A thermal conductive filler and preparation method thereof and epoxy molding compound

By modifying the combination of hexagonal boron nitride and alumina, the problem of the processability and fluidity of traditional epoxy plastic seals is solved, and high thermal conductivity is achieved. High-flow epoxy plastic sealing material can effectively deal with the thermal stress and thermal failure problems of semiconductor devices.

CN118420976BActive Publication Date: 2024-11-05ZHUHAI GREE NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410864648.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-05
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

Traditional epoxy plastic sealing materials have affected processability, fluidity and uniformity in high-filling thermal conductivity fillers, which cannot effectively solve the thermal stress and thermal failure problems of semiconductor devices under high integration and power density.

Method used

By mixing modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina in organic solvents for ultrasonic heating, a thermal conductivity filler similar to a sandwich structure is formed, and epoxy plastic sealing material is prepared in combination with epoxy resin to regulate heat conduction The ratio of fillers in epoxy plastic sealing materials is to overcome the defects of high filling rate and form high thermal conductivity and high fluidity materials.

Benefits of technology

It is achieved to improve the thermal conductivity and fluidity of epoxy plastic sealing materials without affecting processability and fluidity, form a dense phonon transmission network, and enhance the conduction effect of the three-dimensional thermal conductivity network.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118420976B_ABST
    Figure CN118420976B_ABST
Patent Text Reader

Abstract

The present invention specifically discloses a thermally conductive filler and a preparation method thereof and an epoxy molding compound. The preparation method of the thermally conductive filler includes: mixing modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina in an organic solvent, ultrasonically, and then heating and removing water to obtain a thermally conductive filler; the modified hexagonal boron nitride is hexagonal boron nitride modified by polydopamine; the modified large-size alumina and the modified small-size alumina are respectively alumina modified by a silane coupling agent; the particle size of the modified large-size alumina is 1-5 μm; the modified small-size alumina is 0.1-0.9 μm. By surface modification of the hexagonal boron nitride, modified spherical alumina of different sizes are embedded in the gap between adjacent boron nitride sheets, the contact area between the thermally conductive particles is increased, and the strong interaction between alumina and boron nitride promotes the effective conduction of the three-dimensional thermal conductive network, thereby preparing a high thermal conductivity and high fluidity epoxy molding compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of integrated circuits, and in particular relates to a thermal conductive filler and a preparation method thereof, and an epoxy molding compound. Background Art

[0002] Electronic packaging is divided into metal packaging, ceramic packaging and plastic packaging according to different materials. At present, more than 95% of semiconductor devices use plastic packaging, and more than 90% of plastic packaging uses epoxy molding compound. Epoxy molding compound (EMC) has a simple production process and high reliability. It is widely used in semiconductor device packaging to protect chips from the external environment, especially from external mechanical physical forces and external chemical forces, and provides a heat dissipation channel for chips. However, with the improvement of chip integration, the structure is more complex, the power density of various packaging modules increases, and a large amount of heat is generated in the application, which brings serious thermal stress and thermal failure problems. Spherical silica, spherical alumina, angular silica, etc. are often used as thermal conductive fillers in traditional epoxy molding compounds, but it often requires a very high filling rate for the thermal conductivity to show a significant improvement, but the high filling rate will affect the processability, fluidity, uniformity and coating effect of the epoxy molding compound.

[0003] Therefore, the prior art needs to be further developed and improved. Summary of the invention

[0004] In view of the various deficiencies of the prior art and in order to solve the above problems, a thermal conductive filler and a preparation method thereof and an epoxy molding compound are proposed. The present invention provides the following technical solutions:

[0005] A method for preparing a thermally conductive filler, the method comprising: mixing modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina in an organic solvent, ultrasonically treating the mixture, and then heating and removing water to obtain the thermally conductive filler;

[0006] The modified hexagonal boron nitride is hexagonal boron nitride modified with polydopamine;

[0007] The modified large-size alumina and the modified small-size alumina are respectively alumina modified by a silane coupling agent;

[0008] The particle size of the modified large-size alumina is 1-5 μm; the particle size of the modified small-size alumina is 0.1-0.9 μm.

[0009] Furthermore, the mass ratio of the modified hexagonal boron nitride, the modified small-sized alumina and the modified large-sized alumina is (1-10):1:2.

[0010] Furthermore, the mass ratio of the modified hexagonal boron nitride, the modified small-sized alumina and the modified large-sized alumina is 5:1:2.

[0011] Furthermore, the average particle size of the modified large-size alumina is 2 μm; the average particle size of the modified small-size alumina is 0.3 μm.

[0012] Furthermore, the modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina are mixed and ultrasonically treated in an organic solvent for 0.5-3 hours; the modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina are mixed and ultrasonically treated in an organic solvent and then heated for 2-4 hours at a heating temperature of 85-105°C. The dehydration process includes: centrifugal washing with deionized water for 3-5 times at a centrifugal speed of 3000-4000r / min, and vacuum drying at 65-85°C.

[0013] Furthermore, the preparation process of the modified large-size alumina is as follows: spherical alumina with a particle size of 1-5 μm and a silane coupling agent are added to anhydrous ethanol for ultrasonication for 0.5-3 hours, followed by heating for 2-4 hours at a heating temperature of 85-105° C., and centrifugation drying to obtain the modified large-size alumina;

[0014] In terms of mass percentage, the amount of silane coupling agent required for modifying large-sized alumina is 1-10% of spherical alumina with a particle size of 1-5 μm;

[0015] The preparation process of the modified small-sized alumina is as follows: spherical alumina with a particle size of 0.1-0.9 μm and a silane coupling agent are added to anhydrous ethanol for ultrasonication for 0.5-3 hours, followed by heating for 2-4 hours at a heating temperature of 85-105° C., and centrifugation drying to obtain the modified small-sized alumina;

[0016] Calculated by mass percentage, the amount of silane coupling agent required for modifying large-size alumina is 1-10% of the spherical alumina with a particle size of 0.1-0.9 μm.

[0017] Furthermore, the preparation process of the modified hexagonal boron nitride is as follows: the flake diameter of the hexagonal boron nitride is 1-20 μm, the hexagonal boron nitride is added to an ethanol solution for ultrasonication, the pH value is adjusted to 8-9 after ultrasonication, dopamine hydrochloride is added to the above solution and continued to be stirred, and the modified hexagonal boron nitride is obtained by centrifugation and drying, and the amount of dopamine hydrochloride added is 10-15% of the mass of the hexagonal boron nitride.

[0018] In addition, the present invention also provides a thermally conductive filler, which is prepared by the above-mentioned method for preparing the thermally conductive filler.

[0019] The invention also provides an epoxy molding compound, comprising epoxy resin and the above-mentioned thermal conductive filler.

[0020] Furthermore, the mass ratio of the epoxy resin to the thermal conductive filler is 12:120-200.

[0021] Furthermore, the epoxy resin includes at least one of biphenyl epoxy resin, o-cresol epoxy resin, glycidyl ether epoxy resin, multifunctional epoxy resin, bisphenol A epoxy resin, and bisphenol F epoxy resin.

[0022] Beneficial effects:

[0023] 1. This application modifies the surface of hexagonal boron nitride and embeds modified spherical alumina of different sizes into the gaps between adjacent boron nitride sheets to form a sandwich-like structure, thereby increasing the contact area between the thermally conductive particles. The strong interaction between alumina and boron nitride promotes the effective conduction of the three-dimensional thermal conductive network.

[0024] 2. By adjusting the size and dosage ratio of hexagonal boron nitride and alumina of different sizes, the percolation phenomenon of thermally conductive fillers in epoxy molding compounds is explored. The thermally conductive fillers are added to the epoxy molding compound composition to overcome the influence of the high filling rate of the fillers on the processability, fluidity, uniformity and coating effect of the epoxy molding compound, forming a denser phonon transmission network, and providing a high thermal conductivity and high fluidity epoxy molding compound. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a scanning electron microscope image of a thermally conductive filler in the present invention. DETAILED DESCRIPTION

[0026] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention is clearly and completely described below in conjunction with the accompanying drawings of the present invention. Based on the embodiments in this application, other similar embodiments obtained by ordinary technicians in this field without making creative work should all fall within the scope of protection of this application. In addition, the directional words mentioned in the following embodiments, such as "up", "down", "left", "right", etc., are only reference to the directions of the accompanying drawings. Therefore, the directional words used are used to illustrate rather than limit the invention.

[0027] A method for preparing a thermally conductive filler, the method comprising: mixing modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina in an organic solvent, ultrasonically treating the mixture, and then heating and removing water to obtain a thermally conductive filler; the modified hexagonal boron nitride is hexagonal boron nitride modified by polydopamine; the modified large-size alumina and the modified small-size alumina are respectively alumina modified by a silane coupling agent; the particle size of the modified large-size alumina is 1-5 μm; the particle size of the modified small-size alumina is 0.1-0.9 μm. By surface modification of the hexagonal boron nitride, spherical alumina of different sizes are embedded in the gaps between adjacent boron nitride sheets to form a sandwich-like structure, thereby increasing the contact area between the thermally conductive particles, and the strong interaction between alumina and boron nitride promotes the effective conduction of the three-dimensional thermal conductive network.

[0028] like Figure 1 As shown in the figure, the microstructure of the thermal conductive filler was observed by scanning electron microscopy. Figure 1 It can be seen that alumina of different sizes are embedded in the gaps between adjacent modified hexagonal boron nitride sheets. This structure is more beneficial to increase the contact area between thermally conductive particles and form a three-dimensional thermal conductive network. Large-sized alumina can connect boron nitride sheets up and down to promote heat transfer. Small-sized spherical alumina acts as a bridge and can fill the gaps between large-sized balls and the gaps between boron nitride sheets and spheres, improving the integrity of the thermal conduction network and reducing internal defects. By adjusting the size of spherical alumina and the ratio between modified boron nitride and alumina, high thermal conductivity and low viscosity epoxy molding compounds can be prepared.

[0029] Specifically, the modified hexagonal boron nitride, the modified large-size alumina and the modified small-size alumina are mixed and ultrasonically processed in an organic solvent, and the organic solvent may be dimethylformamide.

[0030] In addition, the above-mentioned thermal conductive filler can be combined with epoxy resin to prepare epoxy molding compound. Specifically, the epoxy molding compound includes epoxy resin, curing agent, thermal conductive filler, curing agent accelerator, flame retardant, coupling agent, release agent, colorant, stress modifier, and ion capture agent.

[0031] The epoxy resin is at least two of biphenyl epoxy resin, o-cresol epoxy resin, glycidyl ether epoxy resin, multifunctional epoxy resin, bisphenol A epoxy resin, and bisphenol F epoxy resin;

[0032] The curing agent is at least one of linear phenolic resin, biphenyl phenolic resin, o-cresol phenolic resin, and phenol aralkyl phenolic resin;

[0033] The curing agent accelerator is at least one of 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole;

[0034] The flame retardant is at least one of a phosphorus flame retardant, a nitrogen flame retardant, and a metal hydroxide flame retardant;

[0035] The coupling agent is at least one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane;

[0036] The stress modifier is at least one of carboxyl-terminated liquid nitrile rubber, liquid polybutadiene rubber, and liquid hydroxyl polyether. The stress of the epoxy molding compound is reduced by adding the stress modifier. Compared with silicone resin and silicone oil, this type of modifier is less likely to seep out to prevent contamination of the mold.

[0037] The anion scavenger is at least one of IXE500, IXE550, and IXE770D, which is used to reduce the content of chloride ions in the epoxy molding compound;

[0038] The release agent is carnauba wax;

[0039] The colorant is carbon black.

[0040] The preparation process of epoxy molding compound is as follows:

[0041] The epoxy resin and the curing agent are mixed at high speed to form a mixture; the thermal conductive filler, the curing agent accelerator, the flame retardant, the coupling agent, the stress modifier, the anion scavenger, the release agent and the colorant are added to the mixture and mixed at high speed to obtain a premix;

[0042] The premix is ​​extruded through a twin-screw extruder at a temperature of 110° C. and a screw speed of 80 rpm, and the obtained molten mixed material is cooled, crushed, magnetically separated, and preformed to obtain an epoxy molding compound.

[0043] Example 1: Investigating the effects of the selection of modified hexagonal boron nitride, modified large-size alumina, and modified small-size alumina in thermal conductive fillers on the thermal conductivity and flow properties of epoxy molding compounds

[0044] Different thermally conductive fillers are set, namely, thermally conductive filler 1: modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina; thermally conductive filler 2: unmodified hexagonal boron nitride, modified large-size alumina and modified small-size alumina; thermally conductive filler 3: modified hexagonal boron nitride, unmodified large-size alumina and unmodified small-size alumina; thermally conductive filler 4: unmodified hexagonal boron nitride, unmodified large-size alumina and unmodified small-size alumina; thermally conductive filler 5: unmodified hexagonal boron nitride, unmodified small-size alumina; thermally conductive filler 6: unmodified hexagonal boron nitride.

[0045] Then follow the steps below:

[0046] Preparation of modified hexagonal boron nitride: Weigh hexagonal boron nitride with a sheet diameter of 10 μm, add it to a mixed solution of ethanol and water with a volume ratio of 1:1, stir ultrasonically at 25°C for 2 hours, adjust the solution pH to 8 with dilute hydrochloric acid, and stir at 60°C for 30 minutes. Add dopamine hydrochloride to the above solution in an amount of 12% of the hexagonal boron nitride, and continue stirring for 2 hours. Wash the product by centrifugation with deionized water 4 times at a speed of 3500r / min until the upper dispersion is neutral, and vacuum dry it at 75°C for 24 hours to obtain modified hexagonal boron nitride.

[0047] Preparation of modified large-size alumina: Spherical alumina with an average particle size of 2 μm and γ-aminopropyltriethoxysilane (KH550) were added to anhydrous ethanol, the amount of KH550 was 6% of the mass of the spherical alumina, and ultrasonic treatment was performed for 1 hour. Deionized water was added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain modified large-size alumina.

[0048] Preparation of modified small-sized alumina: Spherical alumina with an average particle size of 0.3 μm and γ-aminopropyltriethoxysilane (KH550) were added to anhydrous ethanol, the amount of KH550 was 6% of the mass of the spherical alumina, and ultrasonic treatment was performed for 1 hour. Deionized water was added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain modified small-sized alumina.

[0049] Preparation of thermally conductive filler: According to the settings of thermally conductive filler 1 to thermally conductive filler 6, the corresponding raw materials were added to dimethylformamide, the solution was ultrasonically treated for 1 hour, and then heated and stirred at 95°C for 3 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain the corresponding thermally conductive fillers 1 to thermally conductive fillers 6, respectively.

[0050] Preparation of epoxy molding compound: 140 parts of corresponding thermal conductive fillers 1 to 6 are mixed with 9 parts of o-cresol epoxy resin, 3 parts of bisphenol A epoxy resin, and 8 parts of linear phenolic resin at high speed to form mixtures 1 to 6; 0.5 parts of 2-methylimidazole, 3 parts of triphenyl phosphate, 0.3 parts of γ-aminopropyl triethoxysilane, 0.4 parts of carboxyl-terminated liquid nitrile rubber, 0.2 parts of IXE500, 0.5 parts of carnauba wax, and 0.2 parts of carbon black are added to mixtures 1 to 6 respectively, and mixed at high speed to obtain premixes 1 to 6;

[0051] Premix 1 to premix 6 are extruded through a twin-screw extruder at a temperature of 110° C. and a screw speed of 80 rpm, respectively. The obtained molten mixed materials are cooled, crushed, magnetically separated, and preformed to obtain epoxy molding compounds 1 to epoxy molding compounds 6.

[0052] Among them, the mass ratio of modified (or unmodified) hexagonal boron nitride, modified (or unmodified) small-sized alumina and modified (or unmodified) large-sized alumina is 5:1:2.

[0053] The thermal conductivity and fluidity of epoxy molding compounds 1 to 6 were tested, and the data shown in Table 1 were obtained.

[0054] Table 1 Thermal conductivity and flow properties of epoxy molding compounds 1 to 6

[0055]

[0056] It can be seen from Table 1 above that: directly adding hexagonal boron nitride and alumina as thermal conductive fillers, the arbitrary distribution of the fillers makes the heat transfer channel incomplete, resulting in a low thermal conductivity of the epoxy molding compound, and the boron nitride is not modified, and the accumulation and blockage between the boron nitride layers will reduce the fluidity of the epoxy molding compound. The thermal conductive filler formed by combining modified hexagonal boron nitride, modified large-sized alumina and modified small-sized alumina can form a better thermal conductive network. The strong interaction between alumina of different sizes and hexagonal boron nitride is improved by each modification, which promotes the effective transfer of the three-dimensional thermal conductive network. Compared with only hexagonal boron nitride or hexagonal boron nitride combined with only one type of alumina, the combination of modified hexagonal boron nitride, modified large-sized alumina and modified small-sized alumina in this application significantly improves the thermal conductivity, and the prepared epoxy molding compound has better fluidity.

[0057] Example 2: Investigating the effect of the ratio of modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina in thermal conductive fillers on the thermal conductivity and flow properties of epoxy molding compounds

[0058] The thermal conductive filler includes modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina. The mass ratios of modified hexagonal boron nitride, modified small-size alumina and modified large-size alumina in the thermal conductive filler are set to be 5:1:2, 6:1:2, 10:1:2, 1:1:2, 15:1:2 and 0:1:2 respectively.

[0059] Then proceed as follows:

[0060] Preparation of modified hexagonal boron nitride: Weigh hexagonal boron nitride with a sheet diameter of 10 μm, add it to a mixed solution of ethanol and water with a volume ratio of 1:1, stir ultrasonically at 25°C for 2 hours, adjust the solution pH to 8 with dilute hydrochloric acid, and stir at 60°C for 30 minutes. Add dopamine hydrochloride to the above solution in an amount of 12% of the hexagonal boron nitride, and continue stirring for 2 hours. Wash the product by centrifugation with deionized water 4 times at a speed of 3500r / min until the upper dispersion is neutral, and vacuum dry it at 75°C for 24 hours to obtain modified hexagonal boron nitride.

[0061] Preparation of modified large-size alumina: Spherical alumina with an average particle size of 2 μm and γ-aminopropyltriethoxysilane (KH550) were added to anhydrous ethanol, the amount of KH550 was 6% of the mass of the spherical alumina, and ultrasonic treatment was performed for 1 hour. Deionized water was added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain modified large-size alumina.

[0062] Preparation of modified small-sized alumina: Spherical alumina with an average particle size of 0.3 μm and γ-aminopropyltriethoxysilane (KH550) were added to anhydrous ethanol, the amount of KH550 was 6% of the mass of the spherical alumina, and ultrasonic treatment was performed for 1 hour. Deionized water was added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain modified small-sized alumina.

[0063] Preparation of thermally conductive filler: According to the dosage ratio of modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina in the thermally conductive filler, the corresponding thermally conductive filler was added into dimethylformamide, the solution was ultrasonically treated for 1 hour, then heated and stirred at 95°C for 3 hours, the product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain the corresponding thermally conductive filler.

[0064] Preparation of epoxy molding compound: 140 parts of corresponding thermal conductive fillers are mixed with 9 parts of o-cresol epoxy resin, 3 parts of bisphenol A epoxy resin, and 8 parts of linear phenolic resin at high speed to form corresponding mixtures; 0.5 parts of 2-methylimidazole, 3 parts of triphenyl phosphate, 0.3 parts of γ-aminopropyl triethoxysilane, 0.4 parts of carboxyl-terminated liquid nitrile rubber, 0.2 parts of IXE500, 0.5 parts of carnauba wax, and 0.2 parts of carbon black are added to the corresponding mixtures respectively, and mixed at high speed to obtain corresponding premixes;

[0065] The corresponding premixes were extruded through a twin-screw extruder at a temperature of 110° C. and a screw speed of 80 rpm, and the obtained molten mixed materials were cooled, crushed, magnetically separated, and preformed to obtain the corresponding epoxy molding compound.

[0066] The thermal conductivity and fluidity of the corresponding epoxy molding compound were tested, and the data shown in Table 2 were obtained.

[0067] Table 2 Thermal conductivity and flow properties of epoxy molding compound at different raw material dosage ratios of conductive fillers

[0068]

[0069] It can be found through Example 2 that as the proportion of modified hexagonal boron nitride in the thermally conductive filler increases, the thermal conductivity and fluidity of the epoxy molding compound first increase and then decrease. When the proportion of modified hexagonal boron nitride in the thermally conductive filler is 5 parts, the thermal conductivity and fluidity of the epoxy molding compound prepared therefrom reach the best. When the proportion of modified hexagonal boron nitride in the thermally conductive filler is more than 10 parts, due to the accumulation of hexagonal boron nitride flakes, the heat transfer rate in the epoxy molding compound is reduced, causing the thermal conductivity and fluidity to decrease. When only spherical alumina is added as the filler and no flaky modified hexagonal boron nitride is added, the thermal conductivity and fluidity of the epoxy molding compound are low due to the performance of the material itself.

[0070] Example 3: Investigating the effect of the size of thermally conductive fillers on the thermal conductivity and flow properties of epoxy molding compounds

[0071] Different sizes of modified hexagonal boron nitride, modified small-size alumina and modified large-size alumina were set respectively. The first group was: the average flake diameter of modified hexagonal boron nitride was 1 μm, the average particle size of modified small-size alumina was 0.3 μm, and the average particle size of modified large-size alumina was 2 μm; the second group was: the average flake diameter of modified hexagonal boron nitride was 5 μm, the average particle size of modified small-size alumina was 0.3 μm, and the average particle size of modified large-size alumina was 2 μm; the third group was: modified hexagonal boron nitride The average flake diameter of square boron nitride is 10μm, the particle size of modified small-size alumina is 0.3μm, and the particle size of modified large-size alumina is 2μm; the fourth group is: the average flake diameter of modified hexagonal boron nitride is 20μm, the particle size of modified small-size alumina is 0.3μm, and the particle size of modified large-size alumina is 2μm; the fifth group is: the average flake diameter of modified hexagonal boron nitride is 10μm, the particle size of modified small-size alumina is 0.5μm, and the particle size of modified large-size alumina is 5μm.

[0072] Then proceed as follows:

[0073] Preparation of modified hexagonal boron nitride: Weigh hexagonal boron nitride, add it to a mixed solution of ethanol and water in a volume ratio of 1:1, stir it ultrasonically at 25°C for 2h, adjust the pH of the solution to 8 with dilute hydrochloric acid, and stir it at 60°C for 30min. Add dopamine hydrochloride to the above solution in an amount of 12% of the hexagonal boron nitride, and continue stirring for 2h. Wash the product by centrifugation with deionized water for 4 times at a speed of 3500r / min until the upper dispersion is neutral, and vacuum dry it at 75°C for 24h to obtain modified hexagonal boron nitride.

[0074] Preparation of modified large-size alumina: The corresponding spherical alumina and γ-aminopropyltriethoxysilane (KH550) are selected and added to anhydrous ethanol, the amount of KH550 is 6% of the mass of the spherical alumina, and ultrasonic treatment is performed for 1 hour. Deionized water is added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product is centrifuged and washed 4 times with deionized water at a speed of 3500r / min, and vacuum dried at 75°C for 24 hours to obtain modified large-size alumina.

[0075] Preparation of modified small-sized alumina: Spherical alumina of corresponding particle size and γ-aminopropyltriethoxysilane (KH550) are added to anhydrous ethanol, the amount of KH550 is 6% of the mass of the spherical alumina, and ultrasonic treatment is performed for 1 hour. Deionized water is added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product is centrifuged and washed 4 times with deionized water at a speed of 3500r / min, and vacuum dried at 75°C for 24 hours to obtain modified small-sized alumina.

[0076] Preparation of thermally conductive filler: According to the size settings of modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina in the thermally conductive filler, the corresponding thermally conductive filler was added to dimethylformamide, the solution was ultrasonically treated for 1 hour, and then heated and stirred at 95°C for 3 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain the corresponding thermally conductive filler.

[0077] Preparation of epoxy molding compound: 140 parts of corresponding thermal conductive fillers are mixed with 9 parts of o-cresol epoxy resin, 3 parts of bisphenol A epoxy resin, and 8 parts of linear phenolic resin at high speed to form corresponding mixtures; 0.5 parts of 2-methylimidazole, 3 parts of triphenyl phosphate, 0.3 parts of γ-aminopropyl triethoxysilane, 0.4 parts of carboxyl-terminated liquid nitrile rubber, 0.2 parts of IXE500, 0.5 parts of carnauba wax, and 0.2 parts of carbon black are added to the corresponding mixtures respectively, and mixed at high speed to obtain corresponding premixes;

[0078] The corresponding premixes were extruded through a twin-screw extruder at a temperature of 110° C. and a screw speed of 80 rpm, and the obtained molten mixed materials were cooled, crushed, magnetically separated, and preformed to obtain the corresponding epoxy molding compound.

[0079] The thermal conductivity and fluidity of the corresponding epoxy molding compounds were tested, and the data shown in Table 3 were obtained.

[0080] Table 3 Thermal conductivity and flow properties of epoxy molding compound under different raw material sizes of thermal conductive fillers

[0081]

[0082] The appropriate hexagonal boron nitride sheet diameter can form a heat conduction network more effectively. If the hexagonal boron nitride sheet diameter is too large, the pores between the fillers are large, which is not conducive to the formation of a heat conduction network. When hexagonal boron nitride with an appropriate sheet diameter is combined with alumina of different sizes, the particles have the best stacking state, which reduces the voids in the inner wall of the material and enhances the ability of the particles to contact each other to form a heat conduction path.

[0083] Example 4: Investigating the effect of the preparation method of modified hexagonal boron nitride on the thermal conductivity and flow properties of epoxy packaging materials

[0084] Hexagonal boron nitride modified with polydopamine, hexagonal boron nitride modified with amino, and unmodified hexagonal boron nitride were selected respectively.

[0085] Then proceed as follows:

[0086] Preparation of hexagonal boron nitride modified by polydopamine: Weigh hexagonal boron nitride with a sheet diameter of 10 μm, add it to a mixed solution of ethanol and water with a volume ratio of 1:1, stir it ultrasonically at 25°C for 2 hours, adjust the pH of the solution to 8 with dilute hydrochloric acid, and stir it at 60°C for 30 minutes. Add dopamine hydrochloride to the above solution in an amount of 12% of the hexagonal boron nitride, and continue stirring for 2 hours. Wash the product by centrifugation with deionized water 4 times at a speed of 3500r / min until the upper dispersion is neutral, and vacuum dry it at 75°C for 24 hours to obtain modified hexagonal boron nitride.

[0087] The preparation of the amino-modified hexagonal boron nitride is carried out according to conventional methods in the prior art.

[0088] Preparation of modified large-size alumina: Spherical alumina with an average particle size of 2 μm and γ-aminopropyltriethoxysilane (KH550) were added to anhydrous ethanol, the amount of KH550 was 6% of the mass of the spherical alumina, and ultrasonic treatment was performed for 1 hour. Deionized water was added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain modified large-size alumina.

[0089] Preparation of modified small-sized alumina: Spherical alumina with an average particle size of 0.3 μm and γ-aminopropyltriethoxysilane (KH550) were added to anhydrous ethanol, the amount of KH550 was 6% of the mass of the spherical alumina, and ultrasonic treatment was performed for 1 hour. Deionized water was added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain modified small-sized alumina.

[0090] Preparation of thermally conductive filler: According to the above settings, hexagonal boron nitride modified with polydopamine, hexagonal boron nitride modified with amino, and unmodified hexagonal boron nitride are selected respectively. The ratio of modified (or unmodified) hexagonal boron nitride, modified small-size alumina and modified large-size alumina in the thermally conductive filler is 5:1:2. The corresponding thermally conductive filler is added to dimethylformamide, the solution is ultrasonically treated for 1 hour, and then heated and stirred at 95°C for 3 hours. The product is centrifuged and washed 4 times with deionized water at a speed of 3500r / min, and vacuum dried at 75°C for 24 hours to obtain the corresponding thermally conductive filler.

[0091] Preparation of epoxy molding compound: 140 parts of corresponding thermal conductive fillers are mixed with 9 parts of o-cresol epoxy resin, 3 parts of bisphenol A epoxy resin, and 8 parts of linear phenolic resin at high speed to form corresponding mixtures; 0.5 parts of 2-methylimidazole, 3 parts of triphenyl phosphate, 0.3 parts of γ-aminopropyl triethoxysilane, 0.4 parts of carboxyl-terminated liquid nitrile rubber, 0.2 parts of IXE500, 0.5 parts of carnauba wax, and 0.2 parts of carbon black are added to the corresponding mixtures respectively, and mixed at high speed to obtain corresponding premixes;

[0092] The corresponding premixes were extruded through a twin-screw extruder at a temperature of 110° C. and a screw speed of 80 rpm, and the obtained molten mixed materials were cooled, crushed, magnetically separated, and preformed to obtain the corresponding epoxy molding compound.

[0093] The thermal conductivity and fluidity of the corresponding epoxy molding compounds were tested, and the data shown in Table 4 were obtained.

[0094] Table 4 Thermal conductivity and flow properties of epoxy molding compound under different hexagonal boron nitride conditions

[0095]

[0096] After hexagonal boron nitride is modified with polydopamine, its surface has abundant amino, imino, catechol and other functional groups, and its surface reactivity is high. Functional polymers can be further grafted to improve the performance of thermal conductive fillers. Compared with unmodified hexagonal boron nitride and amino-modified hexagonal boron nitride, its dispersibility in epoxy resin is significantly enhanced, forming a denser phonon transmission network.

[0097] Example 5: Investigating the effect of the ratio of the epoxy resin composition to the thermal conductive filler on the thermal conductivity and fluidity of the epoxy molding compound

[0098] Different groups of experiments were set up, Group A: According to the mass fraction, the mass amount of the epoxy resin composition was 12 parts, and the amount of the thermally conductive filler was 75 parts. Group B: According to the mass fraction, the mass amount of the epoxy resin composition was 12 parts, and the amount of the thermally conductive filler was 100 parts. Group C: According to the mass fraction, the mass amount of the epoxy resin composition was 12 parts, and the amount of the thermally conductive filler was 140 parts. Group D: According to the mass fraction, the mass amount of the epoxy resin composition was 12 parts, and the amount of the thermally conductive filler was 160 parts. Group E: According to the mass fraction, the mass amount of the epoxy resin composition was 12 parts, and the amount of the thermally conductive filler was 200 parts. Group F: According to the mass fraction, the mass amount of the epoxy resin composition was 12 parts, and the amount of the thermally conductive filler was 260 parts.

[0099] The epoxy resin composition is o-cresol novolac epoxy resin and bisphenol A epoxy resin, and the ratio of o-cresol novolac epoxy resin to bisphenol A epoxy resin is 9:3. The mass ratio of the modified hexagonal boron nitride, the modified small-sized alumina and the modified large-sized alumina is 5:1:2.

[0100] Then proceed as follows:

[0101] Preparation of modified hexagonal boron nitride: Weigh hexagonal boron nitride, add it to a mixed solution of ethanol and water in a volume ratio of 1:1, stir it ultrasonically at 25°C for 2h, adjust the pH of the solution to 8 with dilute hydrochloric acid, and stir it at 60°C for 30min. Add dopamine hydrochloride to the above solution in an amount of 12% of the hexagonal boron nitride, and continue stirring for 2h. Wash the product by centrifugation with deionized water for 4 times at a speed of 3500r / min until the upper dispersion is neutral, and vacuum dry it at 75°C for 24h to obtain modified hexagonal boron nitride.

[0102] Preparation of modified large-size alumina: Spherical alumina with an average particle size of 2 μm and γ-aminopropyltriethoxysilane (KH550) were added to anhydrous ethanol, the amount of KH550 was 6% of the mass of the spherical alumina, and ultrasonic treatment was performed for 1 hour. Deionized water was added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain modified large-size alumina.

[0103] Preparation of modified small-sized alumina: Spherical alumina with an average particle size of 0.3 μm and γ-aminopropyltriethoxysilane (KH550) were added to anhydrous ethanol, the amount of KH550 was 6% of the mass of the spherical alumina, and ultrasonic treatment was performed for 1 hour. Deionized water was added to the mixed solution, and heated and stirred at 85°C for 2 hours. The product was centrifuged and washed 4 times with deionized water at a speed of 3500 r / min, and vacuum dried at 75°C for 24 hours to obtain modified small-sized alumina.

[0104] Preparation of thermally conductive filler: Add the raw materials of thermally conductive filler into dimethylformamide, ultrasonically treat the solution for 1 hour, then heat and stir at 95°C for 3 hours, centrifuge and wash the product with deionized water for 4 times at a speed of 3500r / min, and vacuum dry at 75°C for 24 hours to obtain a thermally conductive filler.

[0105] Preparation of epoxy molding compound: according to the corresponding proportions of the epoxy resin and the thermal conductive filler, the epoxy resin and the thermal conductive filler are mixed at high speed to form a corresponding mixture; 0.5 parts of 2-methylimidazole, 3 parts of triphenyl phosphate, 0.3 parts of γ-aminopropyl triethoxysilane, 0.4 parts of carboxyl-terminated liquid nitrile rubber, 0.2 parts of IXE500, 0.5 parts of carnauba wax, and 0.2 parts of carbon black are added to the corresponding mixture, and mixed at high speed to obtain a corresponding premix;

[0106] The corresponding premixes were extruded through a twin-screw extruder at a temperature of 110° C. and a screw speed of 80 rpm, and the obtained molten mixed materials were cooled, crushed, magnetically separated, and preformed to obtain the corresponding epoxy molding compound.

[0107] The thermal conductivity and fluidity of the corresponding epoxy molding compounds were tested, and the data shown in Table 5 were obtained.

[0108] Table 5 Thermal conductivity and flow properties of epoxy molding compound at different proportions of thermal conductive filler and epoxy resin

[0109]

[0110] It can be seen from Table 5 above that under the same conditions, as the amount of thermal conductive filler increases, the thermal conductivity of the epoxy molding compound increases and the fluidity decreases. By adjusting the proportion of thermal conductive filler, epoxy molding compounds with different thermal conductivity coefficients and fluidity can be prepared.

[0111] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0112] The present invention has been described in detail above. The above description is only a preferred embodiment of the present invention and should not limit the scope of implementation of the present invention. That is, all equivalent changes and modifications made within the scope of this application should still fall within the scope of the present invention.

Claims

1. A method for preparing a thermally conductive filler, characterized in that: The preparation method comprises: mixing modified hexagonal boron nitride, modified large-size alumina and modified small-size alumina in an organic solvent, performing ultrasonic treatment, and then heating and removing water to obtain a thermal conductive filler; The modified hexagonal boron nitride is hexagonal boron nitride modified with polydopamine; The modified large-size alumina and the modified small-size alumina are respectively alumina modified by a silane coupling agent; The mass ratio of the modified hexagonal boron nitride, the modified small-sized alumina and the modified large-sized alumina is 5:1:2; The average particle size of the modified large-size alumina is 2 μm; the average particle size of the modified small-size alumina is 0.3 μm; The average flake diameter of the modified hexagonal boron nitride is 5 μm.

2. The method for preparing a thermally conductive filler according to claim 1, characterized in that: The modified hexagonal boron nitride, modified large-sized alumina and modified small-sized alumina are mixed and ultrasonically treated in an organic solvent for 0.5-3 hours; the modified hexagonal boron nitride, modified large-sized alumina and modified small-sized alumina are mixed and ultrasonically treated in an organic solvent and then heated for 2-4 hours at a heating temperature of 85-105°C. The dehydration process comprises: centrifugal washing with deionized water for 3-5 times at a centrifugal speed of 3000-4000 r / min and vacuum drying at 65-85°C.

3. The method for preparing a thermally conductive filler according to claim 1, characterized in that: The preparation process of the modified large-size alumina is as follows: spherical alumina with a particle size of 1-5 μm and a silane coupling agent are added to anhydrous ethanol for ultrasonication for 0.5-3 hours, followed by heating for 2-4 hours at a heating temperature of 85-105° C., and centrifugation drying to obtain the modified large-size alumina; In terms of mass percentage, the amount of silane coupling agent required for modifying large-sized alumina is 1-10% of spherical alumina with a particle size of 1-5 μm; The preparation process of the modified small-sized alumina is as follows: spherical alumina with a particle size of 0.1-0.9 μm and a silane coupling agent are added to anhydrous ethanol for ultrasonication for 0.5-3 hours, followed by heating for 2-4 hours at a heating temperature of 85-105° C., and centrifugation drying to obtain the modified small-sized alumina; Calculated by mass percentage, the amount of silane coupling agent required for modifying large-size alumina is 1-10% of the spherical alumina with a particle size of 0.1-0.9 μm.

4. The method for preparing a thermally conductive filler according to claim 1, characterized in that: The preparation process of the modified hexagonal boron nitride is as follows: the hexagonal boron nitride has a sheet diameter of 1-20 μm, the hexagonal boron nitride is added to an ethanol solution for ultrasonication, the pH value is adjusted to 8-9 after ultrasonication, dopamine hydrochloride is added to the above solution and continued to be stirred, and the modified hexagonal boron nitride is obtained by centrifugation and drying, and the amount of dopamine hydrochloride added is 10-15% of the mass of the hexagonal boron nitride.

5. A thermally conductive filler, characterized in that: The thermally conductive filler is prepared by the preparation method of the thermally conductive filler according to any one of claims 1 to 4.

6. An epoxy molding compound, characterized in that: The invention comprises epoxy resin and the thermally conductive filler as claimed in claim 5.

7. The epoxy molding compound according to claim 6, characterized in that: The mass ratio of the epoxy resin to the thermal conductive filler is 12:120-200.

8. The epoxy molding compound according to claim 6, characterized in that: The epoxy resin includes at least one of biphenyl epoxy resin, o-cresol epoxy resin, glycidyl ether epoxy resin, multifunctional epoxy resin, bisphenol A epoxy resin and bisphenol F epoxy resin.