Wide temperature range anti-oxidation coating on the surface of carbon aerogel composite material and preparation method at room temperature

By using dual-resin polymeric powder technology to prepare a resin-ceramic powder coating on the surface of carbon airgel composite materials, the problem of insufficient anti-oxidation performance of the material in the 600-1200°C range is solved, and normal temperature preparation and high-efficiency anti-oxidation are achieved , maintaining the material’s low thermal conductivity and high strength.

CN118405942BActive Publication Date: 2024-10-29INST OF METAL RESEARCH - CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410852380.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Carbon airgel composite materials have a fast oxidation rate in high temperature and aerobic environments. Existing anti-oxidation coatings are mainly prepared at high temperatures, resulting in an increase in the thermal conductivity of the material, and the existing coatings have anti-oxidation properties in a wide temperature range. Insufficient, especially the lack of effective protection in the 600-1200°C range.

Method used

Dual-resin polymerized powder technology is used to prepare resin-ceramic powder coating at room temperature. The viscosity and cohesion of the resin are used to form a dense combination. The ceramic powder wrapping structure is closely combined with the surface of the carbon airgel composite material to achieve 600-1200 °C wide temperature range anti-oxidation.

Benefits of technology

This method does not require high-temperature heat treatment, avoids an increase in thermal conductivity, and achieves high-efficiency oxidation resistance of carbon airgel composite materials in the range of 600-1200°C, with the material's bending strength retention rate exceeding 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118405942B_ABST
    Figure CN118405942B_ABST
Patent Text Reader

Abstract

The invention discloses a wide temperature range anti-oxidation coating on the surface of a carbon aerogel composite material (C / CA) and a method for preparing the same at room temperature, and belongs to the technical field of anti-oxidation coatings for porous carbon materials. The invention adopts a dual resin polymer powder technology to realize the room temperature preparation of a dense coating on the surface of C / CA. The method uniformly coats the surface of a carbon aerogel composite material with a ceramic powder-resin slurry, dries it at room temperature, and utilizes the viscosity of the resin and its cohesive force during the drying process to form a tight bond between the ceramic powder and the surface of C / CA. During service, the synergy of the oxidation expansion self-sealing of the ceramic phase and the flow self-healing of the glass phase realizes wide temperature range anti-oxidation. Compared with the traditional coating preparation technology, the room temperature preparation method does not have a high temperature heat treatment process, effectively avoiding the increase of the thermal conductivity of the C / CA substrate, and the obtained coating realizes 600-1200ºC wide temperature range anti-oxidation, and the bending strength retention rate of the material after oxidation at 1200ºC for 2h exceeds 90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-oxidation coatings on the surface of porous carbon materials, and in particular to a wide-temperature range anti-oxidation coating on the surface of a carbon aerogel composite material and a method for preparing the coating at room temperature. Background Art

[0002] Carbon fiber reinforced carbon aerogel composite (C / CA, referred to as carbon aerogel composite) is a porous carbon material with carbon fiber as reinforcement and carbon aerogel (CA) as matrix. It can simultaneously have low density, low thermal conductivity, high strength and toughness and high temperature stability. As a new type of ultra-high temperature thermal insulation-load-bearing integrated material, it shows great application prospects in the thermal protection of high-speed aircraft and their power systems.

[0003] However, the initial oxidation temperature of carbon aerogel composites is low (about 350ºC), and the porous structure causes its oxidation rate to be faster than that of traditional graphite, carbon / carbon composites, etc., which greatly limits the application of such materials in high-temperature, oxygen-containing environments. Preparing an anti-oxidation coating on the surface of the material can effectively isolate oxygen from diffusing into the porous carbon structure, which is an effective means to improve the anti-oxidation performance of such materials. There are few reports on the research of anti-oxidation coatings on the surface of porous carbon material structures, which mainly include the preparation of ceramic coatings by gas-solid reaction of silicon and carbon at high temperature, the preparation of ceramic coatings by high-temperature plasma spraying, and the preparation of ceramic-glass coatings by rapid sintering in a high-temperature micro-oxygen environment. On the one hand, the substrates in the preparation process of the above methods must undergo high-temperature treatment of at least 1400 ºC. During this process, the crystallinity of the carbon aerogel matrix and carbon fiber will be greatly improved, thereby increasing the thermal conductivity of the material and reducing its thermal insulation ability. On the other hand, when C / CA is used as a thermal insulation material, it cannot avoid oxidation despite the heat-proof panel on its surface. Its excellent thermal insulation performance brings a huge temperature gradient, which may reach more than 2000°C on the front side and usually less than 200°C on the back side. Therefore, the static oxidation problem of C / CA cannot be ignored. The coatings reported so far mainly improve the ablation resistance of C / CA above 1500°C, and there are few reports on its anti-oxidation performance in a wider temperature range.

[0004] In order to fill the gap in the research on the oxidation resistance of C / CA in the medium and low temperature range below 1200°C, the present invention proposes a new resin-ceramic powder coating system, and invents a method for preparing a dense coating on the surface of C / CA at room temperature using dual resin polymerization powder technology. The coating prepared by this method can achieve oxidation resistance in a wide temperature range of 600-1200°C. Summary of the invention

[0005] The purpose of the present invention is to provide a wide temperature range anti-oxidation coating on the surface of a carbon aerogel composite material (C / CA) and a method for preparing the same at room temperature. The coating prepared by the method can protect C / CA from oxidation at 600-1200°C, effectively filling the gap of anti-oxidation coating on the surface of C / CA in the range of 600-1200°C. The coating uses the viscosity of the resin and its cohesive force during the drying process to make the ceramic powder form a tight bond at room temperature and adhere to the surface of C / CA. This process does not increase the thermal conductivity of C / CA, and the resin-ceramic powder component, thickness, and density in the coating are easy to control, and the coating has a high bonding strength with the C / CA substrate.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] (1) Carbon fiber reinforced carbon aerogel composite material (density 0.2-1.0g / cm 3 ) cut into the required shape, then polish with 800-grit sandpaper, then ultrasonically clean with alcohol for 10-15 minutes, and then place in an oven at 90-120ºC to dry for 8-10 hours for use.

[0008] (2) Silicon carbide, boron carbide, silicon dioxide, boron trioxide, aluminum trioxide, silicon hexaboride, and zirconium disilicide powders are selected as coating raw materials, ball-milled and blended in a certain proportion, and then passed through a 120-mesh sieve for use.

[0009] (3) Anhydrous ethanol, polyvinyl butyral (PVB) (model Y2908), and boron-modified phenolic resin (Shandong Baiqian Chemical Co., Ltd.) were added into a beaker in a certain proportion, and mechanically stirred to obtain a uniformly mixed and transparent dual resin adhesive.

[0010] (4) The mixed ceramic powder of step (2) and the dual resin binder of step (3) are mixed into a beaker and mechanically stirred to obtain a coating slurry.

[0011] (5) Apply the slurry prepared in step (4) to the surface of the C / CA substrate and allow to dry naturally for 1-15 days to complete the coating preparation.

[0012] In step (1), various densities of C / CA can be selected for coating to prepare the tree coating, with a density range of 0.2-1.0 g / cm 3 .

[0013] In step (2), the particle size of silicon carbide is ≤1µm, the particle size of boron carbide is ≤1µm, the particle size of silicon dioxide is ≤1µm, the particle size of boron trioxide is ≤2µm, the particle size of aluminum trioxide is ≤1µm, the particle size of silicon hexaboride is ≤1µm, and the particle size of zirconium disilicide is ≤2µm.

[0014] In step (2), the particle size of silicon carbide is 500nm-1µm, the particle size of boron carbide is 700nm-1µm, the particle size of silicon dioxide is 50nm-1µm, the particle size of boron trioxide is 500nm-2µm, the particle size of aluminum trioxide is 50nm-1µm, the particle size of silicon hexaboride is 500nm-1µm, and the particle size of zirconium disilicide is 1-2µm.

[0015] In step (2), the particle size of silicon carbide is 1µm, the particle size of boron carbide is 1µm, the particle size of silicon dioxide is 50nm, the particle size of boron trioxide is 1µm, the particle size of aluminum trioxide is 50nm, the particle size of silicon hexaboride is 1µm, and the particle size of zirconium disilicide is 1µm.

[0016] Step (2) The mixed ceramic powder mainly includes but is not limited to the following seven components: Powder 1, silicon carbide (30-40wt.%), boron carbide (30-40wt.%), silicon dioxide (1-10wt.%), diboron trioxide (1-10wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-12wt.%). Powder 2, silicon carbide (12.5-22.5wt.%), boron carbide (47.5-57.5wt.%), silicon dioxide (2-8wt.%), diboron trioxide (3-7wt.%), aluminum trioxide (1-5wt.%), silicon hexaboride (7.5-12.5wt.%), zirconium disilicide (5-9wt.%). Powder 3, silicon carbide (47.5-57.5wt.%), boron carbide (12.5-22.5wt.%), silicon dioxide (2-8wt.%), diboron trioxide (3-7wt.%), aluminum trioxide (1-5wt.%), silicon hexaboride (7.5-12.5wt.%), zirconium disilicide (5-9wt.%). Powder 4, silicon carbide (30-35wt.%), boron carbide (30-35wt.%), silicon dioxide (1-10wt.%), diboron trioxide (7.5-12.5wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-12wt.%). Powder 5, silicon carbide (25-35wt.%), boron carbide (25-35wt.%), silicon dioxide (1-10wt.%), diboron trioxide (7.5-12.5wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-10wt.%). Powder 6, silicon carbide (10-15wt.%), boron carbide (55-60wt.%), silicon dioxide (1-10wt.%), diboron trioxide (1-7wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-10wt.%). Powder 7, silicon carbide (5-10wt.%), boron carbide (55-66wt.%), silicon dioxide (1-10wt.%), boron trioxide (1-7wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-10wt.%).

[0017] In step (3), the dual resin binder preferably contains 5-35 wt.% (preferably 10-25 wt.%, more preferably 10-15 wt.%) of polyvinyl butyral (PVB, model Y2908), and 5 to 35 wt.% (5 to 25 wt.%, more preferably 5-10 wt.%) of boron-modified phenolic resin (Shandong Baiqian Chemical Co., Ltd.) (abbreviated as FQ), and the remaining mass fraction is anhydrous ethanol.

[0018] In step (4), the solid content of the ceramic and oxide solid powders in the slurry is 10-30 wt.% (preferably 20-30 wt.%, more preferably 20-25 wt.%).

[0019] In step (5), the brush is applied 3-5 times, and the slurry is mechanically stirred at a low speed during the coating process to prevent the deposition of ceramic particles from affecting the uniformity of the coating.

[0020] The C / CA surface resin-ceramic powder composite coating proposed in the present invention has the following characteristics: the coating is prepared at room temperature, is a resin-wrapped ceramic particle structure, has a thickness of 80-300µm, is well bonded to the C / CA substrate, and can achieve oxidation resistance in a wide temperature range of 600-1200ºC. After oxidation at 1200ºC for 2h, the bending strength retention rate of the C / CA protected by the coating is more than 90%.

[0021] The present invention adopts dual-resin polymer powder technology to realize the room-temperature preparation of dense coating on the surface of C / CA. This method evenly coats the ceramic powder-resin slurry on the surface of carbon aerogel composite material, dries it at room temperature, and utilizes the viscosity of the resin and its cohesive force during the drying process to make the ceramic powder form a tight bond and adhere to the C / CA surface. During service, the synergy of ceramic phase oxidation expansion self-sealing and glass phase flow self-healing realizes wide temperature range anti-oxidation. Compared with traditional coating preparation technology, this room-temperature preparation method does not have a high-temperature heat treatment process, which effectively avoids the increase in the thermal conductivity of the C / CA substrate. The resulting coating achieves 600-1200ºC wide temperature range anti-oxidation, and the material's bending strength retention rate exceeds 90% after oxidation at 1200ºC for 2 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The surface morphology and cross-sectional morphology of the C / CA surface resin-ceramic powder composite coating of the present invention.

[0023] Figure 2 The XRD diffraction spectrum of the C / CA surface resin-ceramic powder composite coating of the present invention.

[0024] Figure 3 Oxidation weight loss results of 10% PVB-7.5% FQ coating at 600-1200°C.

[0025] Figure 4 Oxidation weight loss of carbon fiber reinforced carbon aerogel composite without coating at 400-1000°C

[0026] Figure 5 Mechanical retention of materials oxidized at 1200ºC for 2h. DETAILED DESCRIPTION

[0027] In order to further understand the present invention, the present invention is described below in conjunction with examples, but the examples are only for further elaboration of the features and advantages of the present invention, rather than for limitation of the claims of the present invention.

[0028] The method of the present invention specifically comprises the following steps:

[0029] (1) Carbon fiber reinforced carbon aerogel composite material (density 0.2-1.0g / cm 3 ) cut into the required shape, then polish with 800-grit sandpaper, then ultrasonically clean with alcohol for 10-15 minutes, and then place in an oven at 90-120ºC to dry for 8-10 hours for use.

[0030] (2) Silicon carbide, boron carbide, silicon dioxide, boron trioxide, aluminum trioxide, silicon hexaboride, and zirconium disilicide powders are selected as coating raw materials, ball-milled and blended in a certain proportion, and then passed through a 120-mesh sieve for use.

[0031] (3) Anhydrous ethanol, polyvinyl butyral (PVB) (model Y2908), and boron-modified phenolic resin (Shandong Baiqian Chemical Co., Ltd.) were added into a beaker in the required proportions and mechanically stirred to obtain a uniformly mixed and transparent dual resin adhesive.

[0032] (4) The mixed ceramic powder of step (2) and the dual resin binder of step (3) are mixed into a beaker and mechanically stirred to obtain a coating slurry.

[0033] (5) Apply the slurry prepared in step (4) to the surface of the C / CA substrate and allow to dry naturally for 1-15 days to complete the coating preparation.

[0034] In step (1), various densities of C / CA can be selected for coating to prepare the tree coating, with a density range of 0.2-1.0 g / cm 3 .

[0035] In step (2), the particle size of silicon carbide is ≤1µm, the particle size of boron carbide is ≤1µm, the particle size of silicon dioxide is ≤1µm, the particle size of boron trioxide is ≤2µm, the particle size of aluminum trioxide is ≤1µm, the particle size of silicon hexaboride is ≤1µm, and the particle size of zirconium disilicide is ≤2µm.

[0036] Preferably, in step (2), the particle size of silicon carbide is 500nm-1µm, the particle size of boron carbide is 700nm-1µm, the particle size of silicon dioxide is 50nm-1µm, the particle size of boron trioxide is 500nm-2µm, the particle size of aluminum trioxide is 50nm-1µm, the particle size of silicon hexaboride is 500nm-1µm, and the particle size of zirconium disilicide is 1-2µm.

[0037] More preferably, in step (2), the particle size of silicon carbide is 1 µm, the particle size of boron carbide is 1 µm, the particle size of silicon dioxide is 50 nm, the particle size of boron trioxide is 1 µm, the particle size of aluminum trioxide is 50 nm, the particle size of silicon hexaboride is 1 µm, and the particle size of zirconium disilicide is 1 µm.

[0038] Step (2) The mixed ceramic powder mainly includes but is not limited to the following seven components: Powder 1, silicon carbide (30-40wt.%), boron carbide (30-40wt.%), silicon dioxide (1-10wt.%), diboron trioxide (1-10wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-12wt.%). Powder 2, silicon carbide (12.5-22.5wt.%), boron carbide (47.5-57.5wt.%), silicon dioxide (2-8wt.%), diboron trioxide (3-7wt.%), aluminum trioxide (1-5wt.%), silicon hexaboride (7.5-12.5wt.%), zirconium disilicide (5-9wt.%). Powder 3, silicon carbide (47.5-57.5wt.%), boron carbide (12.5-22.5wt.%), silicon dioxide (2-8wt.%), diboron trioxide (3-7wt.%), aluminum trioxide (1-5wt.%), silicon hexaboride (7.5-12.5wt.%), zirconium disilicide (5-9wt.%). Powder 4, silicon carbide (30-35wt.%), boron carbide (30-35wt.%), silicon dioxide (1-10wt.%), diboron trioxide (7.5-12.5wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-12wt.%). Powder 5, silicon carbide (25-35wt.%), boron carbide (25-35wt.%), silicon dioxide (1-10wt.%), diboron trioxide (7.5-12.5wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-10wt.%). Powder 6, silicon carbide (10-15wt.%), boron carbide (55-60wt.%), silicon dioxide (1-10wt.%), diboron trioxide (1-7wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-10wt.%). Powder 7, silicon carbide (5-10wt.%), boron carbide (55-66wt.%), silicon dioxide (1-10wt.%), boron trioxide (1-7wt.%), aluminum trioxide (1-6wt.%), silicon hexaboride (5-15wt.%), zirconium disilicide (2-10wt.%).

[0039] In step (3), the proportion of each component in the dual resin binder is 60-85 wt.%, anhydrous ethanol, 5-35 wt.%, and polyvinyl butyral ester PVB in the dual resin binder, 5-30 wt.%;

[0040] In the dual resin binder, polyvinyl butyral ester (PVB, model Y2908) is preferably 5-35 wt.%, boron-modified phenolic resin (Shandong Baiqian Chemical Co., Ltd.) (abbreviated as FQ) is preferably 5-15 wt.%, and the remaining mass fraction is anhydrous ethanol.

[0041] In step (4), the solid content of the ceramic and oxide solid powders in the slurry is 10-30 wt.%.

[0042] In step (5), the brush is applied 3-5 times, and the slurry is mechanically stirred at a low speed during the coating process to prevent the deposition of ceramic particles from affecting the uniformity of the coating.

[0043] All oxidation experiments were carried out in a constant temperature static air atmosphere. The specific process is to raise the muffle furnace to the test temperature, quickly put the sample into the furnace and start recording the oxidation time. After a certain period of time, take out the sample and weigh and record the weight loss of the sample before and after oxidation. Example 1

[0044] C / CA (obtained according to Example 2 in CN113860909 B) was selected as the substrate, and the sample was cut into a sample of length × width × height = 15 × 15 × 10 mm for testing oxidation weight loss. The surface was polished with 800-grit sandpaper, ultrasonically cleaned with alcohol for 5 minutes, and then placed in an oven at 100°C for 10 hours.

[0045] Silicon carbide (35 wt.%), boron carbide (35 wt.%), silicon dioxide (5 wt.%), boron trioxide (5 wt.%), aluminum trioxide (3 wt.%), silicon hexaboride (10 wt.%), zirconium disilicide (7 wt.%) powders were weighed in proportion, ball milled and blended for 10 hours, and then the powders were dried and sieved through a 120-mesh sieve (the powder that passed the sieve was taken for later use) to obtain a mixed ceramic powder. Anhydrous ethanol (85 wt.%), PVB (10 wt.%, Model Y2908), and FQ (5 wt.%, Shandong Baiqian Chemical Co., Ltd.) were weighed in proportion and mechanically stirred to obtain a transparent two-component binder (i.e., a dual resin binder). The content of ceramic solid powder (mixed ceramic powder) in the slurry was 25 wt.%, and a uniform slurry was obtained by mechanical stirring. The ceramic powder slurry was applied to the 6 surfaces of the fiber-reinforced lightweight carbon-based composite material by a brushing process, and the brushing was repeated 4 times. The mixture was naturally dried for 15 days, and finally a resin-ceramic powder composite coating was prepared on the surface of the C / CA by a brushing method. The coating thickness was about 150-250µm, and the microscopic morphology was as follows Figure 1 (d) (e) (f). XRD analysis of the phases in the coating is shown in Figure 2 ,Compared with the XRD results of pure aerogel, there are sharp diffraction peaks on the coating surface.

[0046] The samples were subjected to high-temperature oxidation tests in a muffle furnace at 600, 800, 1000, and 1200ºC, respectively. The samples were taken out and weighed every 20 minutes to record the weight loss of the samples. A total of 6 tests were conducted. The total weight loss results after 6 times were 600ºC (17.43%), 800ºC (36.42%), 1000 ºC (14.11%), and 1200ºC (26.94%). Figure 4 The oxidation weight loss of C / CA uncoated coating in a muffle furnace at 400, 600, 800, and 1000ºC (the test process is the same as above). It can be seen that the antioxidant capacity of the prepared sample is significantly improved in the range of 600-1200ºC. Example 2

[0047] C / CA (obtained according to Example 2 in CN113860909 B) was selected as the substrate, and the samples were cut into samples with length × width × height = 15 × 15 × 10 mm for testing oxidation weight loss, samples with length × width × height = 20 × 20 × 10 mm for testing the bonding strength between the coating and the substrate, and samples with length × width × height = 60 × 10 × 5 mm for testing the bending strength. The surfaces were polished with 800-mesh sandpaper, ultrasonically cleaned with alcohol for 5 minutes, and then placed in an oven for drying at 100°C for 10 hours. Silicon carbide (17.5 wt.%), boron carbide (52.5 wt.%), silicon dioxide (5 wt.%), diboron trioxide (5 wt.%), aluminum trioxide (3 wt.%), silicon hexaboride (10 wt.%), and zirconium disilicide (7 wt.%) powders were weighed in proportion, ball-milled and blended for 10 hours, then the powders were dried and sieved through a 120-mesh sieve (the powder that passed the sieve was taken for later use), to obtain a mixed ceramic powder.

[0048] Anhydrous ethanol (82.5 wt.%), PVB (10 wt.%, Model Y2908), and FQ (7.5wt.%, Shandong Baiqian Chemical Co., Ltd.) were weighed in proportion and mechanically stirred to obtain four transparent two-component binders. The binder solution and the screened ceramic powder were put into a beaker at a mass ratio of 4:1 and mechanically stirred to obtain a slurry. The ceramic powder slurry was applied to the 6 surfaces of the fiber-reinforced lightweight carbon-based composite material by a brushing process. The brushing was repeated 4 times and dried naturally for 15 days. Finally, a resin-ceramic powder composite coating was prepared on the surface of the lightweight carbon-based composite material by a brushing method. The microscopic morphology of the coating is shown in FIG. Figure 1 (g) (h) (i), coating thickness is 100-300µm. XRD analysis of the phases in the coating is shown in Figure 2,The intensity of the diffraction peak increases with the increase of the resin content, indicating that the resin can polymerize the ceramic powder to a certain extent.

[0049] The oxidation weight loss results of 10% PVB-7.5% FQ coating at 600-1200°C are as follows: Figure 3 The bonding strength between the resin-ceramic layer and the substrate is 6.12MPa, and the residual bonding strength of the coating after oxidation at 1200ºC for 2h is 1.4Mpa. The bending strength of C / CA is about 17.35Mpa, the bending strength after brushing the coating is about 23.3Mpa, and the bending strength after oxidation at 1200ºC for 2h is about 15.65Mpa. The strength retention rate reaches 90.2%. For details, see Figure 5 .

[0050] Comparative Example 3

[0051] C / CA (obtained according to Example 2 in CN113860909 B) was selected as the substrate, and the sample was cut into a sample of length × width × height = 15 × 15 × 10 mm for testing oxidation weight loss. The surface was polished with 800 mesh sandpaper, ultrasonically cleaned with alcohol for 5 minutes, and then placed in an oven for drying at 100°C for 10 hours. Silicon carbide (17.5 wt.%), boron carbide (52.5 wt.%), silicon dioxide (5 wt.%), boron trioxide (5 wt.%), aluminum trioxide (3 wt.%), silicon hexaboride (10 wt.%), and zirconium disilicide (7 wt.%) powders were weighed in proportion, ball milled and blended for 10 hours, and then the powder was dried and sieved through a 120-mesh sieve for later use.

[0052] Anhydrous ethanol (90 wt.%) and PVB (10 wt.%, model Y2908) were weighed in proportion and mechanically stirred to obtain four kinds of transparent dual resin binders. The binder solution and the screened ceramic powder were put into a beaker at a mass ratio of 4:1 and mechanically stirred to obtain a slurry. The ceramic powder slurry was applied to the 6 surfaces of the fiber-reinforced lightweight carbon-based composite material by a brushing process, and the brushing was repeated 4 times and dried naturally for 15 days. Finally, a resin-ceramic powder composite coating was prepared on the surface of the lightweight carbon-based composite material by a brushing method. The microscopic morphology of the coating is shown in FIG. Figure 1 (a) (b) (c), coating thickness is 100-300µm. XRD analysis of the phases in the coating is shown in Figure 2 At this time, the bun peak caused by carbon fiber reinforced carbon aerogel can still be observed, indicating that the density of the material wrapped by the binder is not high and the substrate can be detected by X-rays.

[0053] The samples were subjected to high temperature oxidation tests in a muffle furnace at 600, 800, 1000, and 1200°C, and the samples were taken out and weighed every 20 minutes to record the weight loss of the samples. The tests were conducted 4 times in total, and the total weight loss results after 4 times were 600°C (42.8%), 800°C (30.73%), 1000°C (48.74%), and 1200°C (55.66%). It can be seen that the oxidation resistance of the coating prepared with only PVB as a binder in the range of 600, 800, 1000, and 1200°C is not as good as that of the coating prepared with a dual resin binder.

[0054] Comparative Example 4

[0055] C / CA (obtained according to Example 2 in CN113860909 B) was selected as the substrate, and the sample was cut into a sample of length × width × height = 15 × 15 × 10 mm for testing oxidation weight loss. The surface was polished with 800 mesh sandpaper, ultrasonically cleaned with alcohol for 5 minutes, and then placed in an oven for drying at 100°C for 10 hours. Silicon carbide (17.5 wt.%), boron carbide (52.5 wt.%), silicon dioxide (5 wt.%), boron trioxide (5 wt.%), aluminum trioxide (3 wt.%), silicon hexaboride (10 wt.%), and zirconium disilicide (7 wt.%) powders were weighed in proportion, ball milled and blended for 10 hours, and then the powder was dried and sieved through a 120-mesh sieve for later use.

[0056] Anhydrous ethanol (55 wt.%), PVB (5 wt.%, Model Y2908), and FQ (40wt.%, Shandong Baiqian Chemical Co., Ltd.) were weighed in proportion and mechanically stirred to obtain four transparent two-component binders. The binder solution and the screened ceramic powder were put into a beaker at a mass ratio of 9:1 and mechanically stirred to obtain a slurry. The ceramic powder slurry was applied to the 6 surfaces of the fiber-reinforced lightweight carbon-based composite material by a brushing process, and the brushing was repeated 3 times and dried naturally for 15 days. Finally, a resin-ceramic powder composite coating was prepared on the surface of the lightweight carbon-based composite material by a brushing method. The microscopic morphology of the coating is shown in FIG. Figure 1 (j) (k) (l), the coating thickness is 150-400µm. XRD analysis of the phases in the coating is shown in Figure 2 The XRD spectrum corresponding to this ratio has a steamed bun peak, and the resin content can no longer be ignored.

[0057] The samples were subjected to high temperature oxidation tests in a muffle furnace at 600, 800, 1000, and 1200°C, and the samples were taken out and weighed every 20 minutes to record the weight loss of the samples. The tests were conducted 6 times in total, and the total weight loss results after 6 times were 600°C (85.43%), 800°C (64.35%), 1000°C (40.96%), and 1200°C (50.32%). It can be seen that when the content of FQ in the PVB and FQ dual resin exceeds 30 wt.%, the oxidation resistance of the coating in the range of 600, 800, 1000, and 1200°C is not as good as that of the coating prepared with 5-30 wt.% FQ in the dual resin binder.

Claims

1. A method for preparing a wide temperature range anti-oxidation coating on the surface of a carbon aerogel composite material at room temperature, characterized in that: The method uses a brushing or spraying method to evenly attach ceramic powder-resin slurry to the surface of carbon aerogel composite material C / CA, and adopts dual resin polymerization powder technology to realize the preparation of coating at room temperature, which mainly includes the following steps: (1) Cut the carbon fiber reinforced carbon aerogel composite into the desired shape, polish it with sandpaper, then clean it with alcohol, and dry it for later use; (2) Select silicon carbide, boron carbide, silicon dioxide, boron trioxide, aluminum trioxide, silicon hexaboride, and zirconium disilicide powders as coating raw materials, blend them in the required proportions by ball milling, and then pass them through a 100-120 mesh sieve, and take the powder that passes through the sieve to obtain a mixed ceramic powder; (3) Anhydrous ethanol, polyvinyl butyral ester, and boron-modified phenolic resin FQ are mixed in a desired proportion and mechanically stirred to obtain a uniformly mixed dual resin binder; the distribution ratio of each component in the dual resin binder is 60-85 wt.% of anhydrous ethanol, 5-35 wt.% of polyvinyl butyral ester, and 5 to 30 wt.% of boron-modified phenolic resin; (4) Mixing the mixed ceramic powder of step (2) and the dual resin binder of step (3) and mechanically stirring to obtain a coating slurry; in step (4), the content of the mixed ceramic powder in the slurry is 10-30 wt.%; (5) Apply the slurry prepared in step (4) to the surface of the C / CA substrate and allow to dry naturally for 1-15 days to complete the coating preparation.

2. The normal temperature preparation method according to claim 1, characterized in that: In step (2), the particle size of silicon carbide is ≤1µm, the particle size of boron carbide is ≤1µm, the particle size of silicon dioxide is ≤1µm, the particle size of boron trioxide is ≤2µm, the particle size of aluminum trioxide is ≤1µm, the particle size of silicon hexaboride is ≤1µm, and the particle size of zirconium disilicide is ≤2µm.

3. The normal temperature preparation method according to claim 2, characterized in that: In step (2), the particle size of silicon carbide is 500nm-1µm, the particle size of boron carbide is 700nm-1µm, the particle size of silicon dioxide is 50nm-1µm, the particle size of boron trioxide is 500nm-2µm, the particle size of aluminum trioxide is 50nm-1µm, the particle size of silicon hexaboride is 500nm-1µm, and the particle size of zirconium disilicide is 1-2µm.

4. The normal temperature preparation method according to claim 1, characterized in that: The mixed ceramic powder in step (2) mainly includes but is not limited to any one of the following seven powder compositions: Powder 1, silicon carbide 30-40wt.%, boron carbide 30-40wt.%, silicon dioxide 1-10wt.%, boron trioxide 1-10wt.%, aluminum trioxide 1-6wt.%, silicon hexaboride 5-15wt.%, zirconium disilicide 2-12wt.; Powder 2, silicon carbide 12.5-22.5wt.%, boron carbide 47.5-57.5wt.%, silicon dioxide 2-8wt.%, boron trioxide 3-7wt.%, aluminum trioxide 1-5wt.%, silicon hexaboride 7.5-12.5wt.%, zirconium disilicide 5-9wt.; Powder 3, silicon carbide 47.5-57.5wt.%, boron carbide 12.5-22.5wt.%, silicon dioxide 2-8wt.%, boron trioxide 3-7wt.%, aluminum trioxide 1-5wt.%, silicon hexaboride 7.5-12.5wt.%, zirconium disilicide 5-9wt.; Powder 4, silicon carbide 30-35wt.%, boron carbide 30-35wt.%, silicon dioxide 1-10wt.%, boron trioxide 7.5-12.5wt.%, aluminum trioxide 1-6wt.%, silicon hexaboride 5-15wt.%, zirconium disilicide 2-12wt.; Powder 5, silicon carbide 25-35wt.%, boron carbide 25-35wt.%, silicon dioxide 1-10wt.%, boron trioxide 7.5-12.5wt.%, aluminum trioxide 1-6wt.%, silicon hexaboride 5-15wt.%, zirconium disilicide 2-10wt.; Powder 6, silicon carbide 10-15wt.%, boron carbide 55-60wt.%, silicon dioxide 1-10wt.%, boron trioxide 1-7wt.%, aluminum trioxide 1-6wt.%, silicon hexaboride 5-15wt.%, zirconium disilicide 2-10wt.; Powder 7, silicon carbide 5-10wt.%, boron carbide 55-66wt.%, silicon dioxide 1-10wt.%, boron trioxide 1-7wt.%, aluminum trioxide 1-6wt.%, silicon hexaboride 5-15wt.%, zirconium disilicide 2-10wt.%.

5. The normal temperature preparation method according to claim 1, characterized in that: In step (1), a particle having a density of 0.2-1.0 g / cm 3 The carbon fiber reinforced carbon aerogel composite material is cut into a desired shape, polished with 400-2000 mesh sandpaper, then ultrasonically cleaned with alcohol for 5-15 minutes, and then placed in an oven at 90-120° C. to dry for 8-10 hours for use.

6. An anti-oxidation coating on the surface of a carbon aerogel composite material prepared by the room temperature preparation method according to any one of claims 1 to 5.

7. The anti-oxidation coating on the surface of the carbon aerogel composite material according to claim 6, characterized in that: The coating is prepared at room temperature and is a resin-wrapped ceramic particle structure with a thickness of 80~300µm. It is well bonded to the carbon aerogel composite material C / CA substrate and can achieve oxidation resistance in a wide temperature range of 600-1200℃. The flexural strength retention rate of the carbon aerogel composite material C / CA under coating protection reached more than 90% after oxidation at 1200ºC for 2h.

Citation Information

Patent Citations

  • Preparation method of integrated thermal insulation and load-bearing lightweight carbon-based composite material

    CN113860909B

  • Low-cost high-temperature resistant anti-oxidation coating layer and preparation method thereof

    CN109575742A

Cited By

  • Antioxidant modified carbon fiber-carbon aerogel composite material and preparation method thereof

    CN121779138A

  • Aerogel-based composite heat dissipation coating and preparation method thereof

    CN121948933A

  • An aerogel-based composite heat dissipation coating and a method of making the same

    CN121948933B