodium chloroacetate; A2. Soak 5-15g of leather in 300-500mL of deionized water for 10-12h, and then oscillate in a water bath thermostat oscillator for 5-7h to obtain rewet leather; A3. The sodium chloroacetate obtained in step A1 is added to the rewetted leather obtained in step A2 and reacted at a temperature of 40-60°C for 4-8h; In A3, NaHCO3 is used to adjust the pH value of the system to 7-8; The cross-linking process of the TiO2-amino graphene composite material and the carboxylated leather fiber in (4) is as follows: The TiO2-amino graphene composite material and the 3-glycidyloxypropyltrimethoxysilane solution added to the modified leather fiber are stirred for reaction for 3-6 hours. After the reaction is completed, the mixture is filtered, washed with deionized water for 3-5 times, and dried.

2. The novel wear-resistant leather according to claim 1, characterized in that: The plasticizer is one or more of nano calcium carbonate, silicate, diisononyl sebacate, and tributyl citrate.

3. The novel wear-resistant leather according to claim 1, characterized in that: The antioxidant is one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)]pentaerythritol, bis(3,5-di-tert-butyl-4-hydroxyphenyl)sulfide, tris(2,4-di-tert-butylphenyl)phosphite, and dilauryl thiodipropionate.

4. The novel wear-resistant leather according to claim 1, characterized in that: The antibacterial agent is a nano silver antibacterial agent.

5. The novel wear-resistant leather according to claim 2, characterized in that: The foaming agent is one or more of azodicarbonamide, ammonium bicarbonate or sodium bicarbonate.

6. A process for preparing the novel wear-resistant leather according to any one of claims 1 to 5, characterized in that: The steps include: S1. The formula amount of TiO2-amino graphene modified leather fiber, polypropylene, polyisobutylene, plasticizer, antioxidant and antibacterial agent is mixed and calendered to obtain a wear-resistant leather layer; S2. The amount of thermoplastic polyurethane, propylene oxide, polyether polyol, dibutyl sebacate, foaming agent and thickener is mixed uniformly, and then the resulting mixed slurry is applied to the lower surface of the wear-resistant leather layer obtained in S1, foaming, calendering, to obtain a foaming layer; S3. Bond the lower surface of the foaming layer to the base fabric layer to obtain a new type of wear-resistant leather.