A self-diagnostic and self-repairing intelligent coating based on microfluidic technology and its preparation method

Microcapsules prepared through microfluidic technology and interfacial polymerization solve the problem of difficulty in self-detection and self-healing of polymer coatings, realize the self-detection and self-healing functions of the coating, and significantly increase the service life and performance of the coating. performance.

CN118440595BActive Publication Date: 2024-10-01CHINA JILIANG UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410903615.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-01
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

It is difficult for existing polymer coatings to promptly detect and self-repair nano- and micron-level defects when affected by environmental factors, resulting in reduced performance and matrix damage. In addition, existing microcapsule preparation methods have problems with agglomeration and uneven distribution.

Method used

Microfluidic technology was used to prepare microcapsules coated with diagnostic agents and repair agents. Microcracks were observed through a fluorescence microscope and self-repaired under UV light induction. Polyurea was used as the shell material, and 1,3-bis(3-glycidol) Oxypropyl)-1,1,3,3-tetramethyldisiloxane and rhodamine B were used as repair agents and diagnostic agents, and triarylsulfonium hexafluorophosphate was used as a photoinitiator, combined with interfacial polymerization method to prepare spherical microstructures. capsule.

Benefits of technology

The self-detection and self-healing functions of the coating are realized. The microcapsules have a smooth surface and uniform size, which can effectively monitor and repair micro-cracks, extend the service life of the coating, and have practical application prospects in special environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118440595B_ABST
    Figure CN118440595B_ABST
Patent Text Reader

Abstract

The present invention discloses a self-diagnostic and self-repairing intelligent coating based on microfluidic technology and a preparation method thereof, which belongs to the technical field of coatings. The present invention prepares microcapsules by combining a microfluidic T-junction and interfacial polymerization. The wall material of the microcapsule is composed of polyurea, and the core material is composed of a diagnostic agent, a repair agent and a photoinitiator. The self-diagnostic and self-repairing microcapsules are evenly distributed in a coating based on silicone resin. The self-diagnostic and self-repairing coating provided by the present invention has the function of spontaneously detecting microcracks in the coating, and prompting the generation of microcracks in a fluorescent manner. At the same time, it has the function of ultraviolet-induced spontaneous repair of microcracks generated in the coating. The present invention realizes the monitoring and self-healing of the initial formation of microcracks in the coating, and is expected to be practically applied in special environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of coatings, and in particular relates to a self-diagnostic and self-repairing intelligent coating based on microfluidic technology and a preparation method thereof. Background Art

[0002] As a vital functional material and protective technology, polymer coatings are widely used on the surface of important components to improve their protective performance and extend the service life of the substrate. However, during the use of the coating, it is inevitable that microcracks will be generated due to the influence of various environmental factors. The formation and expansion of microcracks will cause a sharp decrease in the mechanical stability of the coating, thereby reducing the performance of the coating and eventually causing permanent damage to the substrate material. If the microcracks are detected in time at the early stage of formation, appropriate measures can be taken to protect the substrate from damage.

[0003] Although self-diagnostic coatings can indicate coating defects, they cannot automatically repair nano- and micro-scale defects. Replacing failed coatings will waste manpower and material resources; developing a resin matrix with higher performance will greatly increase the development cost and time cost. Therefore, it is of great research significance to give the coating a self-diagnostic method to timely self-indicate initial microcracks and give it self-healing behavior to extend the performance cycle and service life of the coating.

[0004] In order to protect the diagnostic agent and the repair agent, there is a method in the prior art to encapsulate the fluorescent molecules and the repair molecules with microcapsules to prevent them from reacting with the active groups in the coating prematurely or being degraded by ultraviolet light, thereby affecting the self-diagnosis and self-repair performance. The biggest advantages of the microcapsule-based external aid self-repairing coating are: the isotropic spherical microcapsules have good dispersion in the resin matrix; a variety of wall materials and core materials; and a rich preparation method. When microcracks appear in the coating, the microcapsules embedded in the resin matrix rupture, and the repair agent flows out to fill the microcrack area, thereby repairing the cracks.

[0005] In a large number of studies, although the preparation methods of microcapsules (such as in situ polymerization, interfacial polymerization, emulsion polymerization, etc.) can obtain better microcapsules to a certain extent, the microcapsules are easy to agglomerate, the preparation process is more complicated, and the distribution is uneven. The precise flow control provided by microfluidics provides a potential means to overcome these limitations. The use of microfluidics to prepare monodisperse emulsions and monodisperse microcapsules can achieve the repeatable and controllable preparation of microcapsules with uniform particle size. At present, there is no report on the preparation of self-diagnostic and self-healing smart coatings of microcapsules that simultaneously encapsulate diagnostic agents and repair agents based on microfluidics. Summary of the invention

[0006] In order to solve the above technical problems, the present invention proposes a self-diagnostic and self-repairing smart coating based on microfluidic technology and a preparation method thereof. The smart coating is prepared by uniformly blending microcapsules coated with diagnostic agents and repair agents with a silicone resin matrix. During the service engineering, the coating can observe the generation of microcracks through a fluorescence microscope and timely perform ultraviolet-induced microcrack self-repair.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A self-diagnostic and self-repairing smart coating based on microfluidic technology, the raw materials of which include microcapsules and a resin matrix;

[0009] The microcapsule is composed of a shell material and a coating material;

[0010] The shell material is polyurea;

[0011] The coating material is a repair agent, a diagnostic agent (fluorescent molecule) and a photoinitiator;

[0012] The repair agent is 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane;

[0013] The diagnostic agent (fluorescent molecule) is rhodamine B;

[0014] The photoinitiator is triarylsulfonium hexafluorophosphate.

[0015] The term "coating material" in the present invention refers to the core material of the microcapsule.

[0016] Furthermore, the resin matrix is ​​a mixture of a self-drying silicone resin and a silane coupling agent in a mass ratio of 20:1; the mass content of the microcapsules in the raw materials is 11.1-14.3%, preferably 11.1%, 12.5% ​​and 14.3%.

[0017] The present invention also provides a method for preparing a self-diagnostic and self-repairing intelligent coating based on microfluidic technology, comprising the following steps:

[0018] The microfluidic technology is used to pump the dispersed phase solution and the continuous phase solution into the polytetrafluoroethylene tube 1 and the polytetrafluoroethylene tube 2 in the microfluidic chip respectively. In the chip, the dispersed phase solution is sheared into uniform droplets by the continuous phase solution. The droplets are passed into the reaction solution which is continuously mechanically stirred to form a polyurea membrane. After the chip shearing of the droplets is completed, the reaction solution is placed in a water bath for continuous heating and stirring. The polyurea membrane grows and becomes thicker to become a polyurea-based microcapsule. The obtained polyurea-based microcapsules are washed with cyclohexane, ultrasonicated, centrifuged and then dried naturally to obtain microcapsules.

[0019] The microcapsules are mixed with a resin matrix to obtain a self-diagnostic and self-repairing smart coating based on microfluidic technology;

[0020] The self-diagnosis and self-repairing smart coating based on microfluidics technology is coated on a glass slide and cured to obtain a self-diagnosis and self-repairing smart coating based on microfluidics technology;

[0021] The preparation method of the dispersed phase solution is as follows: ultrasonically mixing 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, triarylsulfonium hexafluorophosphate, rhodamine B and tetraethylenepentamine;

[0022] The preparation method of the continuous phase solution is: ultrasonically mixing the n-hexadecane solution and polyethylene glycol dipolyhydroxystearate;

[0023] The preparation method of the reaction solution is: ultrasonically mixing 4,4-dicyclohexylmethane diisocyanate, decalin, polyethylene glycol dipolyhydroxystearate and triethylenediamine.

[0024] Furthermore, the flow rate of the dispersed phase solution is 0.02 mL / min, and the flow rate of the continuous phase solution is 0.4-0.6 mL / min.

[0025] Furthermore, the mechanical stirring rate is 100 rpm; the heating stirring parameters are: temperature 40-60°C, time 1-2h, stirring rate 200 rpm.

[0026] Furthermore, in the microfluidic chip, the polytetrafluoroethylene tube 1 is inserted into the polytetrafluoroethylene tube 2 and is 30 mm away from the outlet end of the polytetrafluoroethylene tube 2 .

[0027] Furthermore, the polytetrafluoroethylene tube 1 has an inner diameter of 0.46 mm and an outer diameter of 0.76 mm, and is connected to a syringe containing a dispersed phase solution;

[0028] The polytetrafluoroethylene tube 2 has an inner diameter of 0.96 mm and an outer diameter of 1.26 mm. Its inlet end is connected to a syringe filled with a continuous phase solution, and its outlet end is connected to the reaction solution.

[0029] Compared with the prior art, the present invention has the following advantages and technical effects:

[0030] (1) The smart coating of the present invention has diversified functions by adding microcapsules with self-detection and self-repairing functional molecules, giving the coating self-repair and self-detection functions. When microcracks appear and cause the microcapsules to rupture, the diagnostic agent and healing agent in the microcapsules flow out and fill the microcrack area. At this time, the fluorescent reaction can be observed to monitor the generation of microcracks. When the coating is irradiated under ultraviolet conditions, the microcracks heal themselves due to the curing of the healing agent.

[0031] (2) The core-shell microcapsules obtained based on microfluidics technology and interfacial polymerization have a smooth surface and a small size (~0.95 μm), which is much smaller than the core-shell microcapsules prepared using only traditional microfluidics technology, and are more uniform in size than the core-shell microcapsules prepared only using interfacial polymerization.

[0032] (3) The present invention prepares microcapsules that simultaneously encapsulate diagnostic agents and repair agents based on microfluidic technology and interfacial polymerization. The size structure of the microcapsules and the coverage rate of the repair agent in the microcapsules can be controlled by adjusting the content of each component of the dispersed phase and the flow rate of the dispersed phase and the continuous phase. The obtained microcapsules have a smooth surface morphology and a core-shell structure, with good sphericity and a high degree of monodispersity.

[0033] (4) The highly efficient method for preparing small-sized core-shell microcapsules based on microfluidics and interfacial polymerization has good application prospects in the field of coatings. In addition, the monitoring and self-healing of the initial formation of coating microcracks achieved by the present invention have practical application prospects under special environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0035] Figure 1 It is a schematic diagram of the preparation method of the present invention;

[0036] Figure 2 This is a scanning electron microscope image of the microcapsules prepared in Example 1;

[0037] Figure 3 Thermogravimetric diagrams of microcapsules prepared in Examples 1-3 and the thermal conductivity diagram of Example 1; a-thermogravimetric diagram of Example 2, b-thermogravimetric diagram of Example 1, c-thermogravimetric diagram of Example 3, d-thermogravimetric diagram of Example 1;

[0038] Figure 4 are scanning electron microscope images of microcapsules; a-scanning electron microscope image of comparative example 4, b-scanning electron microscope image of comparative example 1, c-scanning electron microscope image of comparative example 2, d-scanning electron microscope image of comparative example 5, e-scanning electron microscope image of embodiment 2, f-scanning electron microscope image of embodiment 3;

[0039] Figure 5 Thermogravimetric diagrams of microcapsules; a-thermogravimetric diagram of comparative example 5, b-thermogravimetric diagram of comparative example 1, c-thermogravimetric diagram of comparative example 2;

[0040] Figure 6Fluorescence microscope images of the coating before and after microcracks are generated in Example 1; a-fluorescence microscope image of the blank control group, b-fluorescence microscope image of ultraviolet irradiation 0h, c-fluorescence microscope image of ultraviolet irradiation 8h, d-fluorescence microscope image of ultraviolet irradiation 16h, e-fluorescence microscope image of ultraviolet irradiation 24h, f-fluorescence microscope image of ultraviolet irradiation 48h;

[0041] Figure 7 The morphology of the repair process of coating microcracks; a-the morphology of the repair process of coating microcracks in comparative example 4, b-the morphology of the repair process of coating microcracks in example 4, c-the morphology of the repair process of coating microcracks in example 1, d-the morphology of the repair process of coating microcracks in example 5. DETAILED DESCRIPTION

[0042] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0043] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0044] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0045] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0046] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0047] The "room temperature" in the present invention refers to 20-30°C unless otherwise specified.

[0048] The raw materials used in the present invention are all purchased from the market.

[0049] Microfluidics refers to the technology of processing or manipulating tiny fluids in microchannels by making microfluidic chips using glass capillaries or polytetrafluoroethylene tubes. This technology precisely controls the flow and dispersion of multiphase fluids in microscale space, thereby achieving precise control of the size and morphology of composite emulsion particles and producing uniform droplets. Multiple immiscible fluids are sheared into single O / W (W / O) or double O / W / O (W / O / W) or even higher-order template droplets, which are then solidified into microcapsules.

[0050] The present invention prepares microcapsules by a method combining microfluidic T-junction and interfacial polymerization. The wall material of the microcapsule is composed of polyurea, and the core material is composed of a repair agent, a diagnostic agent and a photoinitiator. The self-diagnostic and self-repairing microcapsules are evenly distributed in a coating based on silicone resin. The self-diagnostic and self-repairing coating provided by the present invention has the function of spontaneously detecting microcracks in the coating and prompting the generation of microcracks in a fluorescent manner. At the same time, it has the function of ultraviolet-induced spontaneous repair of microcracks generated in the coating. The present invention realizes the monitoring and self-healing of the initial formation of microcracks in the coating, has important economic significance, and is expected to be practically applied in special environments.

[0051] The present invention provides a self-diagnostic and self-repairing intelligent coating based on microfluidic technology, comprising microcapsules and a resin matrix;

[0052] The microcapsule is composed of a shell material and a coating material;

[0053] The shell material is polyurea, which is harmless, has excellent mechanical and chemical stability, and has a high cross-linking density;

[0054] The coating material is a repair agent, a diagnostic agent (fluorescent molecule) and a photoinitiator;

[0055] The repair agent is 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane;

[0056] The diagnostic agent (fluorescent molecule) is rhodamine B;

[0057] The photoinitiator is triarylsulfonium hexafluorophosphate.

[0058] The present invention uses 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane as a repair agent, which is a specific functional group contained in the molecular structure, such as glycidyloxypropyl. When the coating is damaged and the capsule is broken, the repair agent is released from the microcapsule. At this time, the glycidyloxypropyl forms new chemical bonds or crosslinking points under the action of the photoinitiator and solidifies, thereby filling the damaged area and restoring the integrity of the coating. The fluorescent molecules play an indicating role. When the coating is broken, the fluorescent molecules indicate the cracks, and the repair agent repairs the cracks at the same time, thereby playing a dual role of self-diagnosis and self-repair.

[0059] In the following preferred embodiments of the present invention, the resin matrix is ​​a mixture of self-drying silicone resin and silane coupling agent, with a mass ratio of 20:1; in the self-diagnostic and self-repairing intelligent coating, the mass ratio of microcapsules to resin matrix is ​​1:(6-8), preferably 1:8, 1:7 and 1:6.

[0060] The method for preparing the self-diagnostic and self-repairing intelligent coating based on microfluidic technology comprises the following steps:

[0061] 1) Preparation method of dispersed phase solution: 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, triarylsulfonium hexafluorophosphate, rhodamine B and tetraethylenepentamine are ultrasonically mixed;

[0062] 2) Preparation method of continuous phase solution: ultrasonically mix the n-hexadecane solution and polyethylene glycol dipolyhydroxystearate (as long as the raw materials can be dissolved and dispersed, without special limitation, the same below);

[0063] 3) A method for preparing a reaction solution: ultrasonically mixing 4,4-dicyclohexylmethane diisocyanate, decalin, polyethylene glycol dipolyhydroxystearate and triethylenediamine;

[0064] 4) Using microfluidic technology, using syringe pumps with different flow rates to pump the dispersed phase solution and the continuous phase solution into the polytetrafluoroethylene tube 1 and the polytetrafluoroethylene tube 2 in the microfluidic chip respectively, in the chip, the dispersed phase solution is sheared into uniform droplets by the continuous phase solution, and the droplets are passed into the reaction solution with continuous mechanical stirring, and the polyamine in the polytetrafluoroethylene tube 1 reacts with the isocyanate in the reaction solution, and the interface is immediately polymerized to form a polyurea membrane, which wraps the repair agent, the diagnostic agent and the photoinitiator; after the chip shearing of the droplets is completed, the reaction solution is placed in a water bath for continuous heating and stirring, and the polyurea membrane grows and becomes thicker, turning into polyurea-based microcapsules; the obtained polyurea-based microcapsules are washed with cyclohexane, ultrasonicated for 20-30 minutes, centrifuged at 6000 rpm for 5 minutes, and then dried naturally to obtain microcapsules;

[0065] The present invention performs thermogravimetric testing on the microcapsules in the embodiment to analyze the microcapsules with the best coverage of the repair agent, and then performs step 5) and step 6), and performs performance testing on them.

[0066] 5) mixing the microcapsules with a resin matrix (formed by mixing a self-drying silicone resin and a silane coupling agent in a mass ratio of 20:1) in mass ratios of 1:8, 1:7 and 1:6, respectively, to obtain a self-diagnostic and self-repairing smart coating based on microfluidic technology;

[0067] 6) The self-diagnostic and self-repairing smart coating based on microfluidic technology is coated on a glass slide and cured at 75° C. for more than 24 hours to obtain a self-diagnostic and self-repairing smart coating based on microfluidic technology.

[0068] In the following preferred embodiment 1) of the present invention, the mass ratio of 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, triarylsulfonium hexafluorophosphate, rhodamine B and tetraethylenepentamine is preferably 1.1:0.09:0.09:1.

[0069] In the following preferred embodiment 2) of the present invention, the mass ratio of the n-hexadecane solution to polyethylene glycol dipolyhydroxystearate is 2.784:0.027.

[0070] In the following preferred embodiment 3) of the present invention, the mass ratio of 4,4-dicyclohexylmethane diisocyanate, decalin, polyethylene glycol dipolyhydroxystearate and triethylenediamine is 9:67.2:0.75:0.75.

[0071] In the following preferred embodiment 4) of the present invention, the flow rate of the dispersed phase solution is 0.02 mL / min, and the flow rate of the continuous phase solution is 0.4-0.6 mL / min, preferably 0.4 mL / min, 0.5 mL / min or 0.6 mL / min, and more preferably 0.5 mL / min.

[0072] Before the chip shearing droplet is completed, the mechanical stirring rate is 100 rpm; the parameters of the heating and stirring are: temperature 40-60°C, time 1-2h, stirring rate 200rpm, and heating is specifically: heating and stirring at 40°C for 1h, then heating and stirring at 50°C for 2h, and finally heating and stirring at 60°C for 2h, during which the stirring rate is 200 rpm.

[0073] In the microfluidic chip, the polytetrafluoroethylene tube 1 is inserted into the polytetrafluoroethylene tube 2 and is 30 mm away from the outlet of the polytetrafluoroethylene tube 2. The polytetrafluoroethylene tube 1 has an inner diameter of 0.46 mm and an outer diameter of 0.76 mm, and is connected to a syringe filled with a dispersed phase solution; the polytetrafluoroethylene tube 2 has an inner diameter of 0.96 mm and an outer diameter of 1.26 mm, and its inlet end is connected to a syringe filled with a continuous phase solution, and its outlet end is passed into the reaction solution.

[0074] The technical solution of the present invention is further illustrated by the following embodiments.

[0075] Figure 1 It is a schematic diagram of the preparation method of the present invention.

[0076] Embodiment 1:

[0077] The preparation method of the self-diagnosis and self-repairing intelligent coating based on microfluidic technology comprises the following steps:

[0078] 1) Preparation of dispersed phase solution: 1.1 g of 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, 0.09 g of triarylsulfonium hexafluorophosphate, 0.09 g of rhodamine B and 1 g of tetraethylenepentamine were ultrasonically mixed;

[0079] 2) Preparation of continuous phase solution: 13.92 g of n-hexadecane solution and 0.135 g of polyethylene glycol dipolyhydroxystearate were ultrasonically mixed;

[0080] 3) Preparation of a reaction solution: 9 g of 4,4-dicyclohexylmethane diisocyanate, 67.2 g of decalin, 0.75 g of polyethylene glycol dipolyhydroxystearate and 0.75 g of triethylenediamine were ultrasonically mixed;

[0081] 4) Using microfluidic technology, the flow rate of the dispersed phase solution was adjusted to 0.02 mL / min, and the flow rate of the continuous phase solution was adjusted to 0.5 mL / min. The dispersed phase solution was pumped into the polytetrafluoroethylene tube 1 and the polytetrafluoroethylene tube 2 in the microfluidic chip respectively using a syringe pump. In the chip, the dispersed phase solution was sheared into uniform droplets by the continuous phase solution. The droplets were introduced into the reaction solution that was continuously mechanically stirred at a speed of 100 rpm. The tetraethylene pentamine in the polytetrafluoroethylene tube 1 reacted with the isocyanate in the reaction solution, and the interface was immediately polymerized to form a polyurea membrane, which encapsulated the repair agent, the diagnostic agent and the photoinitiator. After the chip shearing of the droplets was completed, the reaction solution was placed in a water bath and reacted at 40°C for 1 hour, 50°C for 2 hours, and 60°C for 2 hours, while maintaining a speed of 200 rpm, so that the polyurea membrane grew thicker and became polyurea-based microcapsules. The obtained polyurea-based microcapsules were washed with cyclohexane, ultrasonicated for 25 minutes, centrifuged at 6000 rpm for 5 minutes, and then dried naturally to obtain microcapsules.

[0082] 5) mixing the microcapsules with a resin matrix (formed by mixing a self-drying silicone resin and a silane coupling agent in a mass ratio of 20:1) in a mass ratio of 1:7 to obtain a self-diagnostic and self-repairing smart coating based on microfluidic technology;

[0083] 6) The self-diagnostic and self-repairing smart coating based on microfluidic technology is coated on a glass slide and cured at 75° C. for more than 24 hours to obtain a self-diagnostic and self-repairing smart coating based on microfluidic technology (named MC-12.5).

[0084] Figure 2 This is a scanning electron microscope image of the microcapsules prepared in Example 1. Figure 2 It can be seen that according to the method of Example 1, spherical complete microcapsules can be obtained, and the particle size is uniform, about 0.95 μm.

[0085] Example 2

[0086] Same as Example 1, except that in step 4), the flow rate of the continuous phase solution is 0.4 mL / min.

[0087] Example 3

[0088] Same as Example 1, except that in step 4), the flow rate of the continuous phase solution is 0.6 mL / min.

[0089] Figure 3 The thermogravimetric diagrams of the microcapsules prepared in Examples 1-3 and the thermogravimetric diagram of Example 1 are shown in Table 1. Figure 3 It can be seen that the coverage rate of the repair agent in the microcapsules of Example 1 is the highest, up to 14%, the coverage rate of the repair agent in the microcapsules of Example 2 is 9%, and the coverage rate of the repair agent in the microcapsules of Example 3 is 8%. It is found that the coverage rate of the repair agent decreases when the flow rate increases from 0.5 mL / min to 0.6 mL / min. Therefore, the subsequent experiments of the present invention use the microcapsules prepared in Example 1 as raw materials to prepare the coating.

[0090] Example 4

[0091] The same as Example 1, except that in step 5), the microcapsules and the resin matrix are mixed in a mass ratio of 1:8, and the obtained coating is named MC-11.1.

[0092] Example 5

[0093] The same as Example 1, except that in step 5), the microcapsules and the resin matrix are mixed in a mass ratio of 1:6, and the obtained coating is named MC-14.3.

[0094] Comparative Example 1

[0095] Same as Example 1, except that, in step 1), the dispersed phase solution is prepared by ultrasonically mixing 1 g of 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, 0.08 g of triarylsulfonium hexafluorophosphate, 0.08 g of rhodamine B and 1 g of tetraethylenepentamine.

[0096] Comparative Example 2

[0097] Same as Example 1, except that, in step 1), the dispersed phase solution is prepared by ultrasonically mixing 1.2 g of 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, 1 g of triarylsulfonium hexafluorophosphate, 1 g of rhodamine B and 1 g of tetraethylenepentamine.

[0098] Comparative Example 3

[0099] The same as Example 1, except that the repairing agent 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane in step 1) is replaced by epoxy resin. It was found that under this experimental condition, microcapsules were not successfully formed.

[0100] Comparative Example 4

[0101] Step 1) Preparation of dispersed phase solution: Take 1 g of tetraethylenepentamine as dispersed phase solution;

[0102] Step 2) is the same as in Example 1;

[0103] Step 3) is the same as in Example 1;

[0104] Step 4) using microfluidic technology, adjusting the flow rate of the dispersed phase solution to 0.02 mL / min and the flow rate of the continuous phase solution to 0.5 mL / min, and using a syringe pump to pump them into the polytetrafluoroethylene tube 1 and the polytetrafluoroethylene tube 2 in the microfluidic chip respectively, in the chip, the dispersed phase solution is sheared into uniform droplets by the continuous phase solution, and the droplets are introduced into the reaction solution that is continuously mechanically stirred at a speed of 100 rpm, and the tetraethylene pentamine in the polytetrafluoroethylene tube 1 reacts with the isocyanate in the reaction solution, and the interface is immediately polymerized to form a polyurea membrane; after the chip shearing of the droplets is completed, the reaction solution is placed in a water bath and reacted at 40°C for 1 hour, 50°C for 2 hours, and 60°C for 2 hours, maintaining a speed of 200 rpm, so that the polyurea membrane grows and thickens to become a polyurea-based microcapsule; the obtained polyurea-based microcapsules are washed with cyclohexane, ultrasonicated for 25 minutes, and centrifuged at 6000 rpm for 5 minutes and then dried naturally to obtain microcapsules without diagnostic agent repair agent;

[0105] Step 5) mixing the microcapsules with a resin matrix (formed by mixing a self-drying silicone resin and a silane coupling agent in a mass ratio of 20:1) in a mass ratio of 1:7 to obtain a blank coating based on microfluidic technology without a diagnostic agent or a repair agent;

[0106] Step 6) The coating of the microcapsules without a repair agent based on microfluidics is coated on a glass slide and cured at 75° C. for more than 24 hours to obtain a blank coating without a diagnostic agent repair agent based on microfluidics, which is named BS-12.5.

[0107] Comparative Example 5

[0108] Same as Example 3, except that the flow rate of the continuous phase solution in step 4) is 0.2 mL / min.

[0109] Performance Testing

[0110] from Figure 4 As can be seen from e and f in the figure, spherical complete microcapsules can be obtained according to the methods of Examples 2 and 3, and the particle size is uniform, about 0.95 μm; Figure 4 It can be seen from a, b, c, and d in that the sizes of the microcapsules prepared according to Comparative Examples 4, 1, 2, and 5 are all about 0.95 μm, among which the microcapsules of Comparative Example 4 are more obviously agglomerated.

[0111] from Figure 5 As can be seen from a in the figure, the coverage rate of the repair agent in the microcapsules prepared according to the method of Comparative Example 5 is almost 0; Figure 5 It can be seen from b that the repair agent in the microcapsules prepared according to the method of Comparative Example 1 was not successfully coated; Figure 5 As can be seen from c in FIG. 1 , the repair agent in the microcapsules prepared according to the method of Comparative Example 2 was not successfully encapsulated.

[0112] It was also found that the microcapsules prepared according to the method of Comparative Example 4 contained no repairing agent.

[0113] Figure 6 These are fluorescence microscope images of the coating in Example 1 before and after microcracks are generated (0h, 8h, 16h, 24h, 48h); it can be seen from the figure that the complete coating has no fluorescence; when microcracks appear in the coating, the fluorescence effect is strongest at the microcracks; with the increase of ultraviolet irradiation time, the fluorescence effect begins to gradually weaken, indicating that the repair agent in the coating gradually plays a self-repairing role and the fluorescent agent is degraded under ultraviolet irradiation.

[0114] Figure 7 : The morphology of the coating microcrack repair process (8h, 16h, 24h, 48h) in Example 1, Example 4, Example 5 and Comparative Example 4; a is the microcapsules without a repair agent and the resin matrix in Comparative Example 4 prepared in a mass ratio of 1:7. It can be seen from the figure that the coating in Comparative Example 4 without the addition of a repair agent has almost no change in crack morphology after 48h, indicating that the coating in Comparative Example 4 does not have a self-repairing function. Figure 7b, c, and d in the figure are samples prepared by microcapsules and resin matrix prepared in Example 4, Example 1, and Example 5 at a mass ratio of 1:8, 1:7, and 1:6, respectively. It can be seen that in Example 4, Example 1, and Example 5, a repairing agent is added, and the repairing agent begins to work after cracks appear. As the ultraviolet irradiation time increases, the cracks gradually become smaller until they almost disappear, which further proves that Figure 6 Changes from Figure 7 It can be seen from b and c that the repair effect gradually increases with the increase of microcapsules; Figure 7 The content of microcapsules in d is the highest. Due to the uneven dispersion of microcapsules in the resin matrix, the repair effect is slightly lower than Figure 7 c in.

[0115] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A self-diagnostic and self-repairing intelligent coating based on microfluidic technology, characterized in that: The raw materials include microcapsules and resin matrix; The microcapsule is composed of a shell material and a coating material; The shell material is polyurea; The coating material is a repair agent, a diagnostic agent and a photoinitiator; The repair agent is 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane; The diagnostic agent is rhodamine B; The photoinitiator is triarylsulfonium hexafluorophosphate; The resin matrix is ​​a mixture of self-drying silicone resin and silane coupling agent in a mass ratio of 20:1; the mass content of the microcapsules in the raw materials is 11.1-14.3%; The method for preparing the self-diagnostic and self-repairing intelligent coating based on microfluidic technology comprises the following steps: The microfluidic technology is used to pump the dispersed phase solution and the continuous phase solution into the polytetrafluoroethylene tube 1 and the polytetrafluoroethylene tube 2 in the microfluidic chip respectively. In the chip, the dispersed phase solution is sheared into uniform droplets by the continuous phase solution. The droplets are passed into the reaction solution which is continuously mechanically stirred to form a polyurea membrane. After the chip shearing of the droplets is completed, the reaction solution is placed in a water bath for continuous heating and stirring. The polyurea membrane grows and becomes thicker to become a polyurea-based microcapsule. The obtained polyurea-based microcapsules are washed with cyclohexane, ultrasonicated, centrifuged and then dried naturally to obtain microcapsules. The microcapsules are mixed with a resin matrix to obtain a self-diagnostic and self-repairing smart coating based on microfluidic technology; The self-diagnosis and self-repairing smart coating based on microfluidics technology is coated on a glass slide and cured to obtain a self-diagnosis and self-repairing smart coating based on microfluidics technology; The preparation method of the dispersed phase solution is: ultrasonically mixing 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, triarylsulfonium hexafluorophosphate, rhodamine B and tetraethylenepentamine; The preparation method of the continuous phase solution is: ultrasonically mixing the n-hexadecane solution and polyethylene glycol dipolyhydroxystearate; The preparation method of the reaction solution is: ultrasonically mixing 4,4-dicyclohexylmethane diisocyanate, decalin, polyethylene glycol dipolyhydroxystearate and triethylenediamine.

2. The self-diagnostic and self-repairing smart coating based on microfluidic technology according to claim 1, characterized in that: The mass ratio of the 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, triarylsulfonium hexafluorophosphate, rhodamine B and tetraethylenepentamine is 1.1:0.09:0.09:

1.

3. The self-diagnostic and self-repairing smart coating based on microfluidic technology according to claim 1, characterized in that: The mass ratio of the n-hexadecane solution to polyethylene glycol dipolyhydroxystearate is 2.784:0.

027.

4. The self-diagnostic and self-repairing smart coating based on microfluidic technology according to claim 1, characterized in that: The mass ratio of the 4,4-dicyclohexylmethane diisocyanate, decalin, polyethylene glycol dipolyhydroxystearate and triethylenediamine is 9:67.2:0.75:0.

75.

5. The self-diagnostic and self-repairing smart coating based on microfluidic technology according to claim 1, characterized in that: The flow rate of the dispersed phase solution is 0.02 mL / min, and the flow rate of the continuous phase solution is 0.4-0.6 mL / min.

6. The self-diagnostic and self-repairing smart coating based on microfluidic technology according to claim 1, characterized in that: The mechanical stirring rate is 100 rpm; the heating stirring parameters are: temperature 40-60°C, time 1-2h, stirring rate 200 rpm.

Citation Information

Patent Citations

  • Micro-crack self-repairing microcapsule and preparation method thereof

    CN102702838A

  • Self-repairing microcapsules for concrete, preparing method thereof and microcapsule self-healing coating

    CN106220014A

  • Method for generating double-sized micro-droplets based on microfluidic chip

    CN108671970A

  • Double emulsified glass capillary microfluidic chip and phase change microcapsule prepared thereby

    CN109201130A

  • Photo-initiated self-early-warning or self-repairing microcapsule coated fabric and preparation method thereof

    CN115679708A