A hardening coating liquid with high wear resistance and preparation method thereof

By using components such as polyfunctional polyurethane acrylate and modified nanoparticles, a hardened coating liquid with high hardness and wear resistance is solved, and the problem of poor wear resistance and anti-fouling effect of existing coatings is suitable for electronics Protection of the touch screen of the device.

CN118440590BActive Publication Date: 2024-11-29JIANGXI HAOZE OPTICAL FILM TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410729566.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-11-29
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

The coating formed by curing the existing hardened coating liquid has poor wear resistance and anti-fouling effect, which is difficult to meet the protection needs of touch screens of electronic devices.

Method used

The polyfunctional polyurethane acrylate, modified nanoparticles, polyester additive components, epoxy acrylate monomer, leveling agent and photoinitiator are used to form high hardness through copolymerization reaction and surface modification of nanoparticles. and hardening coating liquid with wear resistance.

Benefits of technology

It realizes the high hardness, wear resistance and anti-fouling properties of the coating, significantly improves the comprehensive performance of the coating, and is suitable for the protection of touch screens of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118440590B_ABST
    Figure CN118440590B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of hardening coating liquid, and discloses a hardening coating liquid with high wear resistance and a preparation method thereof. The hardening coating liquid is prepared by mixing multifunctional polyurethane acrylate as a main raw material, with modified nanoparticles and polyester additive components and other additives, wherein the polyester additive component has a block structure, and the structure contains a rigid adamantane heterocycle and a highly hydrophobic fluorine chain segment, which can make the cured coating have a higher hardness, and the cross-linked network can make the coating denser and show a higher hardness. In addition, the presence of the fluorine chain segment can make the coating surface extremely hydrophobic and have excellent antifouling performance. The addition of the modified nanoparticles can not only avoid the decrease in light transmittance caused by the agglomeration of nano cerium dioxide, but also utilize the high strength of nano cerium dioxide to enhance the wear resistance of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hardening coating liquids, and in particular to a hardening coating liquid with high wear resistance and a preparation method thereof. Background Art

[0002] In today's society where electronic devices are developing rapidly, electronic products such as smart phones and LED TVs are widely used, which has led to widespread attention in all walks of life related to them. As we all know, the screens of electronic devices such as smart phones generally need to be protected with a protective film to prevent scratches on the screen during use, which affects the use. Among the many protective films available, hardened films occupy an important position in the field of protective films with their excellent scratch resistance and high transparency. At present, hardened films usually use cellulose acetate, polycarbonate or polybutylene terephthalate as the base film, and a hardening coating liquid is coated on its surface, and then cured. Since a large number of smart phones currently use touch screens, fingerprints are easily left on the screen after friction between fingers and the screen, affecting the appearance. This requires that the coating formed by the curing of the hardened coating liquid needs to have good oil and stain resistance. In addition, in order to avoid scratches on the coating due to slight bumps, the coating also needs to have high hardness and wear resistance.

[0003] Invention patent publication number CN115850803B discloses an anti-fog and anti-glare hardened film, which is prepared by applying two layers of anti-glare coating on a support, using double coatings to ensure coating thickness, ensuring that the coating has high wear resistance and hardness, and using organic particles in the coating to enhance the light transmittance and UV resistance of the coating. However, the construction process of this double-layer structure is relatively complicated and is not conducive to actual production. In addition, the added zinc oxide nanoparticles are prone to agglomeration, which may cause the curing effect of the coating to deteriorate, resulting in a decrease in surface performance.

[0004] To this end, the present invention provides a hardening coating liquid, and the hardened coating after the hardening coating liquid is cured has good comprehensive properties such as wear resistance and anti-fouling, and can be directly used to make a protective film for the touch screen of an electronic device. Summary of the invention

[0005] The object of the present invention is to provide a hardening coating liquid with high wear resistance and a preparation method thereof, so as to solve the problem that the coating formed by curing the hardening liquid has poor wear resistance and antifouling effect.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A hardening coating liquid with high wear resistance, comprising the following components in parts by weight: 60-70 parts of multifunctional polyurethane acrylate, 0.5-1.5 parts of modified nanoparticles, 2-5 parts of polyester additive components, 5-15 parts of epoxy acrylate monomers, 0.5-1 parts of leveling agents, 1-2 parts of photoinitiators, and 30-40 parts of organic solvents;

[0008] The modified nanoparticles are nano-cerium dioxide with surfaces modified by organic modification;

[0009] The polyester additive component is prepared by olefin-modifying a copolymerization product of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and a perfluorocarboxylic acid compound.

[0010] Furthermore, the multifunctional polyurethane acrylate is tetrafunctional polyurethane acrylate or hexafunctional polyurethane acrylate; the epoxy acrylate monomer is any one of glycidyl methacrylate, allyl glycidyl ether or glycidyl acrylate; and the organic solvent is acetone or ethyl acetate.

[0011] Furthermore, the modified nanoparticles are prepared by the following method:

[0012] The nano-cerium dioxide is mixed with Tris-HCl buffer, and ultrasonically dispersed to form a uniform dispersion. Dopamine hydrochloride is then added to the dispersion. After the addition is completed, the pH of the dispersion is adjusted, and the dispersion is stirred at a stirring rate of 200-500r / min for 6-8h at room temperature. The solid material is collected by centrifugation, washed, and dried to obtain modified nanoparticles.

[0013] In the above technical solution, the surface of nano-cerium dioxide contains hydroxyl groups, which can interact with the catechol structure in the dopamine hydrochloride structure, so that an organic binding layer can be coated on the surface of the nano-cerium dioxide to achieve surface modification of the nano-cerium dioxide and obtain modified nanoparticles.

[0014] Furthermore, the pH is 8-9.

[0015] Furthermore, the polyester additive component is prepared by the following method:

[0016] Step 1: Prepare material A

[0017] 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and toluene are added to a reactor, nitrogen is introduced, and after the air in the reactor is exhausted, stirring is started until a homogeneous solution is formed, and then a perfluorocarboxylic acid compound is added to the reactor. After the addition is completed, the temperature is increased to 60-65°C, and stirred at this temperature for 2-4 hours, and then a phase transfer catalyst is added to the reactor, and the temperature is further increased to 70-75°C. After maintaining this temperature condition for 6-8 hours, the temperature is reduced and the material is discharged, and the obtained material is material A;

[0018] Step 2: Preparation of polyester additive components

[0019] Material A is mixed with tetrahydrofuran to form a uniform solution, and then placed in an ice bath. The acyl chloride compound is added to the solution. After the addition is completed, the ice bath is removed and the accelerator is continued to be added. After mechanical stirring for 3-6 hours at room temperature, the material is separated to obtain the polyester additive component.

[0020] In the above technical scheme, 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene contains two equivalent epoxy substituents in its structure, which undergo a ring-opening esterification reaction with two equivalent substituted carboxyl groups in the structure of a perfluorocarboxylic acid compound through the catalytic action of a phase transfer catalyst, and gradually polymerize to form a polyester-type intermediate product with a block structure, i.e., material A. Since new hydroxyl substituents are continuously generated during the ring-opening esterification process, these hydroxyl substituents can further undergo esterification condensation with acyl chloride compounds through the promotion of a promoter, thereby introducing a large number of unsaturated olefinic functional groups into the molecular chain of material A to obtain a polyester additive component.

[0021] Furthermore, in step 1, the perfluorocarboxylic acid compound is perfluorosebacic acid or perfluorooctanedioic acid.

[0022] Furthermore, in step 1, the phase transfer catalyst is any one of tetramethylammonium bromide, tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate or N,N-dimethylbenzylamine.

[0023] Furthermore, in step 2, the acyl chloride compound is methacryloyl chloride or acryloyl chloride.

[0024] Furthermore, in step 2, the promoter is triethylamine or pyridine.

[0025] A hardening coating liquid with high wear resistance comprises the following steps:

[0026] The first step is to weigh each raw material according to the weight and set aside;

[0027] Step 2: Mix the multifunctional polyurethane acrylate and the organic solvent, stir and mix them evenly at a stirring rate of 300-500 r / min, then add the polyester additive component, epoxy acrylate monomer, leveling agent and photoinitiator, and continue stirring for 30-60 minutes to form a precursor solution;

[0028] The third step is to add the modified nanoparticles into the precursor solution and disperse them evenly to obtain a hardening coating solution.

[0029] In the above technical scheme, due to the effect of the photoinitiator, when the hardening coating is exposed to ultraviolet light, the multifunctional polyurethane acrylate, polyester additive component and unsaturated olefin functional groups in the epoxy acrylate monomer structure in the hardening coating will undergo copolymerization to form a network structure in which molecular chains are interwoven with each other. In addition, since the modified nanoparticles are nano-cerium dioxide modified with dopamine, they can interact with the epoxy acrylate monomer during the subsequent heating and curing process, thereby promoting its stable and uniform dispersion in the hardening coating.

[0030] Beneficial effects of the present invention:

[0031] (1) The polyester additive component prepared by the present invention has a block structure, and contains a rigid adamantane heterocycle and a highly hydrophobic fluorine chain segment in the structure. After adding it as an additive to the hardening coating liquid, on the one hand, the presence of the rigid adamantane heterocycle can make the cured coating have a higher hardness, and at the same time, the cross-linked network can make the coating denser and show a higher hardness. In addition, the presence of the fluorine chain segment can make the coating surface extremely hydrophobic, showing a super hydrophobic effect, and thus has excellent anti-fouling performance.

[0032] (2) The present invention performs surface modification on nano-cerium dioxide with a high refractive index so that it can be evenly dispersed in the hardened coating. On the one hand, this can avoid the decrease in light transmittance caused by the agglomeration of nano-cerium dioxide. On the other hand, it can also utilize the high strength of nano-cerium dioxide to enhance the wear resistance of the coating.

[0033] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 This is the infrared analysis chart of material A and polyester added components in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] A hardening coating liquid with high wear resistance, comprising the following components in parts by weight: 60 parts of tetrafunctional polyurethane acrylate, 0.5 parts of modified nanoparticles, 2 parts of polyester additive component, 5 parts of glycidyl methacrylate, 0.5 parts of leveling agent BYK358N, 1 part of photoinitiator benzoin dimethyl ether, and 30 parts of organic solvent ethyl acetate;

[0039] The method for preparing the hardened coating liquid comprises the following steps:

[0040] The first step is to weigh each raw material according to the weight and set aside;

[0041] Step 2: Mix the multifunctional polyurethane acrylate and the organic solvent ethyl acetate, stir and mix them evenly at a stirring rate of 300 r / min, then add the polyester additive component, glycidyl methacrylate, leveling agent BYK358N and photoinitiator benzoin dimethyl ether, and continue stirring for 60 minutes to form a precursor solution;

[0042] The third step is to add the modified nanoparticles into the precursor solution and disperse them evenly to obtain a hardening coating solution.

[0043] The modified nanoparticles are prepared by the following method:

[0044] 1.5 g of nano-cerium dioxide was mixed with 200 mL of Tris-HCl buffer and dispersed by ultrasonic until a uniform dispersion was formed. Then 0.4 g of dopamine hydrochloride was added to the dispersion. After the addition, the pH of the dispersion was adjusted to 9. The mixture was stirred at room temperature at a stirring rate of 500 r / min for 8 h. The solid material was collected by centrifugation, washed, and dried to obtain modified nanoparticles.

[0045] The polyester additive component is prepared by the following method:

[0046] Step 1: Prepare material A

[0047] 0.3 g of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and toluene were added to a reactor, nitrogen was introduced, and after the air in the reactor was exhausted, stirring was started until a homogeneous solution was formed, and then 0.3 g of perfluorosebacic acid was added to the reactor. After the addition was completed, the temperature was raised to 65°C, and stirred at this temperature for 3 hours, and then 0.01 g of tetrabutylammonium hydrogen sulfate was added to the reactor, and the temperature was further raised to 70°C. After maintaining this temperature condition for 8 hours, the temperature was lowered and the material was discharged, and the obtained material was material A;

[0048] Figure 1 This is the infrared analysis chart of material A. After simple analysis, 3391cm-1 The absorption peak at 3062cm is the characteristic absorption peak of hydroxyl group. -1 The absorption peak at 1761 cm is the carbon-hydrogen bond stretching vibration peak on the benzene ring. -1 The absorption peak at 1306 cm is the stretching vibration peak of the carbon-oxygen double bond of the ester group produced by the ring-opening esterification reaction. -1 The absorption peak that appears at is the stretching vibration peak of the carbon-fluorine bond.

[0049] Step 2: Preparation of polyester additive components

[0050] 0.5 g of material A was stirred and mixed with tetrahydrofuran to form a uniform solution, which was then placed in an ice bath. 0.03 g of acryloyl chloride was added to the solution. After the addition was complete, the ice bath was removed and 0.01 g of pyridine was added. After mechanical stirring for 4 hours at room temperature, the material was separated to obtain the polyester additive component.

[0051] The infrared analysis of the polyester additive components is as follows Figure 1 As shown, compared with material A, it has a -1 The hydroxyl absorption peak area at 3032 cm -1 A new absorption peak appears at , which belongs to the carbon-hydrogen stretching vibration peak on the unsaturated carbon-carbon double bond.

[0052] Example 2

[0053] A hardening coating liquid with high wear resistance comprises the following components in parts by weight: 65 parts of tetrafunctional polyurethane acrylate, 1.2 parts of modified nanoparticles prepared in Example 1 of the present invention, 4.5 parts of polyester additive component prepared in Example 1 of the present invention, 8 parts of glycidyl methacrylate, 0.6 parts of leveling agent BYK358N, 1.5 parts of photoinitiator benzoin dimethyl ether, and 35 parts of organic solvent ethyl acetate;

[0054] The method for preparing the hardened coating liquid comprises the following steps:

[0055] The first step is to weigh each raw material according to the weight and set aside;

[0056] Step 2: Mix the multifunctional polyurethane acrylate and the organic solvent ethyl acetate, stir and mix them evenly at a stirring rate of 500 r / min, then add the polyester additive component prepared in Example 1 of the present invention, glycidyl methacrylate, leveling agent BYK358N and photoinitiator benzoin dimethyl ether, and continue stirring for 40 minutes to form a precursor solution;

[0057] Step 3: Add the modified nanoparticles prepared in Example 1 of the present invention into the precursor solution and disperse them evenly to obtain a hardening coating solution.

[0058] Example 3

[0059] A hardening coating liquid with high wear resistance comprises the following components in parts by weight: 70 parts of tetrafunctional polyurethane acrylate, 1.5 parts of modified nanoparticles prepared in Example 1 of the present invention, 5 parts of polyester additive component prepared in Example 1 of the present invention, 15 parts of glycidyl methacrylate, 1 part of leveling agent BYK358N, 2 parts of photoinitiator benzoin dimethyl ether, and 40 parts of organic solvent ethyl acetate;

[0060] The method for preparing the hardened coating liquid comprises the following steps:

[0061] The first step is to weigh each raw material according to the weight and set aside;

[0062] Step 2: Mix the multifunctional polyurethane acrylate and the organic solvent ethyl acetate, stir and mix them evenly at a stirring rate of 500 r / min, then add the polyester additive component prepared in Example 1 of the present invention, glycidyl methacrylate, leveling agent BYK358N and photoinitiator benzoin dimethyl ether, and continue stirring for 30 minutes to form a precursor solution;

[0063] Step 3: Add the modified nanoparticles prepared in Example 1 of the present invention into the precursor solution and disperse them evenly to obtain a hardening coating solution.

[0064] Comparative Example 1

[0065] A hardening coating liquid comprises the following components in parts by weight: 65 parts of tetrafunctional polyurethane acrylate, 1.2 parts of nano-cerium dioxide, 4.5 parts of the polyester additive component prepared in Example 1 of the present invention, 8 parts of glycidyl methacrylate, 0.6 parts of leveling agent BYK358N, 1.5 parts of photoinitiator benzoin dimethyl ether, and 35 parts of organic solvent ethyl acetate;

[0066] The method for preparing the hardened coating liquid comprises the following steps:

[0067] The first step is to weigh each raw material according to the weight and set aside;

[0068] Step 2: Mix the multifunctional polyurethane acrylate and the organic solvent ethyl acetate, stir and mix them evenly at a stirring rate of 500 r / min, then add the polyester additive component prepared in Example 1 of the present invention, glycidyl methacrylate, leveling agent BYK358N and photoinitiator benzoin dimethyl ether, and continue stirring for 40 minutes to form a precursor solution;

[0069] The third step is to add nano-cerium dioxide into the precursor solution and disperse it evenly to obtain a hardening coating solution.

[0070] Comparative Example 2

[0071] A hardening coating liquid, comprising the following components in parts by weight: 65 parts of tetrafunctional polyurethane acrylate, 4.5 parts of the polyester additive component prepared in Example 1 of the present invention, 8 parts of glycidyl methacrylate, 0.6 parts of leveling agent BYK358N, 1.5 parts of photoinitiator benzoin dimethyl ether, and 35 parts of organic solvent ethyl acetate;

[0072] The method for preparing the hardened coating liquid comprises the following steps:

[0073] The first step is to weigh each raw material according to the weight and set aside;

[0074] In the second step, the multifunctional polyurethane acrylate and the organic solvent ethyl acetate are mixed, and after being stirred and mixed uniformly at a stirring rate of 500 r / min, the polyester additive component prepared in Example 1 of the present invention, glycidyl methacrylate, leveling agent BYK358N and photoinitiator benzoin dimethyl ether are added, and stirring is continued for 40 minutes to obtain a hardened coating solution.

[0075] Comparative Example 3

[0076] A hardening coating liquid comprises the following components in parts by weight: 65 parts of tetrafunctional polyurethane acrylate, 1.2 parts of modified nanoparticles, 8 parts of glycidyl methacrylate, 0.6 parts of leveling agent BYK358N, 1.5 parts of photoinitiator benzoin dimethyl ether, and 35 parts of organic solvent ethyl acetate;

[0077] The method for preparing the hardened coating liquid comprises the following steps:

[0078] The first step is to weigh each raw material according to the weight and set aside;

[0079] Step 2: Mix the multifunctional polyurethane acrylate and the organic solvent ethyl acetate, stir and mix them evenly at a stirring rate of 500 r / min, then add glycidyl methacrylate, leveling agent BYK358N and photoinitiator benzoin dimethyl ether, and continue stirring for 40 minutes to form a precursor solution;

[0080] Step 3: Add the modified nanoparticles prepared in Example 1 of the present invention into the precursor solution and disperse them evenly to obtain a hardening coating solution.

[0081] Test Case

[0082] The hardening coating liquids prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were uniformly coated on the surface of a 200 μm thick PET transparent film, and the light intensity was set to 150 mW / cm 2 , irradiated with UV lamp with wavelength of 254nm, after 5min, transferred to 80℃ temperature environment for curing for 8h to form coating film, and the following performance tests were carried out:

[0083] The test method of light transmittance refers to ASTM D1003; the test method of pencil hardness refers to GB / T 6729; a water contact angle meter is used to test the water contact angle; an abrasion resistance tester is used with a load of 500g to test the abrasion resistance performance.

[0084] From the analysis and test results, it can be seen that the hardened coating prepared with modified nanoparticles and polyester additive components as additives has a high light transmittance, high hardness, strong wear resistance, and exhibits super hydrophobic properties after curing, and has a good anti-fouling effect.

[0085] Comparative Example 1 uses unmodified nano-cerium dioxide to replace the modified nanoparticles, which may cause slight agglomeration, resulting in a decrease in light transmittance and wear resistance.

[0086] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A hardening coating liquid with high wear resistance, characterized in that: The invention comprises the following components in parts by weight: 60-70 parts of multifunctional polyurethane acrylate, 0.5-1.5 parts of modified nanoparticles, 2-5 parts of polyester additive components, 5-15 parts of epoxy acrylate monomers, 0.5-1 parts of leveling agents, 1-2 parts of photoinitiators, and 30-40 parts of organic solvents; The modified nanoparticles are nano-cerium dioxide with surfaces modified by organic modification; The modified nanoparticles are prepared by the following method: The nano-cerium dioxide is mixed with Tris-HCl buffer, and ultrasonically dispersed to form a uniform dispersion, and then dopamine hydrochloride is added to the dispersion. After the addition, the pH of the dispersion is adjusted, and the dispersion is stirred at a stirring rate of 200-500 r / min for 6-8 hours at room temperature, and the solid material is collected by centrifugation, washed, and dried to obtain modified nanoparticles; The polyester additive component is prepared by olefinic modification of a copolymerization product of 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and a perfluorocarboxylic acid compound; The polyester additive component is prepared by the following method: Step 1: Prepare material A 4,6-bis(1-adamantyl)-1,3-diglycidyl ether benzene and toluene are added to a reactor, nitrogen is introduced, and after the air in the reactor is exhausted, stirring is started until a homogeneous solution is formed, and then a perfluorocarboxylic acid compound is added to the reactor. After the addition is completed, the temperature is increased to 60-65°C, and stirred at this temperature for 2-4 hours, and then a phase transfer catalyst is added to the reactor, and the temperature is further increased to 70-75°C. After maintaining this temperature condition for 6-8 hours, the temperature is reduced and the material is discharged, and the obtained material is material A; Step 2: Preparation of polyester additive components Material A is mixed with tetrahydrofuran to form a uniform solution, and then placed in an ice bath. The acyl chloride compound is added to the solution. After the addition is completed, the ice bath is removed and the accelerator is continued to be added. After mechanical stirring for 3-6 hours at room temperature, the material is separated to obtain the polyester additive component.

2. A hardening coating liquid with high wear resistance according to claim 1, characterized in that: The multifunctional polyurethane acrylate is tetrafunctional polyurethane acrylate or hexafunctional polyurethane acrylate; the epoxy acrylate monomer is any one of glycidyl methacrylate, allyl glycidyl ether or glycidyl acrylate; and the organic solvent is acetone or ethyl acetate.

3. The hardening coating liquid with high wear resistance according to claim 1, characterized in that: The pH is 8-9.

4. The hardening coating liquid with high wear resistance according to claim 1, characterized in that: In step 1, the perfluorocarboxylic acid compound is perfluorosebacic acid or perfluorooctanedioic acid.

5. The hardening coating liquid with high wear resistance according to claim 1, characterized in that: In step 1, the phase transfer catalyst is any one of tetramethylammonium bromide, tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate or N,N-dimethylbenzylamine.

6. A hardening coating liquid with high wear resistance according to claim 1, characterized in that: In step 2, the acyl chloride compound is methacryloyl chloride or acryloyl chloride.

7. A hardening coating liquid with high wear resistance according to claim 1, characterized in that: In step 2, the promoter is triethylamine or pyridine.

8. A hardening coating liquid with high wear resistance as claimed in claim 1, characterized in that: The following steps are involved: The first step is to weigh each raw material according to the weight and set aside; Step 2: Mix the multifunctional polyurethane acrylate and the organic solvent, stir and mix them evenly at a stirring rate of 300-500 r / min, then add the polyester additive component, epoxy acrylate monomer, leveling agent and photoinitiator, and continue stirring for 30-60 minutes to form a precursor solution; The third step is to add the modified nanoparticles into the precursor solution and disperse them evenly to obtain a hardening coating solution.

Citation Information

Patent Citations

  • Anti-fog and anti-glare hardened film

    CN115850803B

  • Anti-fouling and anti-UV (ultraviolet) coating composition, hard coating film and preparation method

    CN105273586A

  • Wear-resistant antifouling antistatic hardened film and preparation method thereof

    CN112661998A

  • Laminate for coating the surface of optical article

    JP2007137057A

  • Hard Coating Composition and Hard Coating Film Using the Same

    KR1020170097376A