Carbon-carbon thermal insulation board and preparation method thereof
By using a combination of carbon fiber chopped strands, graphite powder, epoxy resin sand and phenolic resin powder in the carbon insulation board, combined with gradient heating curing and carbonization treatment, the problems of low density and high thermal conductivity of the carbon insulation board are solved. Improved mechanical properties and thermal insulation effect, and reduced costs.
Patent Information
- Application Number
- CN202410874717.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-02
AI Technical Summary
Existing carbon insulation boards have low density and strength in high-temperature scenarios, and are not resistant to airflow erosion. They have high thermal conductivity and poor insulation effects.
A combination of chopped carbon fiber, graphite powder, epoxy resin sand and phenolic resin powder is used to form a low-density carbon insulation board through a gradient heating curing process and carbonization treatment, and coupling agents and dispersants are added to the raw materials to Improve pore structure and mechanical properties.
It achieves the low density, low thermal conductivity and high mechanical strength of the carbon insulation board, avoids failure caused by silicone liquid penetration and air flow impact, and reduces material costs.
Smart Images

Figure CN118405932B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation boards, and in particular to a carbon-carbon thermal insulation board and a preparation method thereof. Background Art
[0002] In recent years, solar energy and semiconductors have developed rapidly, and the production of these materials has a direct or indirect relationship with high-temperature furnaces and vacuum furnaces. In these fields, raw materials need to be treated at high temperatures, which is generally completed in high-temperature vacuum furnaces or inert gas protection furnaces. The temperature inside the high-temperature vacuum furnace is generally above 2000°C, and ordinary insulation materials cannot withstand such high temperatures. Carbon-carbon composite material is a new type of material that is tested in high-temperature scenes. Under the protection of inert gas, its maximum operating temperature is above 2000°C. Carbon-carbon composite materials are widely used as thermal insulation materials for high-temperature furnaces due to their low thermal conductivity.
[0003] There are two processes for carbon-to-carbon insulation in the prior art (such as Figure 1 As shown) are as follows:
[0004] I. Needle punching process of hard felt and insulation board
[0005] (a) Carbon-carbon thermal insulation hard felt needle punching process: Select carbon fiber raw fibers and cut them into short strands, which are then combed to obtain a mesh. Generally, 8 meshes are selected and laid in groups of 4 layers, with a total of 2 groups. After being neatly arranged, they are placed on a needle board for needle punching. Since the needles on the needle board have barbs, some fibers will be brought up and connected in the z direction of the mesh, thereby connecting the preform layers to form a whole. After a group of needle punching is completed, the next group of meshes is laid on the semi-finished products of the previous group of needle punching and continues to be needle punched until a whole product (called a preform) is obtained. The preform thickness is 5 mm and the gram weight is 560 g / m 2 .
[0006] (b) Needle punching process of carbon-carbon insulation board: Select carbon fiber raw yarn and cut it into short strands, and then comb it to get a mesh. Generally, 80 meshes and 20 carbon cloths are selected and combined, and 20 groups are laid in the order of 4 layers of mesh + 1 layer of carbon cloth. After being arranged, they are placed on the needle board for needle punching. Since the needles on the needle board have barbs, some fibers will be brought up and connected in the z direction of the mesh, thereby connecting the preform layers to form a whole. After a group of needling is completed, the next group of mesh is laid on the semi-finished product of the previous group and the needling is continued until a whole product is obtained.
[0007] II. Glue impregnation process of carbon-carbon thermal insulation hard felt and thermal insulation board:
[0008] (a) Dipping of carbon-carbon thermal insulation felt: First, spray the preform with a layer of low-viscosity phenolic resin (viscosity 30 cp, residual carbon rate 32%), dry the resin, and then coat the surface with a layer of high-viscosity phenolic resin (viscosity 6000 cp, residual carbon rate 52%). Then, according to the thickness requirements of the thermal insulation felt, stack them up in a certain number of layers.
[0009] (b) Carbon-carbon insulation board impregnation: The preform is pre-impregnated with phenolic resin (viscosity 6000 cp, residual carbon rate 52%).
[0010] III. Thermal curing process:
[0011] The stacked hard felt preform / carbon-carbon sheet preform impregnated with phenolic resin is placed in a mold, and the resin is cross-linked by a flat hot press to solidify the resin, thereby obtaining a carbon fiber resin hard felt (density 0.4~0.5g / cm 3 ) / Carbon fiber resin board (density 1.2~1.3 g / cm 3 ).
[0012] IV. Carbonization process:
[0013] The non-carbon elements (mainly oxygen and hydrogen) in the hot-pressed curing products are removed in the form of gas at a high temperature of 800-900℃; the density of the carbon-carbon thermal insulation felt after carbonization is (0.2~0.3 g / cm 3 ); the density of the carbonized carbon insulation board product is (0.9~1.0 g / cm 3 ).
[0014] However, the carbon-carbon thermal insulation hard felt prepared by the above method has low density and strength, and is not resistant to airflow erosion during use. Carbon-carbon thermal insulation board has greater strength than carbon-carbon thermal insulation hard felt and can withstand airflow erosion, but it has a high density and thermal conductivity, and its thermal insulation effect is not obvious.
[0015] In view of this, the present invention is proposed. Summary of the invention
[0016] The purpose of the present invention is to provide a carbon-carbon thermal insulation board and its preparation method and application. The carbon-carbon thermal insulation board prepared by the present invention forms a certain pore structure inside while ensuring low density, further reducing the thermal conductivity; in addition, the carbon-carbon thermal insulation board also has excellent mechanical strength.
[0017] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0018] In a first aspect, the present invention provides a carbon-carbon thermal insulation board, wherein the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0019] 30~40 pieces of carbon fiber chopped strands
[0020] Graphite powder 20~30 parts
[0021] Epoxy resin sand 20~25 parts
[0022] 20-30 parts of phenolic resin powder;
[0023] The content of carbon fiber chopped strands is 30 to 40 parts, for example, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, etc.
[0024] Among them, the content of graphite powder is 20-30 parts, for example, it can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, etc.
[0025] Among them, the content of epoxy resin sand is 20-25 parts, for example, it can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, etc.
[0026] Among them, the content of phenolic resin powder is 20-30 parts, for example, it can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, etc.
[0027] Among them, the residual carbon rate of the epoxy resin sand is below 15%, for example, it can be 15%, 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, etc.
[0028] Among them, the residual carbon rate of the phenolic resin powder is below 55%, for example, it can be 55%, 54%, 53%, 52%, 51%, 50%, 49%, 48%, 47%, 46%, 45%, 44%, 43%, 42%, 41%, 40%, 35%, 30%, etc.
[0029] In the present invention, a certain proportion of epoxy resin sand and phenolic resin powder are added to the raw materials for preparing the carbon-carbon thermal insulation board to replace the liquid resin coating process used in the past. The resin sand and resin powder have a certain particle size, so the substances lost in the subsequent thermal curing process can form pores inside the product, thereby achieving the purpose of reducing the thermal conductivity coefficient.
[0030] Furthermore, the present invention limits the residual carbon rate of the epoxy resin sand and phenolic resin powder, and the addition of epoxy resin sand and phenolic resin powder with a specific residual carbon rate can also improve the thermal insulation of the carbon-carbon insulation board relative to the carbon-carbon insulation felt, and improve the surface mechanical properties relative to the carbon-carbon insulation board, while ensuring that during use, it will not fail quickly due to the infiltration of silicone liquid, nor fail due to fluffing or stratification caused by the impact of airflow.
[0031] Preferably, the carbon fiber chopped strands are obtained by opening the leftovers of the carbon fiber preform.
[0032] Among them, "scraps of carbon fiber preforms" refers to the preforms of indefinite length left after cutting in the process of preparing carbon fiber preforms to obtain regular and fixed-length carbon fiber preforms. This preform is pure carbon fiber material and has not undergone any cross-linking treatment. Carbon fiber preforms refer to semi-finished products formed by carbon fiber precursors through weaving or needle punching processes.
[0033] In the present invention, the carbon fiber chopped strands selected as the raw materials for preparing the carbon-carbon thermal insulation board can be obtained from the scraps of the carbon fiber preform as described above, without necessarily using carbon fiber raw strands. These materials are relatively low in cost and can achieve waste recycling.
[0034] Preferably, the length of the carbon fiber chopped filaments is 10 to 30 mm, for example, it can be 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, 15 mm, 16 mm, 17 mm, 18 mm, 19 mm, 20 mm, 21 mm, 22 mm, 23 mm, 24 mm, 25 mm, 26 mm, 27 mm, 28 mm, 29 mm, 30 mm, etc.
[0035] Preferably, the particle size of the graphite powder is 1000-1200 mesh, for example, it can be 1000 mesh, 1020 mesh, 1040 mesh, 1060 mesh, 1080 mesh, 1100 mesh, 1120 mesh, 1140 mesh, 1160 mesh, 1180 mesh, 1200 mesh, etc.
[0036] In the present invention, the source of graphite powder selected in the raw material for preparing the carbon-carbon thermal insulation board can be made by crushing the scraps of graphite parts or graphitized carbon-carbon parts after processing. These materials are relatively low in cost and can achieve waste recycling.
[0037] Preferably, the particle size of the epoxy resin sand is 20-30 mesh, for example, it can be 20 mesh, 21 mesh, 22 mesh, 23 mesh, 24 mesh, 25 mesh, 26 mesh, 27 mesh, 28 mesh, 29 mesh, 30 mesh, etc.
[0038] Preferably, the particle size of the phenolic resin powder is 200-300 mesh, for example, it can be 200 mesh, 210 mesh, 220 mesh, 230 mesh, 240 mesh, 250 mesh, 260 mesh, 270 mesh, 280 mesh, 290 mesh, 300 mesh, etc.
[0039] Preferably, the raw materials for preparing the carbon-carbon thermal insulation board also include 1 to 10 parts of a coupling agent, for example, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.
[0040] Preferably, the coupling agent includes an aminosilane coupling agent and / or a long-chain silane coupling agent with a C10 or greater chain length, and preferably a mixture of an aminosilane coupling agent and a long-chain silane coupling agent with a C10 or greater chain length.
[0041] Preferably, the mass ratio of the aminosilane coupling agent to the long-chain silane coupling agent of C10 or more is (3-4):(2-1), for example, it can be 3:2, 3.2:1.8, 3.5:1.5, 3.8:1.2, 4:1, etc.
[0042] Preferably, the aminosilane coupling agent is selected from monoaminosilane coupling agents and / or polyaminosilane coupling agents, preferably polyaminosilane coupling agents.
[0043] Preferably, the monoaminosilane coupling agent is selected from γ- Aminopropyltrimethoxysilane and / or γ- Aminopropyltriethoxysilane.
[0044] Preferably, the polyaminosilane coupling agent is selected from diethylenetriaminopropyltrimethoxysilane, diethylenetriaminopropylmethyldimethoxysilane or N- Any one or a combination of at least two of (piperazinylethyl)-3-aminopropylmethyldimethoxysilane.
[0045] Preferably, the long-chain silane coupling agent with a C10 or higher content is selected from any one of dodecyltriethoxysilane, dodecyltriethoxysilane, hexadecyltriethoxysilane and octadecyltriethoxysilane, or a combination of at least two thereof.
[0046] In the present invention, a certain amount of coupling agent is further added to the raw materials for preparing the carbon-carbon thermal insulation board, and the carbon fiber chopped strands and graphite powder are coated and modified, so that the compatibility of the two inorganic and organic epoxy resin sand and phenolic resin powder is improved, ensuring that the pores formed later are more uniform. In addition, the selection of silane coupling agent and its ratio are further optimized, which is conducive to further reducing the thermal conductivity and can also significantly improve the mechanical strength of the obtained carbon-carbon thermal insulation board.
[0047] Preferably, the raw materials for preparing the carbon-carbon thermal insulation board also include 1 to 10 parts of a dispersant, for example, 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.
[0048] Preferably, the dispersant is selected from any one of polyvinyl pyrrolidone, polyoxyethylene lauryl ether or polyvinyl alcohol, or a combination of at least two thereof.
[0049] Preferably, the polyvinyl pyrrolidone is selected from any one of polyvinyl pyrrolidone K15, polyvinyl pyrrolidone K30 or polyvinyl pyrrolidone K60, or a combination of at least two thereof.
[0050] Preferably, the polyvinyl alcohol is selected from any one of PVA-1199, PVA-1399 or PVA-1799, or a combination of at least two thereof.
[0051] In the present invention, a dispersant is further added to the raw materials for preparing the carbon-carbon thermal insulation board, and the dispersant needs to be a polymer type dispersant, and the use of metal salt dispersants is avoided, which is beneficial to further ensure the dispersion effect of inorganic and organic matter, and is beneficial to further reduce the thermal conductivity coefficient, and can also make the mechanical strength of the obtained carbon-carbon thermal insulation board be more significantly improved.
[0052] Preferably, the density of the carbon-carbon insulation board is 0.5-0.6 g / cm 3 , for example, it can be 0.5 g / cm 3 , 0.51g / cm 3 , 0.52 g / cm 3 , 0.53 g / cm 3 , 0.54 g / cm 3 , 0.55 g / cm 3 , 0.56 g / cm 3 , 0.57 g / cm 3 , 0.58 g / cm 3 , 0.59 g / cm 3 , 0.6 g / cm 3 wait.
[0053] Preferably, the thermal conductivity of the carbon-carbon thermal insulation board is less than 0.8 W / (m·k), for example, it can be 0.8 W / (m·k), 0.75 W / (m·k), 0.7 W / (m·k), 0.65 W / (m·k), 0.6 W / (m·k), 0.55 W / (m·k), 0.54 W / (m·k), 0.53 W / (m·k), 0.52 W / (m·k), 0.5 W / (m·k), 0.49 W / (m·k), 0.48 W / (m·k), 0.45 W / (m·k), 0.4 W / (m·k), 0.35 W / (m·k), 0.3 W / (m·k), 0.25 W / (m·k), 0.2 W / (m·k), etc., preferably less than 0.52 W / (m·k), and more preferably 0.49~0.52 W / (m·k).
[0054] Preferably, the flexural strength of the carbon-carbon thermal insulation board is above 30 MPa, for example, it can be 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 55 MPa, 60 MPa, 62 MPa, 64 MPa, 66 MPa, 68 MPa, 70 MPa, 72 MPa, 74 MPa, 76 MPa, 78 MPa, 80 MPa, etc., preferably above 60 MPa, and more preferably 63~78 MPa.
[0055] In a second aspect, the present invention provides a method for preparing the carbon-carbon thermal insulation board material as described in the first aspect, the preparation method comprising the following steps:
[0056] Mixing: mixing the carbon fiber chopped strands, graphite powder, epoxy resin sand and phenolic resin powder in proportion to prepare a mixture;
[0057] Curing: curing the mixed material by heat preservation through a gradient temperature rising curing process to obtain a rough finished product;
[0058] Carbonization: Carbonizing the crude finished product to obtain the carbon-carbon thermal insulation board.
[0059] Preferably, the carbon fiber chopped strands are obtained by opening the scraps of the carbon fiber preform, and the opening specifically comprises the following steps: placing the scraps of the carbon fiber preform in an opener and opening them at a rotation speed of 300-400 r / min for 30-60 s.
[0060] Wherein, the opening speed is 300~400 r / min, for example, it can be 300 r / min, 310 r / min, 320 r / min, 330 r / min, 340 r / min, 350 r / min, 360 r / min, 370 r / min, 380 r / min, 390 r / min, 400 r / min, etc.
[0061] Wherein, the opening time is 30-60 s, for example, it can be 30 s, 35 s, 40 s, 45 s, 50 s, 55 s, 60 s, etc.
[0062] Preferably, the length of the nail roller in the opener is 5 to 7 cm, for example, it can be 5 cm, 5.5 cm, 6 cm, 6.5 cm, 7 cm, etc.
[0063] Preferably, the density of the nail roller in the opener is 0.1-0.2 nails / cm 2 , for example, it can be 0.1 root / cm 2 , 0.12 root / cm 2 , 0.14 root / cm 2 , 0.16 root / cm 2 , 0.18 root / cm 2 , 0.2 root / cm 2 wait.
[0064] In the present invention, due to the specific composition of the raw materials of the carbon-carbon insulation board and the use of a certain method to modify the carbon fiber chopped strands, the scraps of the carbon fiber preform can be used as the raw material, which has the advantage of further reducing the time required for opening compared to the carbon fiber precursor. This is because the precursor is generally agglomerated into clumps, which requires a longer time to disperse than the scraps, or requires a higher speed and a more dense setting of the nail rollers, otherwise the machined product will have the risk of edge collapse.
[0065] Preferably, the rotation speed of stirring and mixing the carbon fiber chopped strands, graphite powder, epoxy resin sand and phenolic resin powder is 60-70 r / min, for example, it can be 60 r / min, 62 r / min, 64 r / min, 66 r / min, 68 r / min, 70 r / min, etc.
[0066] Preferably, the stirring and mixing time of the carbon fiber chopped strands, graphite powder, epoxy resin sand and phenolic resin powder is 25 to 30 min, for example, it can be 25 min, 26 min, 27 min, 28 min, 29 min, 30 min, etc.
[0067] Preferably, the carbon fiber chopped strands and graphite powder are modified with a coupling agent and / or a dispersant before mixing, and the modification specifically includes the following steps:
[0068] The coupling agent and the dispersant are dispersed in ethanol to obtain a modified liquid; the carbon fiber chopped strands and graphite powder are immersed in the modified liquid, and then concentrated and dried to obtain a modified carbon fiber chopped strands and graphite powder mixture.
[0069] Preferably, the mass ratio of the coupling agent, the dispersant and the ethanol is (0-10):(0-10):100, for example, it can be 0:10:100, 1:9:100, 2:8:100, 3:7:100, 4:6:100, 5:5:100, 6:4:100, 7:3:100, 8:2:100, 9:1:100, 10:0:100, etc.
[0070] Preferably, the immersion temperature is 20-40°C, for example, 20°C, 25°C, 30°C, 35°C, 40°C, etc.
[0071] Preferably, the immersion time is 20 to 40 min, for example, 20 min, 25 min, 30 min, 35 min, 40 min, etc.
[0072] Preferably, the curing step is specifically as follows: after drying the mixed material, loading it into a mold, curing the mixed material by heat preservation through a gradient temperature rising curing process, and finally cooling it to room temperature for demoulding to obtain a rough finished product.
[0073] Preferably, the drying temperature of the mixture is 50-75°C, for example, it may be 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 68°C, 70°C, 72°C, 75°C, etc.
[0074] Preferably, the drying time of the mixture is 2 to 4 h, for example, it can be 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, 3.2 h, 3.4 h, 3.6 h, 3.8 h, 4 h, etc.
[0075] Preferably, the procedure of the gradient temperature rise curing process is specifically as follows:
[0076] First, the mixture is preheated at 85-95° C. and 0.2-0.4 MPa for 55-65 min;
[0077] Then, the first heat preservation treatment is carried out at 130-140°C and 4-6 MPa pressure for 25-35 min;
[0078] Finally, a second insulation treatment is carried out at 170-180°C and a pressure of 14-16 MPa for 115-125 min.
[0079] The temperature of the preheat treatment is 85-95°C, for example, 82°C, 86°C, 88°C, 90°C, 92°C, 94°C, 95°C, etc.
[0080] Among them, the pressure of the preheat treatment is 0.2~0.4 MPa, for example, it can be 0.2 MPa, 0.22 MPa, 0.24 MPa, 0.26 MPa, 0.28 MPa, 0.3 MPa, 0.32 MPa, 0.34 MPa, 0.36 MPa, 0.38 MPa, 0.4 MPa, etc.
[0081] The preheating time is 55 to 65 min, for example, 55 min, 56 min, 58 min, 60 min, 62 min, 64 min, 65 min, etc.
[0082] The first heat preservation treatment time is 130-140°C, for example, it can be 130°C, 132°C, 134°C, 136°C, 138°C, 140°C, etc.
[0083] Among them, the pressure of the first insulation treatment is 4~6 MPa, for example, it can be 4 MPa, 4.2 MPa, 4.4 MPa, 4.6 MPa, 4.8 MPa, 5 MPa, 5.2 MPa, 5.4 MPa, 5.6 MPa, 5.8 MPa, 6 MPa, etc.
[0084] The first heat preservation treatment time is 25 to 35 min, for example, 25 min, 26 min, 28 min, 30 min, 32 min, 34 min, 35 min, etc.
[0085] The second heat preservation treatment time is 170-180°C, for example, it can be 170°C, 172°C, 174°C, 176°C, 178°C, 180°C, etc.
[0086] Among them, the pressure of the second insulation treatment is 14~16 MPa, for example, it can be 14 MPa, 14.2 MPa, 14.4 MPa, 14.6 MPa, 14.8 MPa, 15 MPa, 15.2 MPa, 15.4 MPa, 15.6 MPa, 15.8 MPa, 16 MPa, etc.
[0087] The second heat preservation treatment time is 115-125 min, for example, it can be 115 min, 116 min, 118 min, 120 min, 122 min, 124 min, 125 min, etc.
[0088] Preferably, the density of the crude product is 0.8-0.9 g / cm 3 , for example, it can be 0.8 g / cm 3 , 0.82 g / cm 3 , 0.84 g / cm 3 , 0.86 g / cm 3 , 0.88 g / cm 3 , 0.9 g / cm 3 wait.
[0089] Preferably, the carbonization temperature is 780-820°C, for example, it may be 780°C, 785°C, 790°C, 795°C, 800°C, 805°C, 810°C, 815°C, 820°C, etc.
[0090] Preferably, the carbonization time is 60 to 120 min, for example, it can be 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, 90 min, 100 min, 105 min, 110 min, 115 min, 120 min, etc.
[0091] Preferably, the density of the carbon-carbon insulation board is 0.5-0.6 g / cm 3 , for example, it can be 0.5 g / cm 3 , 0.52g / cm 3 , 0.54 g / cm 3 , 0.56 g / cm 3 , 0.58 g / cm 3 , 0.6 g / cm 3 wait.
[0092] Compared with the prior art, the present invention has the following beneficial effects:
[0093] (1) The carbon-carbon insulation board of the present invention takes into account the advantages and disadvantages of both carbon-carbon insulation board and carbon-carbon insulation hard felt. The thermal insulation performance is improved compared with the carbon-carbon insulation felt, and the surface mechanical properties are improved compared with the carbon-carbon insulation board.
[0094] (2) The carbon-carbon insulation board of the present invention will not fail rapidly due to the infiltration of silicone liquid during use, nor will it fail due to fluffing or delamination caused by the impact of airflow.
[0095] (3) The carbon-carbon insulation board of the present invention uses scraps, graphite powder and epoxy resin sand as the main raw materials. These materials are relatively low in cost and can achieve waste recycling. The total material cost is reduced from 72 yuan / kg to 30 yuan / kg, and the product performance can still be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0096] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0097] Figure 1 The present invention is a process flow chart of two kinds of carbon-carbon insulation products in the prior art.
[0098] Figure 2 This is a process flow chart of the first preparation method of the carbon-carbon thermal insulation board material of the present invention.
[0099] Figure 3 This is a process flow chart of the second preparation method of the carbon-carbon thermal insulation board described in the present invention. DETAILED DESCRIPTION
[0100] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0101] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0102] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0103] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0104] The sources of the resin raw materials in the following examples are as follows:
[0105] Epoxy resin sand was purchased from Zhejiang Sandblasting Machinery Factory, model 20, particle size 20-30 mesh, and residual carbon rate 10%.
[0106] Phenolic resin powder was purchased from Hangmo New Materials Group Co., Ltd., model RD15, particle size 200-300 mesh, and residual carbon rate 50%.
[0107] Example 1
[0108] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0109] 40 pieces of carbon fiber chopped strands
[0110] Graphite powder 20 parts
[0111] Epoxy sand 20 parts
[0112] 20 parts of phenolic resin powder.
[0113] The preparation method of the carbon-carbon thermal insulation board (such as Figure 2 The specific steps include:
[0114] S1. Preprocessing:
[0115] S1-1 Preparation of carbon fiber chopped strands: Place the scraps of the carbon fiber preform in an opener and open it at a speed of 350 r / min for 45 s; wherein the length of the nail roller in the opener is 6 cm and the density is 0.1 strands / cm 2 , and obtained carbon fiber chopped strands with an average length of 20 mm.
[0116] S1-2 Preparation of graphite powder: The scraps of graphitized carbon-carbon parts after processing are crushed to obtain graphite powder with an average particle size of 1100 mesh.
[0117] S2. Mixing:
[0118] After carbon fiber chopped strands, graphite powder, epoxy resin sand and phenolic resin powder were weighed according to the above formula, the materials were put into a mixer and stirred at a speed of 60 r / min for 30 min to obtain a mixed material.
[0119] S3. Curing:
[0120] The mixture is first dried at 50°C for 2 h, then loaded into a mold, and preheated at 90°C and a pressure of 0.3 MPa for 60 min; then heat-insulated at 135°C and a pressure of 5 MPa for 30 min; finally heat-insulated at 175°C and a pressure of 15 MPa for 120 min, and finally cooled to room temperature for demolding to obtain a cured product.
[0121] S4, Carbonization:
[0122] The cured product is carbonized at 800° C. for 90 min to obtain the carbon-carbon thermal insulation board.
[0123] Example 2
[0124] This embodiment provides a carbon-carbon thermal insulation board, which is different from Example 1 only in that the content of the carbon fiber chopped strands is reduced to 35 parts, and the content of the phenolic resin powder is increased to 25 parts. Other components, contents and preparation methods are exactly the same as those in Example 1.
[0125] Example 3
[0126] This embodiment provides a carbon-carbon thermal insulation board, which is different from Example 1 only in that the content of the carbon fiber chopped strands is reduced to 30 parts, and the content of the phenolic resin powder is increased to 30 parts, and the other components, contents and preparation methods are exactly the same as those in Example 1.
[0127] Example 4
[0128] This embodiment provides a carbon-carbon thermal insulation board, which is different from Embodiment 1 only in that the content of the carbon fiber chopped strands is reduced to 35 parts, and the content of the graphite powder is increased to 25 parts. Other components, contents and preparation methods are exactly the same as those in Embodiment 1.
[0129] Example 5
[0130] This embodiment provides a carbon-carbon thermal insulation board, which is different from Example 1 only in that the content of the carbon fiber chopped strands is reduced to 30 parts, the content of the phenolic resin powder is increased to 25 parts, and the content of the graphite powder is increased to 25 parts. The other components, contents and preparation methods are exactly the same as those in Example 1.
[0131] Example 6
[0132] This embodiment provides a carbon-carbon thermal insulation board, which is different from Embodiment 1 only in that the content of the carbon fiber chopped strands is reduced to 30 parts, and the content of the graphite powder is increased to 30 parts, and the other components, contents and preparation methods are exactly the same as those in Embodiment 1.
[0133] Example 7
[0134] This embodiment provides a carbon-carbon thermal insulation board, which is different from Embodiment 1 only in that the content of the carbon fiber chopped strands is reduced to 35 parts, and the content of the epoxy resin sand is increased to 25 parts. Other components, contents and preparation methods are exactly the same as those in Embodiment 1.
[0135] Example 8
[0136] This embodiment provides a carbon-carbon thermal insulation board, which is different from Example 1 only in that the content of the carbon fiber chopped strands is reduced to 30 parts, the content of the phenolic resin powder is increased to 25 parts, and the content of the epoxy resin sand is increased to 25 parts. The other components, contents and preparation methods are exactly the same as those in Example 1.
[0137] Example 9
[0138] This embodiment provides a carbon-carbon thermal insulation board, which is different from Embodiment 1 only in that the content of the carbon fiber chopped strands is reduced to 30 parts, the content of the graphite powder is increased to 25 parts, and the content of the epoxy resin sand is increased to 25 parts. The other components, contents and preparation methods are exactly the same as those in Embodiment 1.
[0139] Example 10
[0140] This embodiment provides a carbon-carbon thermal insulation board, which is different from Embodiment 1 only in that the content of the carbon fiber chopped strands is reduced to 30 parts, and the content of the epoxy resin sand is increased to 30 parts, and the other components, contents and preparation methods are exactly the same as those in Embodiment 1.
[0141] Embodiment 11
[0142] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0143] 35 pieces of carbon fiber chopped strands
[0144] Graphite powder 20 parts
[0145] Epoxy sand 20 parts
[0146] 20 parts of phenolic resin powder
[0147] 3.5 parts of diethylenetriaminopropyltrimethoxysilane
[0148] 1.5 parts of dodecyltriethoxysilane.
[0149] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0150] S1. Preprocessing:
[0151] S1-1 Preparation of carbon fiber chopped strands: Place the leftovers of the carbon fiber preform in an opener and open it at a speed of 300 r / min for 50 s; wherein the length of the nail roller in the opener is 6 mm and the density is 0.2 strands / cm 2 , and obtained carbon fiber chopped strands with an average length of 20 mm.
[0152] S1-2 Preparation of graphite powder: The scraps of graphitized carbon-carbon parts after processing are crushed to obtain graphite powder with an average particle size of 1100 mesh.
[0153] S2. Modification treatment:
[0154] 3.5 parts of diethylenetriaminopropyltrimethoxysilane and 1.5 parts of dodecyltriethoxysilane were dissolved in 100 parts of ethanol to obtain an alcohol solution of silane; the carbon fiber chopped strands and graphite powder obtained in S1 were mixed in proportion, and then immersed in the alcohol solution of silane at 25°C for 30 min, and then concentrated and dried to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0155] S3, Mixing:
[0156] According to the above formula, the modified carbon fiber chopped strands and graphite powder mixture, epoxy resin sand and phenolic resin powder were weighed respectively, and the materials were put into a mixer and stirred at a speed of 60 r / min for 30 min to obtain a mixed material.
[0157] S4, curing:
[0158] The mixture is first dried at 50°C for 2 h, then loaded into a mold, and preheated at 90°C and a pressure of 0.3 MPa for 60 min; then heat-insulated at 135°C and a pressure of 5 MPa for 30 min; finally heat-insulated at 175°C and a pressure of 15 MPa for 120 min, and finally cooled to room temperature for demolding to obtain a cured product.
[0159] S5. Carbonization:
[0160] The cured product is carbonized at 800° C. for 90 min to obtain the carbon-carbon thermal insulation board.
[0161] Example 12
[0162] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0163] 30 pieces of carbon fiber chopped strands
[0164] Graphite powder 20 parts
[0165] Epoxy sand 20 parts
[0166] 25 parts of phenolic resin powder
[0167] 4 parts of diethylenetriaminepropylmethyldimethoxysilane
[0168] 1 part of hexadecyltriethoxysilane.
[0169] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0170] S1. Pretreatment: completely consistent with Example 11.
[0171] S2. Modification treatment:
[0172] 4 parts of diethylenetriaminopropylmethyldimethoxysilane and 1 part of hexadecyltriethoxysilane are dissolved in 100 parts of ethanol to obtain an alcohol solution of silane; the carbon fiber chopped strands and graphite powder obtained in S1 are mixed in proportion, and then immersed in the alcohol solution of silane at 35°C for 25 min, and then concentrated and dried to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0173] S3, mixing: completely the same as in Example 11.
[0174] S4. Curing: completely the same as Example 11.
[0175] S5. Carbonization: completely consistent with Example 11.
[0176] Embodiment 13
[0177] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0178] 30 pieces of carbon fiber chopped strands
[0179] Graphite powder 25 parts
[0180] Epoxy sand 20 parts
[0181] 20 parts of phenolic resin powder
[0182] N- 3 parts of (piperazine ethyl)-3-aminopropylmethyldimethoxysilane
[0183] 2 parts of octadecyltriethoxysilane.
[0184] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0185] S1. Pretreatment: completely consistent with Example 11.
[0186] S2. Modification treatment:
[0187] 3 portions N- (Piperazineethyl)-3-aminopropylmethyldimethoxysilane and 2 parts of octadecyltriethoxysilane are dissolved in 100 parts of ethanol to obtain an alcohol solution of silane; the carbon fiber chopped strands and graphite powder obtained in S1 are mixed in proportion, and then immersed in the alcohol solution of silane at 40°C for 20 min, and then concentrated and dried to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0188] S3, mixing: completely the same as in Example 11.
[0189] S4. Curing: completely the same as Example 11.
[0190] S5. Carbonization: completely consistent with Example 11.
[0191] Embodiment 14
[0192] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0193] 30 pieces of carbon fiber chopped strands
[0194] Graphite powder 20 parts
[0195] Epoxy sand 25 parts
[0196] 20 parts of phenolic resin powder
[0197] γ- 4 parts of aminopropyltrimethoxysilane
[0198] 1 part of dodecyltriethoxysilane.
[0199] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0200] S1. Pretreatment: completely consistent with Example 11.
[0201] S2. Modification treatment:
[0202] 4 portions γ- Aminopropyltrimethoxysilane and 1 part of dodecyltriethoxysilane are dissolved in 100 parts of ethanol to obtain an alcohol solution of silane; the carbon fiber chopped strands and graphite powder obtained in S1 are mixed in proportion, and then immersed in the alcohol solution of silane at 35°C for 25 min, and then concentrated and dried to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0203] S3, mixing: completely the same as in Example 11.
[0204] S4. Curing: completely the same as Example 11.
[0205] S5. Carbonization: completely consistent with Example 11.
[0206] Embodiment 15
[0207] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0208] 30 pieces of carbon fiber chopped strands
[0209] Graphite powder 20 parts
[0210] Epoxy sand 20 parts
[0211] 20 parts of phenolic resin powder
[0212] 8 parts of diethylenetriaminepropylmethyldimethoxysilane
[0213] 2 parts of hexadecyltriethoxysilane.
[0214] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0215] S1. Pretreatment: completely consistent with Example 11.
[0216] S2. Modification treatment:
[0217] 8 parts of diethylenetriaminopropylmethyldimethoxysilane and 2 parts of hexadecyltriethoxysilane are dissolved in 100 parts of ethanol to obtain an alcohol solution of silane; the carbon fiber chopped strands and graphite powder obtained in S1 are mixed in proportion, and then immersed in the alcohol solution of silane at 35°C for 25 min, and then concentrated and dried to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0218] S3, mixing: completely the same as in Example 11.
[0219] S4. Curing: completely the same as Example 11.
[0220] S5. Carbonization: completely consistent with Example 11.
[0221] Example 16
[0222] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0223] 35 pieces of carbon fiber chopped strands
[0224] Graphite powder 20 parts
[0225] Epoxy sand 20 parts
[0226] 20 parts of phenolic resin powder
[0227] Polyvinyl pyrrolidone K305 parts.
[0228] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0229] S1. Pretreatment: completely consistent with Example 11.
[0230] S2. Modification treatment:
[0231] Dissolve 5 parts of polyvinyl pyrrolidone K30 in 100 parts of ethanol to obtain an alcohol solution of K30; mix the carbon fiber chopped strands and graphite powder obtained in S1 in proportion, then immerse them in the alcohol solution of K30 at 30°C for 30 min, and then concentrate and dry them to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0232] S3, mixing: completely the same as in Example 11.
[0233] S4. Curing: completely the same as Example 11.
[0234] S5. Carbonization: completely consistent with Example 11.
[0235] Embodiment 17
[0236] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0237] 30 pieces of carbon fiber chopped strands
[0238] Graphite powder 20 parts
[0239] Epoxy sand 20 parts
[0240] 25 parts of phenolic resin powder
[0241] PVA-13995 copies.
[0242] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0243] S1. Pretreatment: completely consistent with Example 11.
[0244] S2. Modification treatment:
[0245] Dissolve 5 parts of PVA-1399 in 100 parts of ethanol to obtain an alcohol solution of PVA-1399; mix the carbon fiber chopped strands and graphite powder obtained in S1 in proportion, then immerse them in the alcohol solution of PVA-1399 at 30°C for 30 min, and then concentrate and dry to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0246] S3, mixing: completely the same as in Example 11.
[0247] S4. Curing: completely the same as Example 11.
[0248] S5. Carbonization: completely consistent with Example 11.
[0249] Embodiment 18
[0250] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0251] 30 pieces of carbon fiber chopped strands
[0252] Graphite powder 25 parts
[0253] Epoxy sand 20 parts
[0254] 20 parts of phenolic resin powder
[0255] Polyvinyl pyrrolidone K605 parts.
[0256] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0257] S1. Pretreatment: completely consistent with Example 11.
[0258] S2. Modification treatment:
[0259] Dissolve 5 parts of polyvinyl pyrrolidone K60 in 100 parts of ethanol to obtain an alcohol solution of polyvinyl pyrrolidone K60; mix the carbon fiber chopped strands and graphite powder obtained in S1 in proportion, then immerse them in the alcohol solution of polyvinyl pyrrolidone K60 at 30°C for 30 min, and then concentrate and dry to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0260] S3, mixing: completely the same as in Example 11.
[0261] S4. Curing: completely the same as Example 11.
[0262] S5. Carbonization: completely consistent with Example 11.
[0263] Embodiment 19
[0264] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0265] 30 pieces of carbon fiber chopped strands
[0266] Graphite powder 20 parts
[0267] Epoxy sand 25 parts
[0268] 20 parts of phenolic resin powder
[0269] PVA - 17995 copies.
[0270] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0271] S1. Pretreatment: completely consistent with Example 11.
[0272] S2. Modification treatment:
[0273] Dissolve 5 parts of PVA-1799 in 100 parts of ethanol to obtain an alcohol solution of PVA-1799; mix the carbon fiber chopped strands and graphite powder obtained in S1 in proportion, then immerse them in the alcohol solution of PVA-1799 at 30°C for 30 min, and then concentrate and dry to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0274] S3, mixing: completely the same as in Example 11.
[0275] S4. Curing: completely the same as Example 11.
[0276] S5. Carbonization: completely consistent with Example 11.
[0277] Embodiment 20
[0278] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0279] 30 pieces of carbon fiber chopped strands
[0280] Graphite powder 20 parts
[0281] Epoxy sand 20 parts
[0282] 20 parts of phenolic resin powder
[0283] Polyvinyl pyrrolidone K30 10 parts.
[0284] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0285] S1. Pretreatment: completely consistent with Example 11.
[0286] S2. Modification treatment:
[0287] 10 parts of polyvinyl pyrrolidone K30 are dissolved in 100 parts of ethanol to obtain an alcohol solution of K30; the carbon fiber chopped strands and graphite powder obtained in S1 are mixed in proportion, and then immersed in the alcohol solution of K30 at 30°C for 30 min, and then concentrated and dried to obtain a modified mixture of carbon fiber chopped strands and graphite powder.
[0288] S3, mixing: completely the same as in Example 11.
[0289] S4. Curing: completely the same as Example 11.
[0290] S5. Carbonization: completely consistent with Example 11.
[0291] Embodiment 21
[0292] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0293] 30 pieces of carbon fiber chopped strands
[0294] Graphite powder 20 parts
[0295] Epoxy sand 20 parts
[0296] 20 parts of phenolic resin powder
[0297] 3.5 parts of diethylenetriaminopropyltrimethoxysilane
[0298] 1.5 parts of dodecyltriethoxysilane
[0299] Polyvinyl pyrrolidone K305 parts.
[0300] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0301] S1. Preprocessing:
[0302] S1-1 Preparation of carbon fiber chopped strands: Place the leftovers of the carbon fiber preform in an opener and open it at a speed of r / min; wherein the length of the nail roller in the opener is mm and the density is root / cm 2 , and obtained carbon fiber chopped strands with an average length of 20 mm.
[0303] S1-2 Preparation of graphite powder: The scraps of graphitized carbon-carbon parts after processing are crushed to obtain graphite powder with an average particle size of 1100 mesh.
[0304] S2. Modification treatment:
[0305] 3.5 parts of diethylenetriaminopropyltrimethoxysilane, 1.5 parts of dodecyltriethoxysilane and 5 parts of are dissolved in 100 parts of ethanol to obtain an alcohol solution; the carbon fiber chopped strands and graphite powder obtained in S1 are mixed in proportion, and then immersed in the alcohol solution at 30°C for 30 min, and then concentrated and dried to obtain a modified carbon fiber chopped strands and graphite powder mixture.
[0306] S3, Mixing:
[0307] According to the above formula, the modified carbon fiber chopped strands and graphite powder mixture, epoxy resin sand and phenolic resin powder were weighed respectively, and the materials were put into a mixer and stirred at a speed of 60 r / min for 30 min to obtain a mixed material.
[0308] S4, curing:
[0309] The mixture is first dried at 50°C for 2 h, then loaded into a mold, and preheated at 90°C and a pressure of 0.3 MPa for 60 min; then heat-insulated at 135°C and a pressure of 5 MPa for 30 min; finally heat-insulated at 175°C and a pressure of 15 MPa for 120 min, and finally cooled to room temperature for demolding to obtain a cured product.
[0310] S5. Carbonization:
[0311] The cured product is carbonized at 800° C. for min to obtain the carbon-carbon thermal insulation board.
[0312] Embodiment 22
[0313] This embodiment provides a carbon-carbon thermal insulation board, which is different from Embodiment 21 only in that the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0314] 30 pieces of carbon fiber chopped strands
[0315] Graphite powder 20 parts
[0316] Epoxy sand 20 parts
[0317] 20 parts of phenolic resin powder
[0318] 3 parts of diethylenetriaminepropylmethyldimethoxysilane
[0319] 2 parts of hexadecyltriethoxysilane
[0320] Polyvinyl pyrrolidone K605 parts.
[0321] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0322] S1. Pretreatment: completely consistent with Example 21.
[0323] S2. Modification treatment:
[0324] 3 parts of diethylenetriaminopropylmethyldimethoxysilane, 2 parts of hexadecyltriethoxysilane, and 5 parts of polyvinylpyrrolidone K60 are dissolved in 100 parts of ethanol to obtain an alcohol solution; the carbon fiber chopped strands and graphite powder obtained in S1 are mixed in proportion, and then immersed in the alcohol solution at 30°C for 30 min, and then concentrated and dried to obtain a modified carbon fiber chopped strands and graphite powder mixture.
[0325] S3, mixing: completely the same as Example 21.
[0326] S4. Curing: completely consistent with Example 21.
[0327] S5. Carbonization: completely consistent with Example 21.
[0328] Embodiment 23
[0329] This embodiment provides a carbon-carbon thermal insulation board, which is different from Embodiment 21 only in that the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0330] 30 pieces of carbon fiber chopped strands
[0331] Graphite powder 20 parts
[0332] Epoxy sand 20 parts
[0333] 20 parts of phenolic resin powder
[0334] 4 parts of diethylenetriaminepropylmethyldimethoxysilane
[0335] 1 part of dodecyltriethoxysilane
[0336] Polyvinyl pyrrolidone K305 parts.
[0337] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0338] S1. Pretreatment: completely consistent with Example 21.
[0339] S2. Modification treatment:
[0340] 4 parts of diethylenetriaminopropylmethyldimethoxysilane, 1 part of dodecyltriethoxysilane, and 5 parts of polyvinylpyrrolidone K30 are dissolved in 100 parts of ethanol to obtain an alcohol solution; the carbon fiber chopped strands and graphite powder obtained in S1 are mixed in proportion, and then immersed in the alcohol solution at 30°C for 30 min, and then concentrated and dried to obtain a modified carbon fiber chopped strands and graphite powder mixture.
[0341] S3, mixing: completely the same as Example 21.
[0342] S4. Curing: completely consistent with Example 21.
[0343] S5. Carbonization: completely consistent with Example 21.
[0344] Embodiment 24
[0345] This embodiment provides a carbon-carbon thermal insulation board, and the raw materials for preparing the carbon-carbon thermal insulation board include the following components in parts by weight:
[0346] 30 pieces of carbon fiber chopped strands
[0347] Graphite powder 20 parts
[0348] Epoxy sand 20 parts
[0349] 20 parts of phenolic resin powder
[0350] 3.5 parts of diethylenetriaminopropyltrimethoxysilane
[0351] 1.5 parts of dodecyltriethoxysilane
[0352] Polyvinyl pyrrolidone K305 parts.
[0353] The preparation method of the carbon-carbon thermal insulation board (such as Figure 3 The specific steps include:
[0354] S1. Pretreatment: completely consistent with Example 21.
[0355] S2. Mixing:
[0356] According to the above formula, carbon fiber chopped strands, graphite powder, epoxy resin sand, phenolic resin powder, diethylenetriaminopropyltrimethoxysilane, dodecyltriethoxysilane and polyvinylpyrrolidone K30 were weighed respectively, and then the materials were put into a mixer and stirred at a speed of 70 r / min for 1 h to obtain a mixture.
[0357] S3, mixing: completely the same as Example 21.
[0358] S4. Curing: completely consistent with Example 21.
[0359] S5. Carbonization: completely consistent with Example 21.
[0360] Comparative Example 1
[0361] This comparative example provides a carbon-carbon thermal insulation board, which is different from Example 1 only in that epoxy resin sand is not added, the content of phenolic resin powder is increased to 40 parts, and other components, contents and preparation methods are completely consistent with Example 1.
[0362] Comparative Example 2
[0363] This comparative example provides a carbon-carbon thermal insulation board, which is different from Example 1 only in that phenolic resin powder is not added, the epoxy resin sand content is increased to 40 parts, and other components, contents and preparation methods are completely consistent with Example 1.
[0364] Comparative Example 3
[0365] This comparative example provides a carbon-carbon thermal insulation board, which is different from Example 1 only in that the epoxy resin sand is replaced with an equal mass of wet hand-laid epoxy laminating resin (composite material is easy to buy, model EL-2), and the other components, contents and preparation methods are exactly the same as those in Example 1.
[0366] Comparative Example 4
[0367] This comparative example provides a carbon-carbon thermal insulation board, which is different from Example 1 only in that the phenolic resin powder is replaced with an equal mass of phenolic resin (thermosetting resin, Shengquan, EXP0371, viscosity 30 cp, residual carbon 32%), and the other components, contents and preparation methods are exactly the same as those in Example 1.
[0368] Test Case
[0369] Test samples: carbon-carbon thermal insulation boards provided in Examples 1 to 24, and carbon-carbon thermal insulation boards provided in Comparative Examples 1 to 4;
[0370] Test items:
[0371] (1) Density: The test method is GB / T1033.2-2010 "Determination of density of non-foamed plastics"; the test instrument is a water displacement density tester;
[0372] (2) Thermal conductivity: Testing method: YB / T4130-2005 "Test method for thermal conductivity of refractory materials"; testing instrument: thermal conductivity tester;
[0373] (3) Bending strength: The testing method is GB / T1449_2005 “Test method for bending properties of fiber reinforced plastics”; the testing instrument is a universal testing machine.
[0374] The test results are shown in Table 1 below:
[0375] Table 1
[0376]
[0377] As shown in Table 1, the density of the finished carbon-carbon thermal insulation board prepared by the present invention is 0.5-0.6 g / cm 3 , the thermal conductivity can reach below 0.52 W / (m·k), and the bending strength can reach above 60 MPa. This shows that the carbon-carbon thermal insulation board prepared by the present invention forms a certain pore structure inside while ensuring low density, further reducing the thermal conductivity; in addition, the carbon-carbon thermal insulation board also has excellent mechanical strength.
[0378] From the comparison between Example 1 and Comparative Examples 1-2, it can be seen that a certain proportion of epoxy resin sand and phenolic resin powder are added to the raw materials for preparing the carbon-carbon thermal insulation board to replace the liquid resin coating process used in the past. The resin sand and resin powder have a certain particle size, so the substances lost in the subsequent thermal curing process can form pores inside the product, thereby achieving the purpose of reducing the thermal conductivity.
[0379] From the comparison between Example 1 and Comparative Examples 3-4, it can be seen that the epoxy resin sand and phenolic resin powder not used in this application are used, and the epoxy resin and phenolic resin commonly used in the field are selected. Since the epoxy resin and phenolic resin are liquids with a certain viscosity, their dry mixing will cause agglomeration and condensation on the surface of part of the carbon fiber, making it impossible to fully disperse the carbon fiber and graphite, and thus the mechanical strength cannot be further improved. In addition, the residual carbon rate of these two resins is not within the preferred range of this application, resulting in the inability to form pores well inside, and the thermal conductivity is high.
[0380] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a carbon-carbon thermal insulation board, It is characterized in that The preparation method comprises the following steps: Mixing: Mixing the modified carbon fiber chopped strands and the graphite powder mixture, epoxy resin sand and phenolic resin powder in proportion to prepare a mixture; The specific steps of the modification are: dispersing a coupling agent and a dispersant in ethanol to obtain a modified solution; immersing carbon fiber chopped strands and graphite powder in the modified solution, and then concentrating and drying to obtain a modified mixture of carbon fiber chopped strands and graphite powder; Curing: curing the mixed material by heat preservation through a gradient temperature rising curing process to obtain a rough finished product; Carbonization: carbonizing the crude finished product to obtain the carbon-carbon thermal insulation board; The raw materials for preparing the carbon-carbon thermal insulation board include the following components by weight: 30~40 pieces of carbon fiber chopped strands Graphite powder 20~30 parts Epoxy resin sand 20~25 parts 20~30 parts of phenolic resin powder Coupling agent 1~10 parts Dispersant 1~10 parts; Wherein, the residual carbon rate of the epoxy resin sand is less than 15%; the residual carbon rate of the phenolic resin powder is less than 55%; Wherein, the coupling agent is a combination of an aminosilane coupling agent and a long-chain silane coupling agent of C10 or more in a mass ratio of (3-4):(2-1); Wherein, the dispersant is selected from any one of polyvinyl pyrrolidone, polyoxyethylene lauryl ether or polyvinyl alcohol, or a combination of at least two thereof.
2. The method for preparing the carbon-carbon thermal insulation board according to claim 1, It is characterized in that The carbon fiber chopped strands are obtained by opening the leftovers of the carbon fiber preform; And / or, the length of the carbon fiber chopped strands is 10-30 mm.
3. The method for preparing the carbon-carbon thermal insulation board according to claim 1, It is characterized in that The particle size of the graphite powder is 1000-1200 mesh; And / or, the particle size of the epoxy resin sand is 20-30 mesh; And / or, the particle size of the phenolic resin powder is 200-300 meshes.
4. The method for preparing the carbon-carbon thermal insulation board according to claim 1, It is characterized in that The aminosilane coupling agent is selected from monoaminosilane coupling agent and / or polyaminosilane coupling agent; the monoaminosilane coupling agent is selected from γ- Aminopropyltrimethoxysilane and / or γ- Aminopropyltriethoxysilane; the polyaminosilane coupling agent is selected from diethylenetriaminopropyltrimethoxysilane, diethylenetriaminopropylmethyldimethoxysilane or N- Any one or a combination of at least two of (piperazinylethyl)-3-aminopropylmethyldimethoxysilane; Wherein, the long-chain silane coupling agent with C10 or above is selected from any one of dodecyltriethoxysilane, dodecyltriethoxysilane, hexadecyltriethoxysilane and octadecyltriethoxysilane, or a combination of at least two thereof.
5. The method for preparing the carbon-carbon thermal insulation board according to claim 1, It is characterized in that The polyvinyl pyrrolidone is selected from any one of polyvinyl pyrrolidone K15, polyvinyl pyrrolidone K30 or polyvinyl pyrrolidone K60, or a combination of at least two thereof; Wherein, the polyvinyl alcohol is selected from any one of PVA-1199, PVA-1399 or PVA-1799 or a combination of at least two thereof.
6. The method for preparing the carbon-carbon thermal insulation board according to claim 1, It is characterized in that The density of the carbon-carbon insulation board is 0.5-0.6 g / cm 3 ; The thermal conductivity of the carbon-carbon thermal insulation board is less than 0.52 W / (m·k); The carbon-carbon thermal insulation board has a bending strength of more than 72 MPa.
7. The method for preparing the carbon-carbon thermal insulation board according to claim 1, It is characterized in that The carbon fiber chopped strands are obtained by opening the scraps of the carbon fiber preform, and the opening specifically comprises the following steps: The scraps of the carbon fiber preform are placed in an opening machine and opened at a speed of 300-400 r / min for 30-60 s; The length of the nail roller in the opener is 5-7 cm, and the density of the nail roller in the opener is 0.1-0.2 nails / cm 2 .
8. The method for preparing the carbon-carbon thermal insulation board according to claim 1, It is characterized in that The stirring and mixing speed is 60-70 r / min, and the stirring and mixing time is 25-30 min; And / or, the mass ratio of the coupling agent, the dispersant and the ethanol is (5-10):(5-10):100; And / or, the immersion temperature is 20-40° C., and the immersion time is 20-40 min.
9. The method for preparing the carbon-carbon thermal insulation board according to claim 1, It is characterized in that The curing step specifically comprises: drying the mixed material and placing it into a mold, curing the mixed material by heat preservation through a gradient temperature rise curing process, and finally cooling it to room temperature for demoulding to obtain a rough finished product; And / or, the drying temperature of the mixture is 50-75° C., and the drying time of the mixture is 2-4 h; And / or, the procedure of the gradient temperature rise curing process is specifically as follows: First, the mixture is preheated at 85-95° C. and a pressure of 0.2-0.4 MPa for 55-65 min; then, it is heat-insulated at 130-140° C. and a pressure of 4-6 MPa for 25-35 min; and finally, it is heat-insulated at 170-180° C. and a pressure of 14-16 MPa for 115-125 min; And / or, the density of the crude finished product is 0.8-0.9 g / cm 3 ; And / or, the carbonization temperature is 780-820° C., and the carbonization time is 60-120 min; And / or, the density of the carbon-carbon insulation board is 0.5-0.6 g / cm 3 .
Citation Information
Patent Citations
Ultra-high-strength graphene modified engineering plastic and preparation method thereof
CN109082085A
Carbon-carbon composite material slab suitable for hot-press approach quick preparation, and preparation method thereof
CN109437956A
Carbon-plastic composite board
CN110669274A
Preparation method of carbon-carbon composite material plate
CN111039691A
Carbon-based material for thermal insulation device
CN111763096A