A surface modified graphite negative electrode material, preparation method and application thereof
By covering the LiX-doped binary sulfide electrolyte and ternary sulfide electrolyte on the surface of the graphite negative electrode, the inner and outer cladding structure is formed, and the side reaction problem between the graphite negative electrode and the sulfide electrolyte is solved, and the battery's magnification and circulation are improved. Performance, suitable for industrial applications.
Patent Information
- Application Number
- CN202410891479.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The graphite negative electrode is prone to side reactions with the sulfide electrolyte in a sulfide all-solid state battery, resulting in poor ion conduction and electron capacity of the side reaction product and low ion conductivity, affecting the rate performance.
By covering the LiX-doped binary sulfide electrolyte and ternary sulfide electrolyte on the surface of the graphite negative electrode, an inner and outer cladding structure is formed to suppress side reactions and improve the lithium ion transmission rate.
It effectively inhibits the side reaction between graphite and sulfide electrolyte, improves the rate performance and circulation performance of the battery, and is suitable for industrial applications.
Smart Images

Figure CN118431453B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid-state batteries, and in particular to a surface-modified graphite negative electrode material, a preparation method thereof and an application thereof. Background Art
[0002] Graphite has become an excellent negative electrode material due to its advantages of low cost, low lithium potential and high reversible lithium ion insertion and extraction. It has great application prospects in the field of all-solid-state batteries. However, the graphite negative electrode still has the following problems in sulfide all-solid-state batteries, which hinder its further industrial application:
[0003] 1. The potential of the graphite negative electrode lithium insertion platform is low, which is 0.1V (vs. Li / Li + ), its contact with the sulfide electrolyte can easily lead to side reactions at the interface between the two, that is, the sulfide electrolyte is partially reduced to obtain side reaction products, which have poor ion and electron conductivity;
[0004] 2. The contact between the graphite end face and the sulfide electrolyte is random. If the contact area between the graphite end face and the electrolyte becomes smaller, the negative electrode rate performance will deteriorate. In addition, the low ionic conductivity of the electrolyte coating layer is not conducive to improving the rate performance.
[0005] In order to suppress the side reactions between the sulfide electrolyte and the graphite negative electrode, studies have shown that when preparing a composite negative electrode comprising graphite and an electrolyte, replacing the current argyrodite-type electrolyte with a new electrolyte obtained by doping a binary sulfide electrolyte with LiI can suppress the side reactions. Although this method suppresses the occurrence of side reactions, the ionic conductivity of the LiI-doped binary sulfide electrolyte (1mS / cm) is significantly lower than that of the ionic conductivity of the argyrodite-type electrolyte (>5mS / cm), which is not conducive to improving the rate performance. Summary of the invention
[0006] The main purpose of the present invention is to provide a surface modified graphite negative electrode material, a preparation method and application thereof, so as to solve the problems in the prior art that the graphite negative electrode is easy to react with the sulfide electrolyte to generate harmful side reaction products, the ionic conductivity of the composite negative electrode is low, and the rate performance is poor.
[0007] In order to achieve the above-mentioned object, according to a first aspect of the present invention, a surface-modified graphite negative electrode material is provided, which comprises a graphite core, an inner coating layer and an outer coating layer, wherein the inner coating layer is located on the surface of the graphite core, and the outer coating layer is located on the surface of the inner coating layer; the material of the inner coating layer is a binary sulfide electrolyte doped with LiX, and the material of the outer coating layer is a ternary sulfide electrolyte; wherein X is a halogen element; in addition, the mass ratio of the graphite core, the inner coating layer and the outer coating layer is (85-99.5): (0.25-5): (0.25-10).
[0008] Furthermore, in the material of the inner coating layer, the molar ratio of LiX to the binary sulfide electrolyte is 1:(0.5-5).
[0009] Furthermore, the mass ratio of the graphite core, the inner coating layer, and the outer coating layer is (95-97):(1-4):(1-4); and / or, in the material of the inner coating layer, the molar ratio of LiX to the binary sulfide electrolyte is 1:(1-3).
[0010] Further, in the surface-modified graphite negative electrode material, X is one of Cl, Br, and I; and / or
[0011] Binary sulfide electrolytes are Li3PS4, Li7P3S 11 , Li4SnS4; and / or
[0012] The ternary sulfide electrolyte is a sulfide germanium argentum-type electrolyte, which is Li6PS5Cl, Li6PS5Br, Li6PS5I, Li 10 GeP2S 12 At least one of .
[0013] Furthermore, the above X is I, the binary sulfide electrolyte is Li3PS4, and the ternary sulfide electrolyte is Li6PS5Cl.
[0014] According to a second aspect of the present invention, there is provided a method for preparing a surface-modified graphite negative electrode material, comprising the following steps:
[0015] S1, coating a LiX-doped binary sulfide electrolyte on the graphite surface to obtain a graphite negative electrode material with an inner coating layer;
[0016] S2, coating the surface of the graphite negative electrode material having the inner coating layer with a ternary sulfide electrolyte to obtain a surface-modified graphite negative electrode material.
[0017] Furthermore, the coating methods in S1 and S2 are each independently at least one of a solid phase ball milling method, a magnetron sputtering method, a liquid phase coating method, and an atomic layer deposition (ALD) method.
[0018] Further, in S1, the coating method is a solid phase ball milling method, specifically: graphite, lithium sulfide, phosphorus pentasulfide, and LiX are mixed, ball milled, and kept in an inert atmosphere at 180-250° C. for 8-12 hours to obtain a graphite negative electrode material with an inner coating layer;
[0019] In S2, the coating method is a solid phase ball milling method, specifically: a ternary sulfide electrolyte is mixed with a graphite negative electrode material having an inner coating layer, and a surface-modified graphite negative electrode material is obtained by ball milling.
[0020] Furthermore, in S2, the preparation method of the ternary sulfide electrolyte is: lithium sulfide, phosphorus pentasulfide, and lithium chloride are mixed in proportion, and kept warm in an inert atmosphere at 500-600°C for 8-12 hours, and the D50 particle size of the ternary sulfide electrolyte is 0.5-1 μm.
[0021] According to a third aspect of the present invention, a composite negative electrode material is provided, which comprises a surface-modified graphite negative electrode material and a sulfide electrolyte, wherein the mass ratio of the surface-modified graphite negative electrode and the sulfide electrolyte is (50-100): (0-50); the surface-modified graphite negative electrode material is the surface-modified graphite negative electrode material of the first aspect of the present invention or the surface-modified graphite negative electrode material prepared by the preparation method of the second aspect of the present invention.
[0022] According to a fourth aspect of the present invention, there is also provided an all-solid-state lithium battery, which comprises the above-mentioned surface-modified graphite negative electrode material or composite negative electrode material.
[0023] By applying the technical solution of the present invention, the graphite negative electrode is modified, and the LiX-doped binary sulfide electrolyte and ternary sulfide electrolyte are coated on the surface from the inside to the outside, respectively, to solve the problems that the existing graphite negative electrode is easy to react with the electrolyte, and the ion conductivity is low and the rate performance is poor. The modification method of the present invention is simple, and the prepared negative electrode material has good electrical properties and is suitable for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The first cycle 0.05C charge-discharge curve diagram of the all-solid-state battery assembled by using the composite negative electrode materials of Example 1 and Comparative Examples 1-2;
[0025] Figure 2 The dQ / dV curve at 0.05C of the first cycle of the all-solid-state battery assembled by using the composite negative electrode material of Comparative Example 1;
[0026] Figure 3 is a dQ / dV curve at 0.05C of the first cycle of an all-solid-state battery assembled using the composite negative electrode material of Example 1;
[0027] Figure 4 The graph is a cycle performance test graph of an all-solid-state battery assembled with the composite negative electrode materials of Example 1 and Comparative Examples 1-2;
[0028] The above drawings include the following figure numbers: 1. Application Example 1; 2. Application Comparative Example 1; 3. Application Comparative Example 2. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0030] All-solid-state batteries use solid electrolytes, which do not contain flammable or volatile components, avoiding safety hazards such as battery smoke and fire caused by leakage. They have a wide operating temperature range and are safer. However, the interface impedance between the solid electrolyte and the electrode is large, the interface compatibility is poor, and the volume expansion and contraction of the material during the charge and discharge process easily lead to interface separation. These problems limit the further application of all-solid-state batteries.
[0031] The application of graphite as a negative electrode material is relatively mature. Compared with other negative electrode materials, its volume expansion rate when fully embedded with lithium ions is only 10%, so it is suitable for use in all-solid-state batteries. Sulfide electrolytes have the advantages of wide potential window, high voltage, fast transmission rate, no oxidation at high temperature, and no solidification at low temperature. They are widely used in all-solid-state batteries. However, graphite negative electrodes and high ionic conductivity sulfide electrolytes are prone to react to form side reaction products, which hinder the transmission of ions.
[0032] In order to solve the above problems, in a typical embodiment of the present invention, a surface modified graphite negative electrode material is provided, which comprises a graphite core, an inner coating layer and an outer coating layer, wherein the inner coating layer is located on the surface of the graphite core, and the outer coating layer is located on the surface of the inner coating layer, the material of the inner coating layer is a LiX-doped binary sulfide electrolyte, and the material of the outer coating layer is a ternary sulfide electrolyte; wherein X is a halogen element; in addition, the mass ratio of the graphite core, the inner coating layer and the outer coating layer is (85-99.5): (0.25-5): (0.25-10).
[0033] The binary sulfide electrolyte has good chemical stability and a certain ion conductivity. The present invention uses a LiX-doped binary sulfide electrolyte as an inner coating layer to coat the graphite surface, which can inhibit the reaction between the graphite and the high ion conductivity ternary sulfide electrolyte and reduce the interface impedance caused by the side reaction products; the ternary sulfide electrolyte outer coating layer is coated on the surface of the inner coating layer to improve the lithium ion transmission rate; through the above-mentioned double-layer coating, the above-mentioned inner coating layer is arranged between the ternary sulfide electrolyte outer coating layer and the graphite core, and the mass ratio of the graphite core, the inner coating layer and the outer coating layer is controlled, so that the generation of side reaction products can be inhibited while ensuring that the rate performance of the surface modified graphite negative electrode material will not be significantly affected.
[0034] As a preferred embodiment of the present invention, in the material of the inner coating layer, the molar ratio of LiX to the binary sulfide electrolyte is 1:(0.5-5).
[0035] Limiting the molar ratio of LiX to the binary sulfide electrolyte in the inner coating layer can reduce the probability of side reactions between the graphite core and the high ionic conductivity sulfide electrolyte, which is beneficial to improving its ion transfer rate and electron transfer rate.
[0036] As a preferred embodiment of the present invention, the mass ratio of the graphite core, the inner coating layer and the outer coating layer is (95-97): (1-4): (1-4); and / or, in the material of the inner coating layer, the molar ratio of LiX to the binary sulfide electrolyte is 1: (1-3).
[0037] The above-mentioned limitation on the mass ratio of LiX to the binary sulfide electrolyte is to improve the stability of the negative electrode material and further improve the rate performance of the negative electrode material.
[0038] As a preferred embodiment of the present invention, the above X is one of Cl, Br, and I; and / or the binary sulfide electrolyte is Li3PS4, Li7P3S 11 , Li4SnS4; and / or, the ternary sulfide electrolyte is a argyrodite-type electrolyte, the argyrodite-type electrolyte is Li6PS5Cl, Li6PS5Br, Li6PS5I, Li 10 GeP2S 12 At least one of .
[0039] Compared with other lithium halide materials, binary sulfide electrolytes doped with LiCl, LiBr, and LiI as inner coating layers have a better effect of preventing graphite from reacting with high ionic conductivity sulfide electrolytes, which is beneficial to improving the rate performance and cycle performance of the battery. The above binary sulfide electrolytes are commonly used binary sulfide electrolytes, have relatively high ionic conductivity and chemical stability, are easy to prepare, and are widely used in solid-state batteries; the above ternary sulfide electrolytes have better ionic conductivity.
[0040] As a preferred embodiment of the present invention, the above X is I, the binary sulfide electrolyte is Li3PS4, and the ternary sulfide electrolyte is Li6PS5Cl. The negative electrode material prepared with the above materials has the best electrical properties.
[0041] In another typical embodiment of the present invention, a method for preparing a surface-modified graphite negative electrode material is provided, which comprises the following steps:
[0042] S1, coating a LiX-doped binary sulfide electrolyte on the graphite surface to obtain a graphite negative electrode material with an inner coating layer;
[0043] S2, coating a ternary sulfide electrolyte on the surface of a graphite negative electrode material having an inner coating layer to obtain a surface-modified graphite negative electrode material;
[0044] Typically but not limiting, the coating methods in S1 and S2 are each independently at least one of solid phase ball milling, magnetron sputtering, liquid phase coating, and atomic layer deposition (ALD).
[0045] As a preferred embodiment of the present invention, in S1, the coating method is a solid phase ball milling method, which specifically comprises: mixing graphite, lithium sulfide, phosphorus pentasulfide, and LiX, ball milling, and keeping warm in an inert atmosphere at 180-250°C for 8-12 hours to obtain a graphite negative electrode material with an inner coating layer.
[0046] As a preferred embodiment of the present invention, in S2, the coating method is solid-phase ball milling, specifically: the ternary sulfide electrolyte is mixed with the graphite negative electrode material having an inner coating layer, and the surface-modified graphite negative electrode material is obtained by ball milling. The solid-phase ball milling method is to place the solid material in a container using a ball mill, and then add a certain amount of ball milling media. While the container is rotating, the ball milling media impacts, squeezes and rubs the solid material, so that the solid material is crushed and mixed; the solid-phase ball milling method is widely used in the preparation of nanomaterials, alloy powders, ceramic powders, metal abrasives, catalysts and other fields, and has the advantages of simple operation, low cost, and good controllability of the reaction process.
[0047] As a preferred embodiment of the present invention, in S2, the preparation method of the ternary sulfide electrolyte is: lithium sulfide, phosphorus pentasulfide, and lithium chloride are mixed in proportion, and kept warm in an inert atmosphere at 500-600°C for 8-12 hours, with a heating rate of 5-15°C / min; and / or, the D50 particle size of the ternary sulfide electrolyte is 0.5-1μm. The above-mentioned limitation on the D50 particle size of the ternary sulfide electrolyte is to make the ternary sulfide electrolyte uniformly coated on the surface of the graphite negative electrode material with the inner coating layer, and improve the ionic conductivity of the surface-modified graphite negative electrode material.
[0048] In a typical embodiment of the present invention, a composite negative electrode material is provided, the composite negative electrode material comprising the above-mentioned surface-modified graphite negative electrode material and a sulfide electrolyte, wherein the mass ratio of the surface-modified graphite negative electrode material to the sulfide electrolyte is (50-100): (0-50). The composite negative electrode material prepared by mixing the surface-modified graphite negative electrode material with the sulfide electrolyte has a higher ionic conductivity, and by limiting the mass ratio of the two as above, the ionic conductivity can be improved without affecting the insertion of lithium ions into the graphite negative electrode and the release of lithium ions from the graphite negative electrode.
[0049] In another typical embodiment of the present invention, an all-solid-state lithium battery is provided, which comprises the above-mentioned surface-modified graphite negative electrode material or the above-mentioned composite negative electrode material. The above-mentioned all-solid-state lithium battery significantly improves the lithium ion transmission capacity while suppressing the side reaction between graphite and electrolyte, and has excellent rate performance and cycle performance.
[0050] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0051] Examples 1-5
[0052] The surface modified graphite negative electrode material of the present invention is prepared by the method of embodiments 1-5, comprising the following steps:
[0053] S1, graphite, lithium sulfide, phosphorus pentasulfide and LiI are mixed in a molar ratio of 3:1:1, ball milled at a speed of 400 r / min for 10 h, and kept in an argon atmosphere at 200 ° C for 10 h to obtain a graphite negative electrode material with a LiI-doped binary sulfide Li3PS4 electrolyte inner coating layer;
[0054] S2, lithium sulfide, phosphorus pentasulfide, and lithium chloride are added in a ball mill in a molar ratio of 5:1:2, and ball milling is performed to obtain a uniform powder, which is then kept at 550°C in an argon atmosphere for 10 hours at a heating rate of 10°C / min to obtain a argon-type electrolyte Li6PS5Cl, and the above-mentioned argon-type electrolyte is refined to a D50 particle size of 1 μm, and then mixed with the above-mentioned graphite negative electrode with an inner coating layer, and ball milling is performed by solid phase ball milling to obtain a surface-modified graphite negative electrode material having a ternary sulfide electrolyte outer coating layer formed on the surface of the inner coating layer.
[0055] The mass ratios of the graphite core, inner coating layer, and outer coating layer in Examples 1-5 are shown in Table 1.
[0056] Table 1
[0057]
[0058] Embodiment 6-9
[0059] The embodiments of the surface modified graphite negative electrode material of the present invention, the difference between embodiments 6-9 and embodiment 1 is that in S1, the molar ratio of lithium sulfide, phosphorus pentasulfide, and LiI is different. In embodiment 6, the molar ratio of lithium sulfide, phosphorus pentasulfide, and LiI is 4.5:1.5:1, in embodiment 7, the molar ratio of lithium sulfide, phosphorus pentasulfide, and LiI is 1.5:0.5:1, in embodiment 8, the molar ratio of lithium sulfide, phosphorus pentasulfide, and LiI is 1.5:0.5:2, and in embodiment 9, the molar ratio of lithium sulfide, phosphorus pentasulfide, and LiI is 7.5:2.5:1.
[0060] The ratio of the amounts of lithium sulfide, phosphorus pentasulfide, and LiI in the inner coating layer of Examples 6-9 is shown in Table 2.
[0061] Table 2
[0062]
[0063] Comparative Example 1
[0064] A surface-modified graphite negative electrode material is different from Example 1 in that only step S1 is used to coat the surface of natural graphite with a LiI-doped binary sulfide electrolyte inner coating layer, and the operation in step S2 is not performed, thereby obtaining a surface-modified graphite negative electrode material with an inner coating layer.
[0065] Application Examples 1-9 and Application Comparative Example 1
[0066] Application Examples 1-9 and Application Comparative Example 1 are composite negative electrode materials. The surface modified graphite negative electrode materials in Examples 1-9 and Comparative Example 1 are mixed with the ternary sulfide electrolyte Li6PS5Cl, respectively, and mechanically ground at 300 r / min for 30 minutes to obtain the composite negative electrode materials of Application Examples 1-9 and Application Comparative Example 1, wherein the mass ratio of the surface modified graphite negative electrode material to the ternary sulfide electrolyte is 6:4.
[0067] Application Comparative Example 2
[0068] Application Comparative Example 2 is a composite negative electrode material, and its preparation method is: natural graphite and ternary sulfide electrolyte Li6PS5Cl are mixed and ground to obtain the composite negative electrode material.
[0069] The application examples and comparative examples were prepared into half-cells, and the preparation method was as follows: 100 mg of Li6PS5Cl electrolyte was weighed into PEEK with a diameter of 10 mm, pressurized for 1 t and maintained for 1 min, then 13 mg of the composite negative electrode material was weighed and placed on one side of the electrolyte, pressurized for 3.6 t and maintained for 3 min, and then an indium foil with a diameter of 10 mm and a thickness of 100 μm and a lithium foil with a diameter of 9 mm and a thickness of 50 μm were sequentially placed on the other side of the electrolyte as lithium indium negative electrodes, and finally the entire battery cell was pressurized for 2 t and maintained for 3 min, and the electrochemical performance was tested after tightening the screws to apply a test pressure of 15 NM.
[0070] The test results of the first cycle of 0.05C are shown in Table 3, and the test results of rate performance and cycle performance are shown in Table 4. Among them, the rate performance test step tested the performance of 0.05C / 0.05C for one cycle, 0.1C / 0.1C for three cycles, 0.2C / 0.2C for three cycles, 0.5C / 0.5C for three cycles, and 1C / 1C for three cycles.
[0071] Table 3
[0072]
[0073] It can be seen from Table 3 that the 0.05C lithium deintercalation capacity of the all-solid-state battery prepared in Example 1 is similar to that of the all-solid-state battery prepared in Comparative Example 1, and the first efficiency is significantly higher, while the 0.05C lithium deintercalation capacity of the all-solid-state battery prepared in Comparative Example 2 is significantly attenuated, and the first efficiency is also lower; the above test results show that after double-layer coating, the composite negative electrode material exhibits better electrochemical properties.
[0074] Figure 1 This is a first cycle 0.05C charge and discharge curve diagram of an all-solid-state battery assembled using the composite negative electrode materials of Example 1 and Comparative Examples 1-2, which is the same as the above results.
[0075] Figure 2 and Figure 3The dQ / dV curves of the first cycle 0.05C of the all-solid-state batteries assembled with the composite negative electrode materials of Application Comparative Example 1 and Application Example 1 respectively show that there are three groups of obvious redox peaks, corresponding to the fourth-order intercalation reaction: oxidation / reduction potential: -0.39 / -0.41V (vs.Li-In), the second and third-order intercalation reactions: oxidation / reduction potential: -0.45 / -0.49V (vs.Li-In) and the first-order intercalation reaction: oxidation / reduction potential: -0.51 / -0.54V (vs.Li-In). The peak positions in the dQ / dV curves of the three are the same, but the intensities of the three pairs of redox peaks are different, and there is the following intensity relationship: Application Example 1 > Application Comparative Example 1. When the peak positions are the same, the greater the intensity of the curve, the larger the corresponding peak area, that is, the higher the capacity in the corresponding charge and discharge curve, which is the same as the above results.
[0076] Table 4
[0077]
[0078]
[0079] It can be seen from Table 4 that the composite negative electrode materials described in Application Examples 1 to 9 all have good rate performance and cycle performance. The rate performance of Application Comparative Example 1 is poor, and the rate performance and cycle performance of Application Comparative Example 2 are both poor.
[0080] By comparing the test results of Application Examples 1-5 in Table 4, it can be found that when the mass ratio of the graphite core, the inner coating layer and the outer coating layer is (90-99): (0.5-5): (0.5-5), the electrochemical performance is better; when the ratio of the three does not meet the above limitations, it will either affect the rate at which lithium ions enter the graphite core, or increase the contact internal resistance between the negative electrode material and the electrode material, resulting in a certain degree of attenuation of the electrochemical performance.
[0081] By comparing the test results of Application Examples 6-9 and Application Example 1 in Table 4, it can be found that with the change of the composition of the inner coating layer, the half-cell performance changes significantly. When the molar ratio of LiX and binary sulfide electrolyte is 1: (1-3), its rate performance and cycle performance are optimal.
[0082] Figure 4 This is a test diagram of the cycle performance of an all-solid-state battery assembled with the composite negative electrode materials of Application Example 1 and Application Comparative Example 1-2. It can be seen from the figure that the cycle performance of Application Example 1 and Application Comparative Example 1 is significantly better than that of Application Comparative Example 2. This result shows that by coating the graphite, its stability is improved; in addition, by comparing the test results of Application Example 1 and Application Comparative Example 1, it can be found that the transmission rate of lithium ions is effectively improved through double-layer coating.
[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A surface modified graphite negative electrode material, It is characterized in that The surface modified graphite negative electrode material comprises a graphite core, an inner coating layer and an outer coating layer, wherein the inner coating layer is located on the surface of the graphite core, and the outer coating layer is located on the surface of the inner coating layer; the material of the inner coating layer is a binary sulfide electrolyte doped with LiX, and the material of the outer coating layer is a ternary sulfide electrolyte; X is a halogen element; the mass ratio of the graphite core, the inner coating layer and the outer coating layer is (90-99): (0.5-5): (0.5-5); in the material of the inner coating layer, the mass ratio of the LiX to the binary sulfide electrolyte is 1: (1-3).
2. The surface-modified graphite negative electrode material according to claim 1, It is characterized in that The mass ratio of the graphite core, the inner coating layer and the outer coating layer is (95-97): (1-4): (1-4).
3. The surface-modified graphite negative electrode material according to claim 1 or 2, It is characterized in that X is one of Cl, Br, and I; and / or The binary sulfide electrolyte is Li 3 PS 4 , Li 7 P 3 S 11 , Li 4 S N 4 At least one of; and / or The ternary sulfide electrolyte is a argyrodite-type electrolyte, and the argyrodite-type electrolyte is Li 6 PS 5 Cl, Li 6 PS 5 Br, Li 6 PS 5 I. Li 10 G 2 S 12 At least one of .
4. The surface modified graphite negative electrode material according to claim 3, It is characterized in that The X is I, and the binary sulfide electrolyte is Li 3 PS 4 The ternary sulfide electrolyte is Li 6 PS 5 Cl.
5. A method for preparing a surface-modified graphite negative electrode material according to any one of claims 1 to 4, It is characterized in that The steps include: S1, coating a LiX-doped binary sulfide electrolyte on the graphite surface to obtain a graphite negative electrode material with an inner coating layer; S2, coating the surface of the graphite negative electrode material having the inner coating layer with a ternary sulfide electrolyte to obtain the surface modified graphite negative electrode material.
6. The method for preparing the surface modified graphite negative electrode material according to claim 5, It is characterized in that In S1 and S2, the coating methods are each independently at least one of solid phase ball milling, magnetron sputtering, liquid phase coating, and atomic layer deposition.
7. The method for preparing the surface modified graphite negative electrode material according to claim 6, It is characterized in that In S1, the coating method is a solid phase ball milling method, and the solid phase ball milling method is specifically: mixing graphite, lithium sulfide, phosphorus pentasulfide, and LiX, ball milling, and keeping warm in an inert atmosphere at 180-250° C. for 8-12 hours to obtain the graphite negative electrode material with an inner coating layer; and / or In S2, the coating method is a solid phase ball milling method, and the solid phase ball milling method is specifically: mixing the ternary sulfide electrolyte with the graphite negative electrode material having an inner coating layer, and obtaining the surface modified graphite negative electrode material by ball milling; and / or In S2, The preparation method of the ternary sulfide electrolyte is: lithium sulfide, phosphorus pentasulfide and lithium chloride are mixed in proportion, and kept warm in an inert atmosphere at 500-600° C. for 8-12 hours; and / or The D50 particle size of the ternary sulfide electrolyte is 0.5-1 μm.
8. A composite negative electrode material, It is characterized in that The composite negative electrode material comprises a surface-modified graphite negative electrode material and a sulfide electrolyte, wherein the mass ratio of the surface-modified graphite negative electrode material to the sulfide electrolyte is (50-100): (0-50); the surface-modified graphite negative electrode material is the surface-modified graphite negative electrode material described in any one of claims 1 to 4 or the surface-modified graphite negative electrode material prepared by the preparation method described in any one of claims 5 to 7.
9. An all-solid-state lithium battery, It is characterized in that The invention comprises the surface modified graphite negative electrode material according to any one of claims 1 to 4 or the composite negative electrode material according to claim 8.
Citation Information
Patent Citations
Argyrodite type sulfide solid electrolyte containing lithium halide coating layer and preparation of argyrodite type sulfide solid electrolyte
CN114267874A
Negative electrode material and battery
CN115398666A
Coated positive electrode active material, positive electrode material, and battery
CN117337497A
Electrode material, method for producing electrode material, and method for producing all-solid battery
CN117374236A
Electrode material, electrode and all-solid-state battery
CN117476863A