A kind of 304 stainless steel and its preparation method and application
By optimizing the smelting process of 304 stainless steel, its tensile strength and plasticity are improved, the problem of low performance of domestic stainless steel wire is solved, and the preparation of high-performance steel wire for the reinforcement layer of polytetrafluoroethylene hose is achieved.
Patent Information
- Application Number
- CN202410889254.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The tensile strength and plasticity of domestic 304 stainless steel wire are lower than imported products, which affects the stability and applicability of the steel wire reinforcement layer of PTFE hoses.
By optimizing the smelting process of 304 stainless steel, including heating industrial pure iron, electrolytic manganese, metallic chromium, metallic nickel and high-purity graphite in a resistance furnace, adding aluminum particles and rare earths for deoxidation reaction, followed by high-temperature forging and solid solution treatment, it is prepared The ingredients are C: ≤0.02wt%, Si: ≤0.5wt%, Mn: 2.0~4.0wt%, Cr : 24.0~25.0wt%, RE: 0.020~0.042wt%, Ni: 21.0~23.0wt%, Al: 7.0~8.0wt%, N: 0.45~0.55wt%, S: ≤0.005wt%, O: ≤0.005 wt%, P: ≤0.03wt% 304 stainless steel.
The tensile strength and plasticity of 304 stainless steel are significantly improved, making it suitable for steel wire for the reinforcement layer of polytetrafluoroethylene hoses, and has wide application value and prospects.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of metallurgy, and in particular to 304 stainless steel and a preparation method and application thereof. Background Art
[0002] The polytetrafluoroethylene hose consists of four parts: inner tube, steel wire reinforcement layer, rubber layer and metal connectors. It is mainly used in aircraft engine systems. The steel wire reinforcement layer of the polytetrafluoroethylene hose plays a pressure-bearing role, and its pressure-bearing capacity mainly depends on the mechanical properties of the steel wire. At present, the steel wire of the hose reinforcement layer at home and abroad is usually made of 304 austenitic stainless steel through a drawing process, but there is still a certain gap between the existing domestic steel wire products and imported products in terms of tensile strength and plasticity. Through comparative testing and analysis of 0.20 mm steel wire imported from Japan and domestic steel wire, it is found that the average tensile strength of domestic steel wire is about 400 MPa lower than that of imported steel wire, which directly affects the stability and applicability of the steel wire reinforcement layer of the polytetrafluoroethylene hose in my country.
[0003] A feasible way to improve the tensile strength and plasticity of 304 stainless steel wire is to optimize the smelting process of 304 stainless steel, thereby achieving the improvement of the tensile strength and plasticity of 304 stainless steel. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a 304 stainless steel and a preparation method and application thereof.
[0005] In the first aspect of the present invention, the present invention provides a method for preparing 304 stainless steel. According to a specific embodiment of the present invention, the method comprises:
[0006] S1: putting industrial pure iron, electrolytic manganese, metallic chromium, metallic nickel and high-purity graphite into a resistance furnace, and heating the resistance furnace;
[0007] S2: adding aluminum particles and rare earth RE in sequence to carry out deoxidation reaction;
[0008] S3: Cooling down the resistance furnace to obtain a 304 stainless steel ingot;
[0009] S4: subjecting the 304 stainless steel ingot to high temperature forging and solution treatment, and obtaining 304 stainless steel after cooling.
[0010] In the second aspect of the present invention, the present invention provides a 304 stainless steel. According to a specific embodiment of the present invention, the composition of the 304 stainless steel includes: C: ≤0.02wt%, Si: ≤0.5wt%, Mn: 2.0-4.0wt%, Cr: 24.0-25.0wt%, RE: 0.020-0.042wt%, Ni: 21.0-23.0wt%, Al: 7.0-8.0wt%, N: 0.45-0.55wt%, S: ≤0.005wt%, O: ≤0.005wt%, P: ≤0.03wt%, and the balance is Fe and other inevitable impurity elements.
[0011] In the third aspect of the present invention, the present invention provides an application of the 304 stainless steel described in the second aspect. According to a specific embodiment of the present invention, the application includes application of the 304 stainless steel in a polytetrafluoroethylene hose.
[0012] The beneficial effects of the present invention are:
[0013] By alloying 304 stainless steel with rare earths, the tensile strength and plasticity are effectively improved. It can be used to make steel wire for the reinforcement layer of polytetrafluoroethylene hoses, and has broad application value and prospects.
[0014] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0015] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but should not be construed as limiting the present invention.
[0016] In the first aspect of the present invention, the present invention provides a method for preparing 304 stainless steel. According to a specific embodiment of the present invention, the method comprises:
[0017] S1: Put industrial pure iron, electrolytic manganese, metallic chromium, metallic nickel and high-purity graphite into a resistance furnace, and heat the resistance furnace.
[0018] In this step, the weight of the required raw materials is calculated according to the elemental composition of the target steel grade, and the smelting raw materials are prepared. Specifically, industrial pure iron, electrolytic manganese, metal chromium, metal nickel and high-purity graphite are added to a high-purity magnesium oxide crucible, and then the outer graphite crucible and sleeve are placed in a resistance furnace, and the resistance furnace is heated to obtain molten raw materials.
[0019] In some embodiments, the purity of the industrial pure iron is 99.9-100wt%, and the purity of the high-purity graphite is 99.9-100wt%.
[0020] Specifically, the heating of the resistance furnace includes two steps:
[0021] Sa. When heated to a temperature of 400~600 ℃, introduce argon gas at a flow rate of 4~6 L / min.
[0022] In this step, the resistance furnace is powered on to increase the temperature at a rate of 5-8 °C / min. When the temperature rises to 400-600 °C, argon gas is introduced at a flow rate of 4-6 L / min to exhaust as much air as possible from the furnace.
[0023] Sb, heat to a temperature of 1550~1650 ℃ and keep the temperature constant for 5~15 min.
[0024] In this step, the resistance furnace is powered on and the temperature is raised at a rate of 3-5 °C / min. When the temperature rises to 1550-1650 °C, the temperature is kept constant for 5-15 min to ensure that the raw materials are completely melted.
[0025] S2: Aluminum particles and rare earth RE are added in sequence to carry out deoxidation reaction.
[0026] In this step, aluminum particles and rare earth RE are added in sequence for deoxidation reaction. Specifically, aluminum particles are first added for pre-deoxidation reaction, the temperature of the pre-deoxidation reaction is 1550-1650°C, and the time is 1-3 min; then rare earth RE is added for deep deoxidation reaction, the temperature of the deep deoxidation reaction is 1550-1650°C, and the time is 30-40 min, so as to ensure that rare earth RE reacts fully with molten steel.
[0027] In some embodiments, the rare earth RE is any one of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, yttrium, and scandium, or a mixture of any two or more thereof.
[0028] In some embodiments, the addition amount of the rare earth RE is controlled to be 0.06-0.11wt% of the smelting raw material, preferably 0.06-0.09wt%, for example 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, 0.10wt%, 0.11wt%, etc.
[0029] S3: Cooling down the resistance furnace.
[0030] In this step, the resistance furnace is cooled to obtain a 304 stainless steel ingot. Specifically, the cooling rate is 5-8 °C / min, and the argon flow rate is adjusted to 2-3 L / min. When the furnace temperature drops to 100-200 °C, the argon flow rate is adjusted to zero.
[0031] S4: High temperature forging and solution treatment of 304 stainless steel ingot.
[0032] In this step, in order to forge the internal defects of the molten steel generated during casting, such as bubble-type cavities, looseness and shrinkage cavities, and at the same time improve the structure of the stainless steel, thereby improving the mechanical properties of the stainless steel, the above-mentioned ingot is further forged at high temperature to obtain a forged square rod, and then the forged square rod is solution treated and cooled to obtain 304 stainless steel.
[0033] In some embodiments, the high temperature forging includes heat preservation, initial forging and final forging, the heat preservation temperature is 1100~1180℃, the time is 1~2h; the initial forging temperature is 1130~1150℃; the final forging temperature is 850~900℃.
[0034] In some embodiments, the solution treatment is performed in a muffle furnace at a temperature of 1030-1070° C. for a time of 0.4-0.6 h.
[0035] In a second aspect of the present invention, the present invention provides a 304 stainless steel. According to a specific embodiment of the present invention, the composition of the 304 stainless steel includes: C: ≤0.02wt%, Si: ≤0.5wt%, Mn: 2.0-4.0wt%, Cr: 24.0-25.0wt%, RE: 0.020-0.042wt%, Ni: 21.0-23.0wt%, Al: 7.0-8.0wt%, N: 0.45-0.55wt%, S: ≤0.005wt%, O: ≤0.005wt%, P: ≤0.03wt%, and the balance is Fe and other inevitable impurity elements.
[0036] In some embodiments, the cross-sectional reduction rate of the 304 stainless steel is 79-82%, for example, 79%, 80%, 81%, 82%, etc.
[0037] In some embodiments, the tensile strength of the 304 stainless steel is 690-715 MPa, for example, 690 MPa, 695 MPa, 700 MPa, 705 MPa, 710 MPa, 715 MPa, etc.
[0038] In some embodiments, the elongation of the 304 stainless steel is 58-61%, for example, 58%, 59%, 60%, 61%, etc.
[0039] In the third aspect of the present invention, the present invention provides an application of the 304 stainless steel described in the second aspect. According to a specific embodiment of the present invention, the application includes application of the 304 stainless steel in a polytetrafluoroethylene hose.
[0040] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Example 1
[0042] (1) Raw materials including industrial pure iron, electrolytic manganese, metallic chromium, metallic nickel and high-purity graphite with a total weight of about 600 g are placed in a 99wt% high-purity magnesium oxide crucible with a size of Φ62 mm × 72 mm. Then the outer graphite crucible and sleeve are placed in a 1kg molybdenum disilicide resistance furnace, and the resistance furnace is heated:
[0043] a. Control the heating rate to 8 ℃ / min. When the temperature rises to 600 ℃, introduce argon at a flow rate of 5 L / min.
[0044] b. Control the heating rate to 5 ℃ / min. When the temperature reaches 1600 ℃, keep it constant for 10 min.
[0045] (2) First, add 0.27 g aluminum particles for pre-deoxidation, the pre-deoxidation reaction temperature is 1600 ° C, and the time is 2 min; after the aluminum particles are melted, add 0.36 g rare earth Ce for deep deoxidation, the deep deoxidation reaction temperature is 1600 ° C, and the time is 30 min to ensure that the rare earth and the steel liquid react fully;
[0046] (3) The current of the molybdenum disilicide resistance furnace was manually adjusted to zero and the temperature was started to drop, wherein the cooling rate was 8 °C / min, and the argon flow rate was adjusted to 2.5 L / min. When the furnace temperature dropped to 100 °C, the argon flow rate was adjusted to zero, and after cooling, a 304 stainless steel ingot was obtained;
[0047] (4) The 304 stainless steel ingot is subjected to high temperature forging, wherein the holding temperature is 1150°C for 1.5 h; the initial forging temperature is 1150°C; the final forging temperature is 850°C, and a 22 mm × 12 mm square bar is obtained by forging; then, the ingot is heated from room temperature to 1050°C in a muffle furnace, held for 0.5 h, and then rapidly water-cooled to obtain a product with a single structure and uniform performance.
[0048] Example 2
[0049] In step (2), the amount of rare earth Ce added is 0.54 g, and the rest is the same as in Example 1.
[0050] Example 3
[0051] In step (2), the amount of rare earth Ce added is 0.66 g, and the rest is the same as in Example 1.
[0052] Comparative Example 1
[0053] In step (2), the amount of rare earth Ce added is 0.72 g, and the rest is the same as in Example 1.
[0054] Comparative Example 2
[0055] In step (2), no rare earth Ce is added, and the rest is the same as in Example 1.
[0056] Table 1 Chemical composition of 304 stainless steel (mass fraction / %)
[0057]
[0058] Table 2 Room temperature tensile results of 304 stainless steel
[0059] serial number Tensile strength / MPa Elongation / % Sectional shrinkage / % Example 1 713.9 60.2 80.5 Example 2 702.1 61.0 81.2 Example 3 691.6 58.4 79.3 Comparative Example 1 659.4 54.5 79.6 Comparative Example 2 673.4 47.7 78.9
[0060] Table 1 shows the chemical composition of 304 stainless steel in various embodiments and comparative examples, and Table 2 shows the tensile test results of 304 stainless steel in various embodiments and comparative examples at room temperature according to GB / T228-2002. From the data, adding rare earth to 304 stainless steel can significantly increase the tensile strength, elongation and cross-sectional shrinkage of stainless steel. The present invention effectively improves the tensile strength and plasticity by alloying 304 stainless steel with rare earth, and can be used to make steel wire for reinforcing layer of polytetrafluoroethylene hose, which has wide application value and prospects.
[0061] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0062] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing 304 stainless steel, characterized in that: The method comprises: (1) Putting raw materials including industrial pure iron, electrolytic manganese, metallic chromium, metallic nickel and high-purity graphite with a total weight of 600 g into a resistance furnace, and heating the resistance furnace; (2) adding aluminum particles and rare earth Ce in sequence to carry out deoxidation reaction; (3) Cooling the resistance furnace to obtain a 304 stainless steel ingot; (4) subjecting the 304 stainless steel ingot to high temperature forging and solution treatment, and obtaining 304 stainless steel after cooling; In step (1), the resistance furnace is heated: a. Control the heating rate to 8 ℃ / min. When the temperature rises to 600 ℃, introduce argon at a flow rate of 5 L / min. b. Control the heating rate to 5 ℃ / min. When the temperature rises to 1600 ℃, keep the temperature constant for 10 min. In step (2), 0.27 g of aluminum particles are added for a pre-deoxidation reaction at a temperature of 1600°C for 2 min. After the aluminum particles are melted, 0.36 g of rare earth Ce is added for a deep deoxidation reaction at a temperature of 1600°C for 30 min. In step (3), the cooling process: the cooling rate is controlled to be 8°C / min, and the argon flow rate is adjusted to 2.5L / min. When the furnace temperature drops to 100°C, the argon flow rate is adjusted to zero; In step (4), the high temperature forging includes heat preservation, initial forging and final forging, the heat preservation temperature is 1150°C, the time is 1.5 h; the initial forging temperature is 1150°C; the final forging temperature is 850°C; then heating from room temperature to 1050°C, keeping the temperature for 0.5 h and then rapid water cooling; The composition of the 304 stainless steel is: C: 0.035wt%, Si: 0.007wt%, Mn: 0.97wt%, Cr: 18.75wt%, Ce: 0.020wt%, Ni: 8.1wt%, Al: 0.048wt%, N: 0.0057wt%, S: 0.003wt%, O: 0.0004wt%, P: 0.004wt%, and the balance is Fe and other inevitable impurity elements; The 304 stainless steel has a cross-sectional shrinkage of 80.5%, a tensile strength of 713.9 MPa, and an elongation of 60.2%.
2. A method for preparing 304 stainless steel, characterized in that: The method comprises: (1) Putting raw materials including industrial pure iron, electrolytic manganese, metallic chromium, metallic nickel and high-purity graphite with a total weight of 600 g into a resistance furnace, and heating the resistance furnace; (2) adding aluminum particles and rare earth Ce in sequence to carry out deoxidation reaction; (3) Cooling the resistance furnace to obtain a 304 stainless steel ingot; (4) subjecting the 304 stainless steel ingot to high temperature forging and solution treatment, and obtaining 304 stainless steel after cooling; In step (1), the resistance furnace is heated: a. Control the heating rate to 8 ℃ / min. When the temperature rises to 600 ℃, introduce argon at a flow rate of 5 L / min. b. Control the heating rate to 5 ℃ / min. When the temperature reaches 1600 ℃, keep the temperature constant for 10 min. In step (2), 0.27 g of aluminum particles are added for a pre-deoxidation reaction at a temperature of 1600°C for 2 min. After the aluminum particles are melted, 0.54 g of rare earth Ce is added for a deep deoxidation reaction at a temperature of 1600°C for 30 min. In step (3), the cooling process: the cooling rate is controlled to be 8°C / min, and the argon flow rate is adjusted to 2.5L / min. When the furnace temperature drops to 100°C, the argon flow rate is adjusted to zero; In step (4), the high temperature forging includes heat preservation, initial forging and final forging, the heat preservation temperature is 1150°C, the time is 1.5 h; the initial forging temperature is 1150°C; the final forging temperature is 850°C; then heating from room temperature to 1050°C, keeping the temperature for 0.5 h and then rapid water cooling; The composition of the 304 stainless steel is: C: 0.032wt%, Si: 0.024wt%, Mn: 1.08wt%, Cr: 18.71wt%, Ce: 0.029wt%, Ni: 8.27wt%, Al: 0.050wt%, N: 0.0052wt%, S: 0.003wt%, O: 0.0008wt%, P: 0.004wt%, and the balance is Fe and other inevitable impurity elements; The 304 stainless steel has a cross-sectional shrinkage of 81.2%, a tensile strength of 702.1 MPa, and an elongation of 61.0%.
3. A method for preparing 304 stainless steel, characterized in that: The method comprises: (1) Putting raw materials including industrial pure iron, electrolytic manganese, metallic chromium, metallic nickel and high-purity graphite with a total weight of 600 g into a resistance furnace, and heating the resistance furnace; (2) adding aluminum particles and rare earth Ce in sequence to carry out deoxidation reaction; (3) Cooling the resistance furnace to obtain a 304 stainless steel ingot; (4) subjecting the 304 stainless steel ingot to high temperature forging and solution treatment, and obtaining 304 stainless steel after cooling; In step (1), the resistance furnace is heated: a. Control the heating rate to 8 ℃ / min. When the temperature rises to 600 ℃, introduce argon at a flow rate of 5 L / min. b. Control the heating rate to 5 ℃ / min. When the temperature reaches 1600 ℃, keep the temperature constant for 10 min. In step (2), 0.27 g of aluminum particles are added for a pre-deoxidation reaction at a temperature of 1600°C for 2 min. After the aluminum particles are melted, 0.66 g of rare earth Ce is added for a deep deoxidation reaction at a temperature of 1600°C for 30 min. In step (3), the cooling process: the cooling rate is controlled to be 8°C / min, and the argon flow rate is adjusted to 2.5L / min. When the furnace temperature drops to 100°C, the argon flow rate is adjusted to zero; In step (4), the high temperature forging includes heat preservation, initial forging and final forging, the heat preservation temperature is 1150°C, the time is 1.5 h; the initial forging temperature is 1150°C; the final forging temperature is 850°C; then heating from room temperature to 1050°C, keeping the temperature for 0.5 h and then rapid water cooling; The composition of the 304 stainless steel is: C: 0.037wt%, Si: 0.022wt%, Mn: 1.18wt%, Cr: 18.67wt%, Ce: 0.042wt%, Ni: 8.36wt%, Al: 0.053wt%, N: 0.0053wt%, S: 0.003wt%, O: 0.0010wt%, P: 0.003wt%, and the balance is Fe and other inevitable impurity elements; The 304 stainless steel has a cross-sectional shrinkage of 79.3%, a tensile strength of 691.6 MPa, and an elongation of 58.4%.
Citation Information
Cited By
Antique processing technology for stainless steel surface
CN122038705A