A kind of microsphere with high flame retardant property and its preparation method and application

By preparing high flame retardant properties microspheres, the problem of poor flame retardant effect and compatibility in polymers is solved, and more efficient flame retardant effect and toxic gas barrier are achieved, and fire hazards and material density are reduced.

CN118440404BActive Publication Date: 2024-11-05CHINA CONSTR EIGHTH ENG GRP (SHANDONG) NEW MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410568401.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-11-05
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

Existing expandable graphite has limited flame retardant effects in polymers, is prone to settlement and agglomeration, and cannot effectively block toxic gases, resulting in serious fire hazards.

Method used

By preparing high flame retardant microspheres, using materials such as urea phosphate, urea, expandable graphite, etc., a composite microsphere containing ammonium polyphosphate and modified silane chains is formed through multiple reactions, thereby improving the adhesion and phase of expandable graphite. Capacitance and introduction of amino groups and double bonds to enhance their binding force with polyurethane matrix and toxic gas adsorption capacity.

Benefits of technology

The flame retardant effect of expandable graphite and compatibility with the substrate are improved, and a dense flame retardant carbon layer is formed to effectively block toxic gases, reduce fire hazards, and reduce the amount of use, avoiding the problem of shedding caused by excessive material density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004830102890000091
    Figure BDA0004830102890000091
  • Figure BDA0004830102890000092
    Figure BDA0004830102890000092
  • Figure BDA0004830102890000121
    Figure BDA0004830102890000121
Patent Text Reader

Abstract

The present application discloses a kind of high flame retardant microsphere and its preparation method and application, belonging to the technical field of flame retardant microsphere. The preparation method of the high flame retardant microsphere includes the following steps: (1) phosphoric acid and urea are mixed and reacted, and then expandable graphite is added for emulsification, polymerization, and crushing to obtain intermediate microsphere A; (2) intermediate microsphere A and N-aminoethyl-3-aminopropyltriethoxysilane are reacted to obtain intermediate microsphere B; (3) monomer A, formaldehyde compound and intermediate microsphere B are reacted to obtain intermediate microsphere C, monomer A is selected from at least one of p-acetoxystyrene, diacetone acrylamide, and benzylidene acetone; (4) intermediate microsphere C is placed in 3-mercaptopropyltriethoxysilane solution and reacted to obtain high flame retardant microsphere. The microsphere can improve the flame retardant effect of expandable graphite and the compatibility of expandable graphite with polyurethane matrix, and can also absorb and block the toxic gas generated when the matrix burns, reducing the combustion hazard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a highly flame-retardant microsphere and a preparation method and application thereof, belonging to the technical field of flame-retardant microspheres. Background Art

[0002] With the extensive use of various polymers, especially as building and decoration materials, the danger and harm of fire have greatly increased. The casualties and property losses caused by fire are increasing every year. The flammability of polymers has become one of the main obstacles to expanding their application areas. Therefore, the development of flame-retardant polymers and polymer flame-retardant additives has become a top priority in polymer material science research.

[0003] Due to the closed-cell structure inside the rigid polyurethane material and the fact that it is a high molecular weight polymer with a very low thermal conductivity, polyurethane materials are generally also used as exterior wall insulation materials for buildings. However, the polyurethane matrix itself is flammable, so it is easy to cause polyurethane fire accidents. In order to improve the flame retardancy of polyurethane insulation materials and comply with the requirements of the times for environmental protection, halogen-free flame retardants are usually added to the polyurethane matrix to obtain polyurethane composite materials with flame retardant properties.

[0004] At present, the most common halogen-free flame retardant in polyurethane is expandable graphite. When encountering a high temperature environment, expandable graphite can expand rapidly to hundreds of times its own volume, covering the surface of the burning material to form a dense insulating protective carbon layer. At the same time, expandable graphite has a small heat release per unit time and a small mass loss, and the expansion product has excellent oxidation resistance and high temperature resistance. It can effectively resist the invasion of flames in a fire, block the further contact of matter and heat between the flame and the polymer material, slow down the continued combustion of the polymer, and make the peak time of heat release in the thermal degradation process of the polymer as late as possible or make the heat release as smooth and even as possible, ultimately achieving the purpose of flame retardancy.

[0005] However, since expandable graphite mainly relies on its own volume expansion property to be flame retardant, its chemical bonding with the material matrix during the expansion process is weak, and the interaction between the expanded graphites after expansion is also weak. Therefore, after specific combustion, the flame retardant carbon layer produced by the expanded graphite has poor mechanical properties and is easily formed into fly ash when subjected to open flame impact or heat convection, resulting in cracks in the flame retardant carbon layer, which cannot be effectively flame retardant, and the unburned substrate continues to burn, thus limiting the application of expandable graphite in polymer flame retardancy.

[0006] In order to solve this problem, the patent CN201410503405.7 inserts a phosphorus-containing compound (ammonium polyphosphate) between graphite layers, so that the expandable graphite obtained has a higher expansion volume, while improving the adhesion between the expanded graphite, thereby obtaining a better flame retardant effect. Although this method can improve the flame retardant effect of expandable graphite in the substrate to a certain extent, new problems will be introduced. The modified expandable graphite has poor compatibility with the polymer matrix, and it is difficult to form a uniform and stable state with the matrix. The expandable graphite will settle and agglomerate, thereby affecting the performance of the product. And the expandable graphite prepared by the method is still weak in bonding with the matrix, so that stratification is easily produced between the flame retardant carbon layer and the matrix, reducing the protection of the matrix.

[0007] In addition, some polymer matrices will produce a large amount of toxic gases during combustion, such as HCN, HS, CO, CO2, etc. Therefore, even if the expandable graphite can achieve flame retardancy in the early stage of polymer combustion, it cannot block and absorb the toxic gases. The presence of the above gases will also cause serious harm to the human body and the environment. Summary of the invention

[0008] In order to solve the above problems, a high flame retardant microsphere and a preparation method and application thereof are provided. The high flame retardant microsphere prepared by the preparation method can not only improve the adhesion between expanded graphite in the flame retardant carbon layer, thereby improving the flame retardant effect of the expandable graphite; it can also improve the compatibility of the expandable graphite with the polyurethane matrix, so that the expandable graphite can be evenly dispersed in the matrix without sedimentation and agglomeration, thereby improving the protection of the flame retardant carbon layer to the matrix; and the microsphere can also absorb and block the toxic gas generated when the matrix burns, further reducing the combustion hazard.

[0009] According to one aspect of the present application, a method for preparing microspheres with high flame retardancy is provided, comprising the following steps:

[0010] (1) Phosphoric acid and urea in a molar ratio of (0.5-1):1 are mixed, reacted at 80-100° C. to obtain urea phosphate, expandable graphite, a dispersant, and an emulsifier are added to the urea phosphate, and stirred at 80-100° C. to obtain a colloid, the colloid is emulsified in an emulsifier, and then transferred to a polymerization furnace to polymerize at 150-240° C. and 10-45 KPa to obtain a composite material, and the composite material is cooled, dried, and crushed to obtain intermediate microspheres A;

[0011] (2) mixing the intermediate microsphere A and N-aminoethyl-3-aminopropyltriethoxysilane in a solvent and heating to 80° C. to react, and then filtering, washing, and drying to obtain the intermediate microsphere B with amino groups;

[0012] (3) reacting monomer A, formaldehyde compound and intermediate microsphere B under an acidic catalyst, filtering, washing and drying to obtain intermediate microsphere C, wherein monomer A is selected from at least one of p-acetoxystyrene, diacetone acrylamide and benzylidene acetone;

[0013] (4) The intermediate microspheres C are placed in a 3-mercaptopropyltriethoxysilane solution, reacted under the initiator, and then filtered, washed, and dried to obtain microspheres with high flame retardancy.

[0014] In the preparation method, the intermediate microspheres A obtained in step (1) contain ammonium polyphosphate between the graphite layers, which can improve the adhesion between the expandable graphite, thereby improving the flame retardant effect of the expandable graphite. In step (2), N-aminoethyl-3-aminopropyltriethoxysilane is used to react with the intermediate microspheres A to obtain the intermediate microspheres B. Firstly, the compatibility of the intermediate microspheres B with the polyurethane substrate can be improved, so that the expandable graphite and the matrix form a uniform and stable state, and the sedimentation and agglomeration of the expandable graphite are avoided, thereby improving the performance uniformity of the polymer matrix and the flame retardant uniformity of the expandable graphite to the matrix. Secondly, the intermediate microspheres B contain NH and NH2 groups, which can not only absorb toxic gases to reduce the combustion hazard, but also participate in the reaction of isocyanate to form polyurethane, form a chemical bond with the polyurethane matrix, and improve the bonding force between the expandable graphite and the matrix, so that the flame retardant carbon layer is tightly combined with the matrix, and the protection of the matrix is ​​improved. In step (3), the intermediate microspheres C can also be obtained by reacting with the monomer A formaldehyde compound. The intermediate microspheres C prepared in step (3) can introduce functional groups such as benzene rings, carbonyl groups, ester groups, and amino groups into expandable graphite due to the presence of monomer A. The benzene rings can strengthen the matrix and improve the mechanical properties of the matrix. The carbonyl groups and ester groups can further increase the compatibility with the polyurethane matrix. The amino groups can further increase the number of binding sites with the polyurethane matrix and increase the adsorption of toxic gases. Since the monomers A in step (3) all contain double bonds, 3-mercaptopropyltriethoxysilane is used in step (4) to react with the double bonds to obtain silane-terminated high flame retardant microspheres, which can further improve the dispersibility and stability of expandable graphite in the matrix, and improve the adhesion between expandable graphites, so that the strength and density of the flame retardant carbon layer are improved, thereby adsorbing and effectively blocking toxic gases and reducing the harm of toxic gases to the human body.

[0015] The intermediate microspheres A obtained in the above step (1) allow ammonium polyphosphate to be contained between graphite layers, which not only improves the bonding force between expandable graphites and increases the strength of the flame-retardant carbon layer, but also can simultaneously improve the flame-retardant properties of expandable graphite because the ammonium polyphosphate itself is also flame-retardant. In steps (2) to (4), the surface of the expandable graphite contains modified molecular chains, which can firstly achieve the adsorption of toxic gases; secondly, improve the compatibility of the expandable graphite with the matrix, improve the dispersion uniformity of the expandable graphite, avoid the sedimentation or agglomeration of the expandable graphite, and also improve the performance uniformity of the polyurethane composite material; thirdly, it can be chemically combined with the polyurethane matrix, so that the flame-retardant carbon layer is tightly combined with the matrix, effectively blocking the toxic gas, and can also improve the density, uniformity and mechanical strength of the flame-retardant carbon layer, and can resist the impact of open flames or heat convection.

[0016] The highly flame-retardant microspheres prepared by the above method can effectively reduce the usage amount when used as flame retardants due to their more uniform dispersion, thereby reducing the density of the material and avoiding the problem of falling off due to excessive mass when used as building exterior walls.

[0017] Optionally, in step (1), the expandable graphite accounts for 5-30% of the weight of the urea phosphate, the dispersant accounts for 0.5% of the weight of the urea phosphate, and the emulsifier accounts for 0.5% of the weight of the urea phosphate.

[0018] In the above step (1), the intermediate microspheres A are obtained by adopting a homogenizing emulsification process, which can solve the problem of difficult dispersion of expandable graphite and ammonium polyphosphate emulsion. Under the high shear force of the homogenizing emulsifier, a large number of small droplets are formed inside the emulsion, so that the microstructure of the expandable graphite particles wrapped by the ammonium polyphosphate emulsion is realized. During the polymerization process, the expandable graphite particles can be evenly dispersed, thereby improving the modification effect of ammonium polyphosphate on the expandable graphite.

[0019] Since the expandable graphite contains ammonium polyphosphate between the layers, the ammonium polyphosphate decomposes into ammonia and polyphosphoric acid when heated. The ammonia can dilute the oxygen concentration, and the polyphosphoric acid has good thermal stability. The expandable graphite expands rapidly after heating, which can effectively isolate the oxygen required for combustion. At the same time, the interior has a porous property, which absorbs the combustion smoke and reduces the possibility of re-combustion. It can also effectively isolate the combustion oxygen and improve the flame retardant properties of the material.

[0020] Optionally, in step (2), the weight ratio of the intermediate microsphere A to N-aminoethyl-3-aminopropyltriethoxysilane is 1:(1-2);

[0021] The heating reaction time in step (2) is 8-10 hours.

[0022] The surface of expandable graphite contains a large number of hydroxyl groups. Through the reaction of N-aminoethyl-3-aminopropyltriethoxysilane and intermediate microspheres A, N-aminoethyl-3-aminopropyltriethoxysilane can react with the hydroxyl groups to achieve the grafting of N-aminoethyl-3-aminopropyltriethoxysilane on the surface of expandable graphite. The above reaction conditions can increase the reaction rate of N-aminoethyl-3-aminopropyltriethoxysilane and intermediate microspheres A, and increase the amount of N-aminoethyl-3-aminopropyltriethoxysilane on the surface of expandable graphite, thereby synergistically improving the flame retardancy, reinforcement, adsorption of toxic gases and density improvement of the microspheres with high flame retardancy on the substrate.

[0023] If the weight of N-aminoethyl-3-aminopropyltriethoxysilane is too much, the amount of N-aminoethyl-3-aminopropyltriethoxysilane on the surface of expandable graphite increases. Combined with the reactions of the subsequent steps (3) and (4), too many molecular chains are introduced to the surface of expandable graphite, which weakens the bonding force between expandable graphites. The flame retardant carbon layer will still have cracks, and the flame retardant and toxic gas barrier effects will be reduced. If the weight of N-aminoethyl-3-aminopropyltriethoxysilane is too little, the modification effect of expandable graphite will be reduced, and the flame retardant, reinforcement, toxic gas adsorption and density improvement effects of the matrix will all be reduced.

[0024] Optionally, in step (3), the weight ratio of monomer A, formaldehyde compound and intermediate microsphere B is (1-2): (1-3): 1;

[0025] The reaction temperature of step (3) is 50-60°C and the reaction time is 8-12h;

[0026] Preferably, the acidic catalyst is selected from at least one of nicotinic acid, sulfuric acid, acetic acid and nitric acid.

[0027] The above-mentioned weight ratio and reaction conditions can improve the reaction efficiency of monomer A, formaldehyde compounds and intermediate microspheres B, and promote monomer A and formaldehyde compounds to react with the amino groups in N-aminoethyl-3-aminopropyltriethoxysilane, thereby introducing new functional groups, increasing the number of functional groups in the intermediate microspheres B, and further synergistically improving the flame retardant and reinforcing effects of expandable graphite on the matrix.

[0028] Optionally, the monomer A is selected from diacetone acrylamide and benzylidene acetone;

[0029] The formaldehyde compound is selected from trioxymethylene and / or polyformaldehyde.

[0030] Optionally, the molar ratio of diacetone acrylamide to benzyl acetone is 3:1.

[0031] It has been verified that when a single type of monomer A reacts with formaldehyde compounds and intermediate microspheres B, after monomer A is connected to intermediate microspheres B, it will hinder the subsequent reaction of monomer A, thereby reducing the reaction participation rate of monomer A, resulting in a part of the molecular chain on the surface of the intermediate microsphere C being terminated with monomer A, and the other part being terminated with N-aminoethyl-3-aminopropyltriethoxysilane. The selection of diacetone acrylamide and benzylidene acetone in a molar ratio of 3:1 as monomer A can increase the reaction participation rate of monomer A, so that the reaction rate of N-aminoethyl-3-aminopropyltriethoxysilane on the surface of intermediate microspheres B and monomer A is greater than 98%. In addition, two functional groups with amino groups and benzene rings can be simultaneously given to the intermediate microspheres C, thereby enhancing the mechanical strength of the matrix and the chemical bonding with the matrix, thereby achieving a close and uniform connection between the expandable graphite and the matrix.

[0032] Optionally, in step (4), the weight ratio of the intermediate microspheres C to 3-mercaptopropyltriethoxysilane is 1:(5-10);

[0033] Preferably, the initiator in step (4) is a free radical initiator, the reaction temperature is 60-70° C., and the reaction time is at least 5 hours.

[0034] Preferably, the free radical initiator is AIBN.

[0035] The surface of the intermediate microsphere C is capped with monomer A, so that the surface of the intermediate microsphere contains a large number of double bonds. In step (4), the double bonds react with the thiol group to reintroduce siloxane molecular chains into the flame-retardant microspheres. At this time, both ends of the molecular chains on the surface of the flame-retardant microspheres are siloxane molecular chains, which can improve the dispersibility and stability of the flame-retardant microspheres in the matrix. Under the premise of stable dispersion, the reaction uniformity of the amino groups in the molecular chains on the surface of the flame-retardant microspheres with isocyanate can be improved, and then the uniformity of chemical bonding with the matrix can be improved, and the expandable graphite can be uniformly embedded in the matrix. In a high temperature environment, the expandable graphite has a strong bonding force with the matrix, and the toxic matrix produced by the matrix is ​​adsorbed and blocked at the first time, thereby improving the safety of the polyurethane thermal insulation material.

[0036] Optionally, the particle size of the intermediate microsphere A is 0.5-10 μm. The above particle size is conducive to the subsequent modification of the intermediate microsphere A in steps (2)-(4), thereby obtaining microspheres with high flame retardancy and the best synergistic performance.

[0037] Optionally, the expansion coefficient of the expandable graphite is 250-290 ml / g.

[0038] According to another aspect of the present application, there is provided a highly flame retardant microsphere prepared by the method for preparing highly flame retardant microspheres described in any one of the above items.

[0039] According to another aspect of the present application, there is provided application of the above-mentioned highly flame retardant microspheres in flame retardant materials.

[0040] The beneficial effects of this application include but are not limited to:

[0041] 1. The method for preparing highly flame-retardant microspheres of the present application adopts steps (1)-(4) to modify the expandable graphite, which can improve the bonding force between the expandable graphite in the flame-retardant carbon layer, thereby improving the mechanical properties of the flame-retardant carbon layer, thereby effectively flame-retarding and protecting the substrate.

[0042] 2. The method for preparing highly flame-retardant microspheres of the present application, steps (2)-(4) introduce modified molecular chains into the surface of expandable graphite, both ends of the molecular chains are siloxane chains, which can improve the compatibility of expandable graphite with the polyurethane matrix, thereby avoiding the sedimentation and agglomeration of expandable graphite in the matrix, and improving the performance uniformity of the polyurethane composite material.

[0043] 3. In the method for preparing highly flame-retardant microspheres of the present application, the amino functional groups introduced in step (2) and step (3) can chemically react with isocyanate, thereby forming a chemical bond between the expandable graphite and the matrix, thereby increasing the protective strength of the flame-retardant carbon layer on the matrix. In addition, due to the porous structure of the expandable graphite and the presence of amino groups on its surface, toxic gases can be adsorbed, thereby reducing the combustion hazard of the polyurethane composite material.

[0044] 4. The method for preparing highly flame-retardant microspheres of the present application, after the expandable graphite is modified, the dispersion uniformity of the expandable graphite and the bonding property with the matrix are improved, and the amount of expandable graphite used is reduced while ensuring the flame retardant effect, thereby reducing the density of the material, and avoiding the problem of polyurethane composite materials falling off due to excessive mass when used as building exterior walls. And while reducing the material density, the thermal insulation and mechanical strength of the composite material can still be maintained. DETAILED DESCRIPTION

[0045] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0046] Unless otherwise specified, the raw materials in the examples and comparative examples of the present application were purchased through commercial channels.

[0047] Unless otherwise specified, the methods used in the embodiments of the present application are conventional methods in the prior art.

[0048] Example 1

[0049] This embodiment relates to a method for preparing microspheres with high flame retardancy, which comprises the following steps:

[0050] (1) Phosphoric acid and urea are mixed at a molar ratio of 0.5:1, and reacted at 100° C. to obtain urea phosphate, and expandable graphite, a dispersant, and an emulsifier are added to the urea phosphate, wherein the expandable graphite accounts for 5% of the weight of the urea phosphate, the dispersant accounts for 0.5% of the weight of the urea phosphate, and the emulsifier accounts for 0.5% of the weight of the urea phosphate, and the mixture is stirred at 100° C. to obtain a colloid, and the colloid is placed in an emulsifier for emulsification and then transferred to a polymerization furnace for polymerization at 240° C. and 10 KPa to obtain a composite material, and the composite material is cooled, dried, and crushed to obtain intermediate microspheres A, wherein the particle size of the intermediate microspheres A is 0.5 μm;

[0051] (2) Mixing intermediate microspheres A and N-aminoethyl-3-aminopropyltriethoxysilane in a weight ratio of 1:1 in N,N-dimethylformamide and heating to 80°C, reacting for 10 hours under nitrogen protection, filtering, washing, and drying to obtain intermediate microspheres B with amino groups;

[0052] (3) para-acetoxystyrene, trioxymethylene and the intermediate microsphere B in a weight ratio of 1:1:1 are mixed in methanol, 37% concentrated hydrochloric acid is slowly added dropwise, and the amount of concentrated hydrochloric acid added is 30% of the weight of the intermediate microsphere B. Then, the reaction is carried out at 50° C. under nitrogen protection for 12 hours, and the reaction solution is neutralized to neutrality with sodium bicarbonate, filtered, washed, and dried to obtain the intermediate microsphere C;

[0053] (4) The intermediate microspheres C with a weight ratio of 1:5 are placed in a solution of 3-mercaptopropyltriethoxysilane, wherein the solvent is a mixed solvent of ethanol and water with a volume ratio of 5:1, and then AIBN accounting for 1% of the weight of the intermediate microspheres is added. After reacting at 70° C. under nitrogen protection for 5 hours, the microspheres with high flame retardancy are obtained by filtration, washing, and drying.

[0054] Example 2

[0055] This embodiment relates to a method for preparing microspheres with high flame retardancy, which comprises the following steps:

[0056] (1) Phosphoric acid and urea are mixed at a molar ratio of 1:1, and reacted at 80° C. to obtain urea phosphate, and expandable graphite, a dispersant, and an emulsifier are added to the urea phosphate, wherein the expandable graphite accounts for 30% of the weight of the urea phosphate, the dispersant accounts for 0.5% of the weight of the urea phosphate, and the emulsifier accounts for 0.5% of the weight of the urea phosphate, and the mixture is stirred at 80° C. to obtain a colloid, and the colloid is placed in an emulsifier for emulsification and then transferred to a polymerization furnace for polymerization at 150° C. and 45 KPa to obtain a composite material, and the composite material is cooled, dried, and crushed to obtain intermediate microspheres A, wherein the particle size of the intermediate microspheres A is 10 μm;

[0057] (2) The intermediate microspheres A and N-aminoethyl-3-aminopropyltriethoxysilane in a weight ratio of 1:2 were mixed in N,N-dimethylformamide and heated to 80°C. The mixture was reacted for 8 hours under nitrogen protection. The intermediate microspheres B with amino groups were obtained by suction filtration, washing and drying. The reaction equation is as follows:

[0058]

[0059] (3) Mixing monomer A, trioxymethylene and the intermediate microsphere B in a weight ratio of 2:3:1 in methanol, slowly adding 37% concentrated hydrochloric acid, the amount of concentrated hydrochloric acid added is 30% of the weight of the intermediate microsphere B, and then reacting for 8 hours at 60° C. under nitrogen protection, neutralizing the reaction solution with sodium bicarbonate to neutrality, filtering, washing and drying to obtain intermediate microspheres C, wherein the monomer A is selected from diacetone acrylamide and benzylidene acetone in a molar ratio of 3:1, and the reaction equation is as follows:

[0060]

[0061] Wherein R represents monomer A, and both amino groups in the intermediate microsphere B in this step can participate in the reaction, thereby obtaining two compounds of the structure of Formula 1 and the structure of Formula 2, and the compound of the structure of Formula 1 accounts for more than 70% in the above reaction;

[0062] (4) placing the intermediate microspheres C at a weight ratio of 1:10 in a solution of 3-mercaptopropyltriethoxysilane, wherein the solvent is a mixed solvent of ethanol and water at a volume ratio of 5:1, and then adding AIBN accounting for 1% of the weight of the intermediate microspheres. After reacting at 60°C under nitrogen protection for 8 hours, the microspheres are filtered, washed, and dried to obtain microspheres with high flame retardancy. In this step, the carbon-carbon double bond in the monomer A undergoes an addition reaction with 3-mercaptopropyltriethoxysilane.

[0063] Example 3

[0064] The difference between this embodiment and embodiment 2 is that in step (1), the expandable graphite accounts for 40% of the weight of urea phosphate, and the remaining steps are the same as those in embodiment 2.

[0065] Example 4

[0066] The difference between this embodiment and embodiment 2 is that in step (2), the weight ratio of the intermediate microsphere A to N-aminoethyl-3-aminopropyltriethoxysilane is 1:0.5, and the remaining steps are the same as those in embodiment 2.

[0067] Example 5

[0068] The difference between this embodiment and embodiment 2 is that in step (3), the weight ratio of monomer A, formaldehyde compound and intermediate microsphere B is 0.8:3:1, and the remaining steps are the same as those in embodiment 2.

[0069] Example 6

[0070] The difference between this embodiment and embodiment 2 is that in step (3), monomer A is selected from diacetone acrylamide and benzyl acetone in a molar ratio of 1:3, and the remaining steps are the same as those in embodiment 2.

[0071] Example 7

[0072] The difference between this embodiment and embodiment 2 is that in step (4), the weight ratio of the intermediate microspheres C to 3-mercaptopropyltriethoxysilane is 1:3, and the remaining steps are the same as those in embodiment 2.

[0073] Example 8

[0074] The difference between this embodiment and embodiment 2 is that the particle size of the intermediate microsphere A is 15 μm, and the remaining steps are the same as those in embodiment 2.

[0075] Comparative Example 1

[0076] The difference between this comparative example and Example 2 is that step (1) is not performed, and in step (2), expandable graphite and N-aminoethyl-3-aminopropyltriethoxysilane in a weight ratio of 1:2 are directly reacted, the particle size of the expandable graphite is 10 μm, and the remaining steps are the same as in Example 2.

[0077] Comparative Example 2

[0078] The difference between this comparative example and Example 2 is that steps (2) to (4) are not performed, the intermediate microsphere A is the final microsphere with high flame retardancy, and the remaining steps are the same as those in Example 2.

[0079] Comparative Example 3

[0080] The difference between this comparative example and Example 2 is that step (4) is not performed, the intermediate microspheres C are the final microspheres with high flame retardancy, and the remaining steps are the same as those in Example 2.

[0081] Comparative Example 4

[0082] The difference between this comparative example and Example 2 is that 3-aminopropyltriethoxysilane is used in step (2) instead of N-aminoethyl-3-aminopropyltriethoxysilane, and the remaining steps are the same as Example 2.

[0083] Test Example 1

[0084] The highly flame retardant microspheres prepared by the above-mentioned embodiments and comparative examples were subjected to gas adsorption tests. The test results are shown in Table 1. The test method is as follows:

[0085] Experimental group: 1g of highly flame-retardant microspheres were placed in the non-combustible plate of the reactor, and a polyurethane sheet (5cm long * 5cm wide * 1cm thick) without flame retardant was fixed and hung in the reactor. Oxygen (100ml / min) was introduced into the reactor, and the polyurethane sheet was ignited and burned with an ignition device until it was completely burned. The concentrations of HCN, CO2, CO, NO, and NO2 in the reactor were tested.

[0086] Blank group: A polyurethane sheet of the same material and size was fixed and hung in the reactor. Nothing was placed in the non-combustible sheet. After the combustion was completed, the concentrations of HCN, CO2, CO, NO, and NO2 in the reactor were recorded.

[0087] The polyurethane sheets of the experimental group and the blank group were prepared by placing polyether polyol, foam leveler, catalyst, blowing agent and water in a weight ratio of 75:2.7:1.5:1.5:1 in a container, mixing and stirring with a high-speed stirrer for 2 minutes to obtain a uniform mixed liquid, then adding PAPI and stirring at a high speed for 20 seconds to obtain a mixture. The weight ratio of PAPI to water was 100:1. The mixture was quickly added to the mold for foaming, and the closed mold temperature was controlled at 65°C for 30 minutes for aging. After the foaming was completed, the mold was opened and cut into 5 cm long * 5 cm wide * 1 cm thick pieces.

[0088] The highly flame-retardant microspheres prepared in the examples and comparative examples were subjected to experimental group tests in turn, and the adsorption rates of various gases were calculated based on the comparison of the tested gas concentrations with the blank group. The calculation method is as follows:

[0089] HCN adsorption rate = (HCN concentration in blank group - HCN concentration in experimental group) / HCN concentration in blank group * 100;

[0090] CO2 adsorption rate = (CO2 concentration of blank group - CO2 concentration of experimental group) / CO2 concentration of blank group * 100;

[0091] CO adsorption rate = (CO concentration of blank group - CO concentration of experimental group) / CO concentration of blank group * 100;

[0092] NO adsorption rate = (NO concentration in blank group - NO concentration in experimental group) / NO concentration in blank group * 100;

[0093] NO2 adsorption rate = (NO2 concentration in blank group - NO2 concentration in experimental group) / NO2 concentration in blank group * 100.

[0094] Table 1

[0095]

[0096] According to the data in Table 1, the highly flame-retardant microspheres prepared in the present application can adsorb HCN, CO2, CO, NO, and NO2. Therefore, when they are used in polyurethane sheets, they can adsorb and block the toxic gases produced in the early stages of combustion, thereby reducing combustion hazards.

[0097] Test Example 2

[0098] The highly flame retardant microspheres prepared in the above embodiments and comparative examples were added to polyurethane to prepare a flame retardant polyurethane sheet, and the density, thermal conductivity, flame retardancy and mechanical properties of the polyurethane sheet were tested. The results are shown in Table 2 below. The preparation method of the polyurethane sheet is:

[0099] Polyether polyol, foam leveler, catalyst, blowing agent, water and highly flame retardant microspheres in a weight ratio of 75:2.7:1.5:1.5:1:30 were placed in a container and mixed with a high-speed stirrer for 2 minutes to obtain a uniform mixed liquid. PAPI was then added and stirred at a high speed for 20 seconds to obtain a mixture. The weight ratio of PAPI to water was 100:1. The mixture was quickly added to a mold for foaming. The temperature of the closed mold was controlled at 65°C and the time was maintained for 30 minutes for maturation. After the foaming was completed, the mold was opened, and samples of different sizes were prepared according to the standard and performance tests were carried out.

[0100] Table 2

[0101]

[0102] According to the data in Table 2, the high flame retardant microspheres of the present application have good flame retardant properties in the polyurethane material and do not affect the thermal insulation and mechanical strength of the material of the present application. Due to the modification of the high flame retardant microspheres, the chemical connection between the expandable graphite and the matrix can be enhanced, and the thermal insulation and mechanical strength of the material can also be improved to a certain extent.

[0103] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing microspheres with high flame retardancy, characterized in that: The steps include: (1) Phosphoric acid and urea are mixed in a molar ratio of (0.5-1):1, reacted at 80-100°C to obtain urea phosphate, expandable graphite, dispersant and emulsifier are added to the urea phosphate, and stirred at 80-100°C to obtain a colloid, the colloid is emulsified in an emulsifier, and then transferred to a polymerization furnace to polymerize at 150-240°C and 10-45KPa to obtain a composite material, and the composite material is cooled, dried and crushed to obtain intermediate microspheres A, wherein the expandable graphite accounts for 5-30% by weight of the urea phosphate, the dispersant accounts for 0.5% by weight of the urea phosphate, and the emulsifier accounts for 0.5% by weight of the urea phosphate; (2) mixing the intermediate microsphere A and N-aminoethyl-3-aminopropyltriethoxysilane in a solvent and heating to 80° C. to react, filtering, washing, and drying to obtain intermediate microspheres B with amino groups, wherein the weight ratio of the intermediate microspheres A to N-aminoethyl-3-aminopropyltriethoxysilane is 1:(1-2); (3) reacting monomer A, formaldehyde compound and intermediate microsphere B under an acid catalyst, filtering, washing and drying to obtain intermediate microsphere C, wherein monomer A is selected from at least one of p-acetoxystyrene and diacetone acrylamide, and the weight ratio of monomer A, formaldehyde compound and intermediate microsphere B is (1-2): (1-3): 1; (4) The intermediate microspheres C are placed in a 3-mercaptopropyltriethoxysilane solution, wherein the weight ratio of the intermediate microspheres C to 3-mercaptopropyltriethoxysilane is 1:(5-10). After reacting with an initiator, the solution is filtered, washed, and dried to obtain microspheres with high flame retardancy.

2. The method for preparing microspheres with high flame retardancy according to claim 1, characterized in that: The heating reaction time in step (2) is 8-10 hours.

3. The method for preparing microspheres with high flame retardancy according to claim 1, characterized in that: The reaction temperature of step (3) is 50-60°C and the reaction time is 8-12h.

4. The method for preparing microspheres with high flame retardancy according to claim 1, characterized in that: The monomer A is selected from diacetone acrylamide; The formaldehyde compound is selected from trioxymethylene and / or polyformaldehyde.

5. The method for preparing microspheres with high flame retardancy according to claim 1, characterized in that: The particle size of the intermediate microsphere A is 0.5-10 μm.

6. Highly flame retardant microspheres prepared by the method for preparing highly flame retardant microspheres according to any one of claims 1 to 5.

7. Use of the highly flame retardant microspheres according to claim 6 in flame retardant materials.