A high thermal conductivity potting glue and preparation method thereof
By using specific components and modified particle structures in the potting glue, combined with the dense network segments of the epoxy block, the problem of unbalanced performance of existing potting glues in outdoor use is solved, and high thermal conductivity is achieved. The comprehensive performance of waterproof, weather resistance and UV resistance has been improved significantly, which has significantly improved the reliability and service life of the product.
Patent Information
- Application Number
- CN202410874019.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-02
AI Technical Summary
Existing potting glues cannot take into account good thermal conductivity and waterproof, weather resistance, UV resistance and chemical corrosion resistance in outdoor use, resulting in insufficient reliability and service life of the product in complex environments.
The preparation method of high thermal conductivity potting adhesive is adopted, including component A and component B. Polysiloxane, silicone oil and modified particles are added to component A, and methylsilane, additives and epoxy are added to component B. The segments are formed by specific component ratios and preparation methods to form potting glue with excellent thermal conductivity, and the multi-tin oxide particle coating structure of modified particles and the dense network segment structure of epoxy blocks are improved. Its mechanical properties and corrosion resistance after curing.
It achieves good performance of high thermal conductivity potting glue in outdoor applications, including excellent thermal conductivity, water resistance, weather resistance and UV resistance, which significantly improves the reliability and service life of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of potting adhesives, and in particular to a high thermal conductivity potting adhesive and a preparation method thereof. Background Art
[0002] With the rapid development of photovoltaic products, electronic products, and new energy vehicle industries in recent years, people's functional requirements for products are also constantly increasing, which has also prompted the performance upgrade of products in related industries. In particular, the demand for higher power, efficacy, and service life also means that there will be greater risks of static electricity and heat generation. Therefore, how to effectively solve this risk in the process of iterative upgrades of industries / products has also become an urgent problem for manufacturers to solve, and potting glue is one of the research focuses. Potting refers to the process of mechanically or manually pouring liquid organic resin substances into empty slots or gaps containing photovoltaic modules, electronic components, circuits or devices to form a solidification process under normal temperature or slightly high temperature conditions. This type of organic resin substance is usually called potting glue.
[0003] As the demand direction stabilizes, the performance requirements for potting glue are more certain, but good thermal conductivity is still the primary performance of potting glue. On this basis, facing different product objects and usage environments, the performance requirements of potting glue also have different focuses. Especially in complex outdoor environments, there are certain requirements for the waterproof, weather-resistant, UV-resistant, and chemical-resistant properties of potting glue. Although existing potting glue products can provide good thermal conductivity, they cannot take into account more outdoor use requirements at the same time, and cannot achieve balanced performance in terms of waterproof, weather-resistant, UV-resistant, and chemical-resistant properties. Summary of the invention
[0004] Therefore, in order to solve the above problems, the applicant provides a high thermal conductivity potting glue and a preparation method thereof. The high thermal conductivity potting glue prepared by the present application not only has excellent high thermal conductivity, but also has good waterproof, weather-resistant, UV-resistant and corrosion-resistant properties, and can provide good product reliability in outdoor applications, greatly increasing its use quality and service life, and has a very excellent market prospect, providing an excellent solution to the potting glue problem.
[0005] In order to solve the above problems, the first aspect of the present application provides a high thermal conductive potting glue, which includes component A and component B; in parts by mass, the component A includes: 80-120 parts of polysiloxane, 30-40 parts of silicone oil, 10-30 parts of modified particles, and 1-10 parts of filler; the component B includes: 30-40 parts of methyl silane, 5-15 parts of auxiliary agent, 5-15 parts of epoxy block, and 50-70 parts of silicone oil.
[0006] As a preferred solution, the average viscosity of the polysiloxane is 5000-18000 cp at 25°C.
[0007] As a preferred solution, the average viscosity of the polysiloxane is 6000-14000 cp at 25°C.
[0008] As a preferred solution, the mass ratio of the polysiloxane to the modified particles is (90-110): (15-25).
[0009] As a preferred solution, the polysiloxane is a composition of vinylmethyl polysiloxane and hydroxypolydimethylsiloxane.
[0010] As a preferred solution, the mass ratio of the vinylmethyl polysiloxane to the hydroxypolydimethyl siloxane is (1-2): (4.5-5.5).
[0011] As a preferred solution, the mass ratio of the vinylmethyl polysiloxane to the hydroxypolydimethyl siloxane is 1.5:5.
[0012] As a preferred solution, the silicone oils are all side chain high hydrogen-containing silicone oils.
[0013] As a preferred solution, the hydrogen content of the side chain high hydrogen silicone oil is 1.4-2.0%.
[0014] As a preferred solution, the hydrogen content of the side chain high hydrogen silicone oil is 1.5-1.8%.
[0015] The hydrogen-containing silicone oil added in this application can effectively guarantee the preparation quality of the potting compound, maintain good various properties, improve the curing effect and rate, and avoid internal glue flow and bubble phenomenon. The specific hydrogen-containing silicone oil can not only form a good connection effect with the modified particles with multiple surface hydrogen-containing groups and epoxy block in the raw materials, but also produce a certain degree of cross-linking dehydrogenation inside the potting compound, thereby greatly speeding up the formation of the potting compound curing system, and the appropriate hydrogen content can control the strength of the overall cross-linking effect, enhance the reactivity with the hydroxyl-containing materials in the components, and improve the connection strength of the cross-linking network and the number of cross-linking sites, which not only ensures the adhesion and strength of the potting compound after curing, but also can quickly discharge the gas generated by the reaction to ensure the curing inertia inside the colloid, thereby ensuring a good overall curing effect and potting compound performance.
[0016] As a preferred solution, the preparation method of the modified particles comprises the following steps: S1: mixing tin oxide, succinic anhydride and γ-aminoethylaminopropyltrimethoxysilane in deionized water, heating to 60-65°C, stirring at 100-200 r / min for 3-4 hours, and centrifuging and precipitating after completion to obtain pretreated tin oxide; S2: adding the pretreated tin oxide to a 2-2.4 MPa high-pressure closed reactor and mixing it evenly with chromium nitrate nonahydrate and deionized water, and then in the reaction A deionized water solution of 2,5-dihydroxybenzoic acid is added dropwise to the kettle, the reaction temperature is 120-150°C, and the adding time is 2-2.5h; S3: after the adding is completed, the mixture is stirred at a speed of 100-200r / min for 30-40min, then the temperature is raised to 200-220°C and the mixture is reacted for 20-26h. After the reaction is completed, the mixture is cooled to 60-80°C and the pressure is released. The product is centrifuged and filtered, washed with ethanol and dried at 120-140°C until the product quality does not change, thereby obtaining the modified particles.
[0017] As a preferred solution, the mass ratio of tin oxide, succinic anhydride and γ-aminoethylaminopropyltrimethoxysilane is (1-2): (1.5-2.5): (0.5-1).
[0018] As a preferred solution, the mass ratio of the pretreated tin oxide, chromium nitrate nonahydrate and 2,5-dihydroxybenzoic acid is (2-2.5): (4-5): (1-1.2).
[0019] As a preferred solution, the mass ratio of pretreated tin oxide, chromium nitrate nonahydrate and 2,5-dihydroxybenzoic acid is 2.2:4.5:1.2.
[0020] As a preferred solution, the average particle size of the tin oxide is 10-30 nm.
[0021] As a preferred solution, the average particle size of the modified particles is 500-800 nm.
[0022] As a preferred solution, the specific surface area of the modified particles is 700-800m 2 / g.
[0023] The modified particles added in the present application can greatly improve the mechanical properties of the potting glue after curing and the UV resistance, waterproof and weather resistance after curing. The prepared modified particles form a reunion particle point structure with multiple coatings of tin oxide particles, which is supported by an organic framework and has a certain mechanical support site function inside the potting glue. The porous adsorption structure contained in it can not only adsorb the tin oxide coating, but also fix and adsorb the water molecules inside the potting glue, and can stably preserve the water molecules at the limit temperature, thereby actually removing the active water inside the potting glue system, reducing the migration efficiency of the active groups and obtaining good weather resistance; on the other hand, when the modified particles are on the curing surface of the potting glue, the surface roughness peak-valley structure formed by its structure and the surface of the potting glue colloid can greatly reduce the surface energy and greatly improve the surface hydrophobicity; and the modified particles can form a heterojunction structure of tin oxide particles and organic frameworks, and when light energy is input, it ensures the aggregation of carriers and electron holes on the surfaces of different structures, thereby greatly enhancing the absorption capacity, reducing the actual forbidden band distance, and greatly reducing the damage effect of light on the potting glue when used outdoors.
[0024] As a preferred solution, the filler is a composition of white carbon black and pullulan.
[0025] As a preferred solution, the mass ratio of white carbon black to amylopectin is (1-2): (2.5-3).
[0026] As a preferred solution, the mass ratio of white carbon black to amylopectin is 1:2.5.
[0027] As a preferred solution, the methylsilane is a combination of methyltriethoxysilane and vinyltrimethoxysilane.
[0028] As a preferred solution, the mass ratio of methyltriethoxysilane to vinyltrimethoxysilane is (3-4):(1-1.2).
[0029] As a preferred solution, the mass ratio of methyltriethoxysilane to vinyltrimethoxysilane is 3.5:1.1.
[0030] As a preferred solution, the auxiliary agent is an organic tin salt, a coupling agent, a defoaming agent and a flame retardant.
[0031] As a preferred solution, the mass ratio of the organic tin salt, coupling agent, defoaming agent and flame retardant is (0.5-1): (1-2): (0.5-1.5): (5-8).
[0032] As a preferred solution, the mass ratio of the organic tin salt, coupling agent, defoaming agent and flame retardant is 0.6:1.5:1:7.
[0033] As a preferred solution, the organic tin salt is dibutyltin diacetylacetonate.
[0034] As a preferred solution, the coupling agent is at least one of 3-aminopropyltriethoxysilane, aminopropyltrimethoxysilane, γ-aminoethylaminopropyltrimethoxysilane, and γ-aminoethylaminopropyltriethoxysilane.
[0035] As a preferred solution, the flame retardant is at least one of aluminum hydroxide, magnesium hydroxide and aluminum oxide.
[0036] As a preferred solution, the epoxy block material is an ethylene oxide-propylene oxide block copolymer.
[0037] As a preferred solution, the weight average molecular weight of the epoxy block is 1000-5000.
[0038] As a preferred solution, the epoxy block material is a composition of an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 1000-1500 and an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 4500-5000.
[0039] As a preferred solution, the mass ratio of the ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 1000-1500 to the ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 4500-5000 is (3-4): (1-1.5).
[0040] As a preferred solution, the mass ratio of the ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 1000-1500 to the ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 4500-5000 is 4:1.2.
[0041] The epoxy block of the specific composition added in this application not only effectively improves the thermal conductivity of the potting glue, but also effectively guarantees its mechanical properties and corrosion resistance after curing. The different epoxy blocks added can work together with the components in the system (such as branched starch and polysiloxane, etc.) to form a dense network segment structure interconnected by multiple branches. The existence of this structure can greatly increase the interconnection and entanglement strength between the molecular chains, thereby greatly enhancing the compactness of the internal system of the potting glue itself, and improving the internal digestion and bearing capacity of the sub-stress when external forces act, greatly improving the upper limit of bearing; when external forces act, the surface that should have formed cracks is reconverted into a silver streak state for dispersion and propagation. On the other hand, its complex network segment structure can greatly increase the free resistance of liquid molecules or active molecules inside the potting glue, thereby greatly reducing the frequency of contact and collision of internal and external active molecules, ensuring excellent purity of the internal molecular chains of the potting glue during long-term use, and greatly reducing chemical deterioration.
[0042] The second aspect of the present application provides a method for preparing the above-mentioned high thermal conductivity potting glue, and the preparation method comprises the following steps: S1: Mix the raw materials required for component A in a high-speed mixer and set aside; S2: Mix the raw materials required for component B in a high-speed mixer and set aside; S3: Slowly add component B to component A at a speed of 200~400r / min, control the total addition time to 20~25min, and then continue stirring for 40~60min. After completion, evacuate the product to obtain it.
[0043] The beneficial effects of this application are:
[0044] 1. The high thermal conductivity potting glue provided in this application not only has excellent high thermal conductivity, but also has good waterproof, weather-resistant, UV-resistant and corrosion-resistant properties. It can provide good product reliability in outdoor applications, greatly increase its quality of use and service life, and has a very good market prospect, providing an excellent solution to the potting glue problem.
[0045] 2. A high thermal conductivity potting glue provided in the present application, the addition of a specific hydrogen-containing silicone oil can effectively ensure the preparation quality of the potting glue, maintain good various properties, improve the curing effect and rate, and avoid internal glue flow and bubble phenomena; the specific hydrogen-containing silicone oil can not only form a good connection effect with the modified particles with multiple surface hydrogen-containing groups and epoxy block in the raw materials, but also can produce a certain degree of cross-linking dehydrogenation effect inside the potting glue, thereby greatly accelerating the formation of the potting glue curing system, and the appropriate hydrogen content can control the strength of the overall cross-linking effect, enhance the reactivity with the hydroxyl-containing material in the component, and improve the connection strength of the cross-linking network and the number of cross-linking sites.
[0046] 3. A high thermal conductivity potting compound provided in the present application, wherein the added modified particles form an agglomerated particle point structure coordinated by multiple tin oxide particles and adsorbed with multiple coatings, the interior of the structure is supported by an organic framework and has a certain function as a mechanical support site inside the potting compound, and the porous adsorption structure contained therein can not only adsorb the tin oxide coating, but also fix and adsorb the water molecules inside the potting compound, and can stably preserve the water molecules at a critical temperature, thereby actually removing the active moisture inside the potting compound system, reducing the migration efficiency of the active groups and thus obtaining good weather resistance.
[0047] 4. A high thermal conductivity potting compound provided in the present application, the epoxy block of a specific composition added therein not only effectively improves the thermal conductivity of the potting compound, but also effectively ensures its mechanical properties and corrosion resistance after curing. It can promote the formation of a dense network segment structure interconnected by multiple branches inside the potting compound. The existence of this structure can greatly increase the mutual connection and entanglement strength between the molecular chains, thereby greatly enhancing the compactness of the potting compound's own internal system; on the other hand, it also greatly increases the free resistance of liquid molecules or active molecules inside the potting compound, thereby greatly reducing the frequency of contact and collision between internal and external active molecules, and ensuring excellent purity of the molecular chains inside the potting compound during long-term use. DETAILED DESCRIPTION
[0048] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.
[0049] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.
[0050] Example 1
[0051] Embodiment 1 The first aspect provides a high thermal conductive potting glue, which includes component A and component B; in parts by mass, the component A includes: 100 parts of polysiloxane, 35 parts of silicone oil, 24 parts of modified particles, and 6 parts of filler; the component B includes: 35 parts of methyl silane, 10.1 parts of auxiliary agent, 10 parts of epoxy block, and 60 parts of silicone oil.
[0052] The polysiloxane is a composition of vinylmethyl polysiloxane and hydroxypolydimethyl siloxane, and the mass ratio of the two is 1.5:5.
[0053] The viscosity of vinyl methyl polysiloxane is 6800 cp at 25° C., and it was purchased from Hubei Chengfeng Chemical Co., Ltd.; the viscosity of hydroxy polydimethyl siloxane is 12000 cp at 25° C., and it was purchased from Shanghai Kaiyin Chemical.
[0054] The silicone oils are all side-chain high-hydrogen silicone oils with an average hydrogen content of 1.6%. They were purchased from Shenzhen Xinyongsheng New Materials Co., Ltd.
[0055] The preparation method of the modified particles comprises the following steps, calculated by mass: S1: 1.8 parts of tin oxide, 2.4 parts of succinic anhydride and 0.8 parts of γ-aminoethylaminopropyltrimethoxysilane are mixed in 50 parts of deionized water, the temperature is raised to 60°C, and the reaction is stirred at a speed of 120r / min for 3 hours. After completion, the pre-treated tin oxide is centrifuged and washed to obtain pre-treated tin oxide; S2: 2.2 parts of pre-treated tin oxide are added to a 2.4MPa high-pressure closed reactor and mixed with 4.5 parts of chromium nitrate nonahydrate and 60 S3: after the addition is completed, the mixture is stirred at a speed of 180 r / min for 35 min, and then the temperature is raised to 210°C and the reaction is kept for 25 h. After the reaction is completed, the temperature is lowered to 65°C for decompression, the product is centrifuged, washed with ethanol and dried at 140°C until the product quality does not change, and the modified particles are obtained.
[0056] The average particle size of tin oxide is 15 nm; the average particle size of modified particles is 780 nm.
[0057] The specific surface area of the modified particles is 724m 2 / g.
[0058] The filler is a composition of white carbon black and amylopectin, and the mass ratio of the two is 1:2.5. Amylopectin is purchased from amylopectin products sold by Wuhan Huaxiang Kejie Biotechnology Co., Ltd., and the amylopectin content is ≥70%.
[0059] The methylsilane is a composition of methyltriethoxysilane and vinyltrimethoxysilane, and the mass ratio of the two is 3.5:1.1.
[0060] The additives are organic tin salt, coupling agent, defoaming agent and flame retardant, and the mass ratio is 0.6:1.5:1:7.
[0061] The organic tin salt is dibutyltin diacetylacetonate; the coupling agent is gamma-aminoethylaminopropyltrimethoxysilane; and the flame retardant is aluminum hydroxide.
[0062] The epoxy block material is a composition of BASF L31 (ethylene oxide-propylene oxide block copolymer, weight average molecular weight 1100) and BASF L85 (ethylene oxide-propylene oxide block copolymer, weight average molecular weight 4600), with a mass ratio of 4:1.2.
[0063] The second aspect of the present embodiment provides a method for preparing the above-mentioned high thermal conductivity potting glue, and the preparation method comprises the following steps: S1: Mix the raw materials required for component A in a high-speed mixer and set them aside; S2: Mix the raw materials required for component B in a high-speed mixer and set them aside; S3: Slowly add component B to component A at a speed of 300r / min, control the total addition time to 22min, and then continue stirring for 50min. After completion, evacuate the product to obtain it.
[0064] Example 2
[0065] The first aspect of Example 2 provides a high thermal conductive potting glue, which includes component A and component B; in parts by mass, the component A includes: 90 parts of polysiloxane, 30 parts of silicone oil, 15 parts of modified particles, and 6 parts of filler; the component B includes: 30 parts of methyl silane, 10.1 parts of auxiliary agent, 10 parts of epoxy block, and 50 parts of silicone oil.
[0066] The polysiloxane is a composition of vinylmethyl polysiloxane and hydroxypolydimethyl siloxane, and the mass ratio of the two is 2:4.5.
[0067] The viscosity of vinyl methyl polysiloxane is 6800 cp at 25° C., and it was purchased from Hubei Chengfeng Chemical Co., Ltd.; the viscosity of hydroxy polydimethyl siloxane is 12000 cp at 25° C., and it was purchased from Shanghai Kaiyin Chemical.
[0068] The silicone oil is a side-chain high-hydrogen silicone oil with an average hydrogen content of 1.6%. It was purchased from Shenzhen Xinyongsheng New Materials Co., Ltd.
[0069] The preparation method of the modified particles comprises the following steps, calculated by mass: S1: 1.8 parts of tin oxide, 2.4 parts of succinic anhydride and 0.8 parts of γ-aminoethylaminopropyltrimethoxysilane are mixed in 50 parts of deionized water, the temperature is raised to 60°C, and the reaction is stirred at a speed of 120r / min for 3 hours. After completion, the pre-treated tin oxide is centrifuged and washed to obtain pre-treated tin oxide; S2: 2.2 parts of pre-treated tin oxide are added to a 2.4MPa high-pressure closed reactor and mixed with 4.5 parts of chromium nitrate nonahydrate and 60 S3: after the addition is completed, the mixture is stirred at a speed of 180 r / min for 35 min, and then the temperature is raised to 210°C and the reaction is kept for 25 h. After the reaction is completed, the temperature is lowered to 65°C for decompression, the product is centrifuged, washed with ethanol and dried at 140°C until the product quality does not change, and the modified particles are obtained.
[0070] The average particle size of tin oxide is 15 nm; the average particle size of modified particles is 780 nm.
[0071] The specific surface area of the modified particles is 724m 2 / g.
[0072] The filler is a composition of white carbon black and amylopectin, and the mass ratio of the two is 1: 3. Amylopectin is purchased from amylopectin products sold by Wuhan Huaxiang Kejie Biotechnology Co., Ltd., and the amylopectin content is ≥70%.
[0073] The methylsilane is a composition of methyltriethoxysilane and vinyltrimethoxysilane, and the mass ratio of the two is 4:1.2.
[0074] The additives are organic tin salt, coupling agent, defoaming agent and flame retardant, and the mass ratio is 0.6:1.5:1:7.
[0075] The organic tin salt is dibutyltin diacetylacetonate; the coupling agent is gamma-aminoethylaminopropyltrimethoxysilane; and the flame retardant is aluminum hydroxide.
[0076] The epoxy block material is a composition of BASF L31 (ethylene oxide-propylene oxide block copolymer, weight average molecular weight 1100) and BASF L85 (ethylene oxide-propylene oxide block copolymer, weight average molecular weight 4600), with a mass ratio of 3.5:1.4.
[0077] The second aspect of the present embodiment provides a method for preparing the above-mentioned high thermal conductivity potting glue, and the preparation method comprises the following steps: S1: Mix the raw materials required for component A in a high-speed mixer and set them aside; S2: Mix the raw materials required for component B in a high-speed mixer and set them aside; S3: Slowly add component B to component A at a speed of 300r / min, control the total addition time to 22min, and then continue stirring for 50min. After completion, evacuate the product to obtain it.
[0078] Comparative Example 1
[0079] The specific implementation of this comparative example is basically the same as that of Example 1, except that the silicone oil is a side-chain hydrogen-containing silicone oil with an average hydrogen content of 0.8%, which is purchased from Shandong Shengyilong Chemical Co., Ltd.
[0080] Comparative Example 2
[0081] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified particles comprises the following steps, calculated by mass: S1: adding 2.2 parts of tin oxide to a 2.4MPa high-pressure closed reactor and mixing them evenly with 4.5 parts of chromium nitrate nonahydrate and 60 parts of deionized water, then dropwise adding 1.2 parts of a deionized water solution of 2,5-dihydroxybenzoic acid (40 parts in total) into the reactor, the dropwise reaction temperature is 140°C, and the dropwise addition time is 2h; S3: after the dropwise addition is completed, the mixture is stirred at a speed of 180r / min for 35min, then the mixture is heated to 210°C and reacted for 25h, after the reaction is completed, the mixture is cooled to 65°C and the pressure is released, the product is centrifuged and filtered, washed with ethanol and dried at 140°C until the product quality does not change, and the modified particles are obtained.
[0082] The average particle size of tin oxide is 15 nm; the average particle size of modified particles is 624 nm.
[0083] The specific surface area of the modified particles is 1064m 2 / g.
[0084] Comparative Example 3
[0085] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified particles comprises the following steps, calculated by mass: S1: 3 parts of tin oxide, 1 part of succinic anhydride and 0.2 parts of γ-aminoethylaminopropyltrimethoxysilane are mixed in 60 parts of deionized water, the temperature is raised to 60°C, and the reaction is stirred at a speed of 120r / min for 3h. After completion, the centrifugal precipitation is washed to obtain pretreated tin oxide; S2: 2.2 parts of pretreated tin oxide are added to a 2.4MPa high-pressure closed reactor and mixed with 4 .5 parts of chromium nitrate nonahydrate and 60 parts of deionized water are mixed evenly, and then 1.2 parts of 2,5-dihydroxybenzoic acid deionized water solution (40 parts in total) are added dropwise into the reactor, the reaction temperature is 140°C, and the dropping time is 2h; S3: after the dropping is completed, the temperature is kept at 180r / min and stirred for 35min, and then the temperature is raised to 210°C and kept for reaction for 25h. After the reaction is completed, the temperature is lowered to 65°C for pressure release, the product is centrifuged, washed with ethanol and dried at 140°C until the product quality does not change, and the modified particles are obtained.
[0086] The average particle size of tin oxide is 15 nm; the average particle size of modified particles is 697 nm.
[0087] The specific surface area of the modified particles is 893m 2 / g.
[0088] Comparative Example 4
[0089] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified particles comprises the following steps, calculated by mass: S1: 1.8 parts of tin oxide, 2.4 parts of succinic anhydride and 0.8 parts of γ-aminoethylaminopropyltrimethoxysilane are mixed in 50 parts of deionized water, the temperature is raised to 60°C, and the reaction is stirred at a speed of 120r / min for 3h. After completion, the centrifugal precipitation is washed to obtain pretreated tin oxide; S2: 3.5 parts of pretreated tin oxide are added to a 2.4MPa high-pressure closed reactor and mixed with 2 .25 parts of chromium nitrate nonahydrate and 60 parts of deionized water are mixed evenly, and then 1.5 parts of 2,5-dihydroxybenzoic acid deionized water solution (30 parts in total) are added dropwise into the reactor. The reaction temperature is 140°C and the addition time is 2.5h. S3: After the addition is completed, the mixture is stirred at a speed of 180r / min for 35min, and then the temperature is raised to 210°C and the mixture is kept for reaction for 24h. After the reaction is completed, the temperature is lowered to 65°C for pressure release, the product is centrifuged, washed with ethanol and dried at 140°C until the product quality does not change, and the modified particles are obtained.
[0090] The average particle size of tin oxide is 15 nm; the average particle size of modified particles is 1047 nm.
[0091] The specific surface area of the modified particles is 607m 2 / g.
[0092] Comparative Example 5
[0093] The specific implementation of this comparative example is basically the same as that of Example 1, except that the epoxy block is BASF L88, an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 10,000.
[0094] Comparative Example 6
[0095] The specific implementation of this comparative example is basically the same as that of Example 1, except that the epoxy block material is a composition of BASF L31 (ethylene oxide-propylene oxide block copolymer, weight average molecular weight 1100) and BASF L85 (ethylene oxide-propylene oxide block copolymer, weight average molecular weight 4600), with a mass ratio of 1:1.
[0096] Comparative Example 7
[0097] The specific implementation of this comparative example is basically the same as that of Example 1, except that the epoxy block material is a composition of BASF L31 (ethylene oxide-propylene oxide block copolymer, weight average molecular weight 1100) and BASF L85 (ethylene oxide-propylene oxide block copolymer, weight average molecular weight 4600), with a mass ratio of 8:1.
[0098] Performance Evaluation
[0099] 1. Thermal conductivity test: The thermal conductivity test of the potting glue prepared in the embodiment and the comparative example was carried out with reference to ISO 22007-2 standard. The measured values were taken as the average value of 10 tests and recorded in Table 1.
[0100] 2. UV resistance test: The size of the test sample is 1cm×1cm×0.2cm. The cured potting glue sample is placed in a water-UV irradiation test box and observed once every 2 days. The irradiation power is 220W. If there are obvious yellowing, cracking, or damage on the surface of the potting glue sample during each observation, take it out directly and continue testing the remaining samples. Repeat the above steps until 21 days later. Test 50 samples in each group, record the number of samples remaining after 21 days, and record the results in Table 1.
[0101] 3. Surface waterproofness: The sessile drop method is used for testing. The test sample size is 1cm×1cm×0.2cm, the test water drop is 2.5μL, the test standard time is 10s, and the water contact angle of the corresponding potting glue surface is measured. The measured value is the average of 10 tests and recorded in Table 1.
[0102] 4. Mechanical strength: Refer to GB / T 528-2009 to test the tensile strength of the potting compound. The measured value is the average value of 10 tests and recorded in Table 1.
[0103] Table 1 Performance test results
[0104]
[0105] From the examples and comparative examples of the present application and the data results in Table 1, it can be seen that the thermal conductivity, UV resistance, water resistance and mechanical properties of Examples 1 and 2 using the specific technical solution of the present application are significantly better than those of Comparative Examples 1 to 7. This is mainly because the technical solution adopted in Examples 1 and 2 can not only greatly improve its mechanical support and absorption capacity for ultraviolet light energy through modified particles, but also promote the formation of a dense network segment structure interconnected by multiple branches inside the potting compound. The existence of this structure can greatly increase the interconnection and entanglement strength between the molecular chains, thereby greatly enhancing the compactness of the potting compound's own internal system; on the other hand, it also greatly increases the free resistance of liquid molecules or active molecules inside the potting compound, thereby greatly reducing the frequency of contact and collision between internal and external active molecules, ensuring excellent purity of the molecular chains inside the potting compound during long-term use, and thus obtaining more excellent performance results than Comparative Examples 1 to 7.
Claims
1. A high thermal conductivity potting compound, characterized by: It includes component A and component B; In parts by mass, the component A comprises: 80-120 parts of polysiloxane, 30-40 parts of silicone oil, 10-30 parts of modified particles, and 1-10 parts of filler; the component B comprises: 30-40 parts of methylsilane, 5-15 parts of auxiliary agent, 5-15 parts of epoxy block, and 50-70 parts of silicone oil; The average viscosity of the polysiloxane at 25° C. is 5000 to 18000 cp; The mass ratio of the polysiloxane to the modified particles is (90-110): (15-25); The polysiloxane is a composition of vinylmethyl polysiloxane and hydroxy polydimethyl siloxane; the mass ratio of the vinylmethyl polysiloxane to the hydroxy polydimethyl siloxane is (1-2): (4.5-5.5); The silicone oils are all side chain high hydrogen silicone oils; the hydrogen content of the side chain high hydrogen silicone oils is 1.4-2.0%; The preparation method of the modified particles comprises the following steps: S1: mixing tin oxide, succinic anhydride and γ-aminoethylaminopropyltrimethoxysilane in deionized water, heating to 60-65° C., stirring at a speed of 100-200 r / min for 3-4 hours, and then centrifuging and precipitating to obtain pretreated tin oxide; S2: adding the pretreated tin oxide to a 2-2.4 MPa high-pressure closed reactor, mixing it with chromium nitrate nonahydrate and deionized water, and then adding dropwise in the reactor. Add a deionized aqueous solution of 2,5-dihydroxybenzoic acid, add dropwise at a reaction temperature of 120-150°C and a dropwise addition time of 2-2.5 hours; S3: after the dropwise addition is completed, keep warm at a speed of 100-200 r / min and stir for 30-40 minutes, then raise the temperature to 200-220°C and keep warm for 20-26 hours, cool to 60-80°C and release the pressure after the reaction is completed, centrifuge and filter the product, wash with ethanol and dry at 120-140°C until the product quality does not change, thereby obtaining modified particles; The mass ratio of the tin oxide, succinic anhydride and γ-aminoethylaminopropyltrimethoxysilane is (1-2): (1.5-2.5): (0.5-1); The mass ratio of the pretreated tin oxide, chromium nitrate nonahydrate and 2,5-dihydroxybenzoic acid is (2-2.5): (4-5): (1-1.2); The filler is a composition of white carbon black and pullulan; the mass ratio of the white carbon black to the pullulan is (1-2): (2.5-3); The epoxy block material is a composition of an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 1000-1500 and an ethylene oxide-propylene oxide block copolymer with a weight average molecular weight of 4500-5000, and the mass ratio of the two is (3-4): (1-1.5).
2. The high thermal conductivity potting compound according to claim 1, characterized in that: The average particle size of the tin oxide is 10-30 nm.
3. The high thermal conductivity potting compound according to claim 2, characterized in that: The average particle size of the modified particles is 500-800 nm; the specific surface area of the modified particles is 700-800 m 2 / g.
4. The high thermal conductivity potting compound according to claim 3, characterized in that: The methylsilane is a composition of methyltriethoxysilane and vinyltrimethoxysilane; the mass ratio of the methyltriethoxysilane to the vinyltrimethoxysilane is (3-4): (1-1.2).
5. The high thermal conductivity potting compound according to claim 4, characterized in that: The auxiliary agents are organic tin salt, coupling agent, defoaming agent and flame retardant.
6. The high thermal conductivity potting compound according to claim 5, characterized in that: The mass ratio of the organic tin salt, coupling agent, defoaming agent and flame retardant is (0.5-1): (1-2): (0.5-1.5): (5-8).
7. A method for preparing the high thermal conductivity potting compound according to any one of claims 1 to 6, characterized in that: Preparation method The following steps are involved: S1: Mix the raw materials required for component A in a high-speed mixer and set aside; S2: Mix the raw materials required for component B in a high-speed mixer and set aside; S3: Slowly add component B to component A at a speed of 200-400 r / min, controlling the total addition time to be 20-25 min, and then continue stirring for 40-60 min. After completion, evacuate the product to obtain the product.