A method for preparing hydrophilic modified polyvinylidene fluoride filter membrane

Through sodium hydroxide treatment and graft polymerization technology, hydrophilic monomers and crosslinking agents are introduced on the polyvinylidene fluoride filter membrane to form a crosslinking network structure, which solves the problem of insufficient hydrophilicity of the polyvinylidene fluoride filter membrane. It achieves excellent hydrophilic properties and bactericidal effects, extending the service life of the membrane.

CN118454487BActive Publication Date: 2024-11-08SHANGHAI LEPURE BIOTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410625821.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-20
Publication Date
2024-11-08
Estimated Expiration
2044-05-20

AI Technical Summary

Technical Problem

Due to the low surface energy, poor wetting performance and strong hydrophobicity of polyvinylidene fluoride, polyvinylidene fluoride membranes are easily contaminated by organic matter, resulting in shortening of service life. The existing modification methods have problems such as hydrophilic component release, high equipment investment and structural damage. .

Method used

The polyvinylidene fluoride filter membrane is treated with sodium hydroxide, and hydrophilic monomers and crosslinking agents are introduced on its surface through graft polymerization technology to form a crosslinking network structure to enhance its hydrophilic properties, and at the same time, it uses modified vinyl groups. The quaternary ammonium salt intermediate initiates a reaction with ammonium persulfate to form a modified film with excellent hydrophilic properties.

Benefits of technology

The permanent modification of the polyvinylidene fluoride filter membrane is achieved, which improves its hydrophilic properties and bactericidal effect, avoids the dissolution and release of hydrophilic components, extends the service life of the membrane, and simplifies the modification process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118454487B_ABST
    Figure CN118454487B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of filter membranes, and discloses a method for preparing a hydrophilic modified polyvinylidene fluoride filter membrane. The invention uses ethylenediamine, 5-chlorovaleric acid, 1,3-propane sultone, 3-chloropropylene and the like as raw materials, and reacts to prepare a modified vinyl quaternary ammonium salt intermediate, and then carries out graft polymerization with an alkalized polyvinylidene fluoride filter membrane under the initiation of ammonium persulfate to obtain a hydrophilic modified polyvinylidene fluoride filter membrane. The modified polyvinylidene fluoride filter membrane prepared by the invention has excellent hydrophilic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of filtration membranes, in particular to a method for preparing a hydrophilic modified polyvinylidene fluoride filtration membrane. Background Art

[0002] Polyvinylidene fluoride filter membrane is a membrane material with excellent performance. It has excellent chemical corrosion resistance, radiation resistance, heat resistance and other properties. It is widely used in chemical, textile, food and other fields. However, due to the low surface energy, poor wettability and strong hydrophobicity of polyvinylidene fluoride, it is easily contaminated by organic matter, resulting in a shortened membrane service life. Therefore, how to improve the hydrophilicity of polyvinylidene fluoride filter membrane to extend its service life is the focus of current research.

[0003] Traditional modification methods include blending modification, grafting polymerization modification, etc., and the methods used include plasma method, radiation initiation, ultraviolet light initiation polymerization, etc., but these methods have their own defects. In traditional blending modification, the hydrophilic components exist in the filter membrane in the form of physical mixing, which will lead to the continuous release of hydrophilic components, especially when coexisting with acids, alkalis, and strong oxidizing substances, the dissolution release is very serious, which will also lead to changes in the performance of the filter membrane itself; secondly, the procurement of plasma, ultraviolet light and other radiation modification methods, on the one hand, the equipment investment is expensive, on the other hand, these high-energy treatment methods will cause the destruction of the filter membrane structure, thereby causing changes in the performance of the filter membrane. Therefore, the development of a simple, easy-to-obtain, and permanent modification method that does not damage the filter membrane is a common goal in the field of membrane modification. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing a hydrophilic modified polyvinylidene fluoride filter membrane. The modified polyvinylidene fluoride filter membrane prepared by the present invention has excellent hydrophilicity.

[0006] (II) Technical solution

[0007] A method for preparing a hydrophilic modified polyvinylidene fluoride filter membrane, the preparation method comprising:

[0008] (1) Adding the polyvinylidene fluoride filter membrane to a 5-10 mol / L sodium hydroxide solution, stirring at 70-85° C. for 6-10 h, cooling to room temperature, washing with deionized water, and drying to obtain an alkali-treated polyvinylidene fluoride filter membrane.

[0009] (2) Adding a hydrophilic monomer and a cross-linking agent to an isopropanol solvent, stirring and dispersing, adding the alkali-treated polyvinylidene fluoride filter membrane thereto, soaking for 2-10 minutes, adding ammonium persulfate thereto at 60-90° C., reacting for 1-10 minutes, cooling to room temperature after the reaction, washing with deionized water, and drying to obtain a hydrophilically modified polyvinylidene fluoride filter membrane.

[0010] Preferably, in step (2), the hydrophilic monomer is one or more of triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and a modified vinyl quaternary ammonium salt intermediate.

[0011] Preferably, in step (2), the cross-linking agent is ethylene glycol dimethacrylate.

[0012] Preferably, in step (2), the mass fraction of the hydrophilic monomer is 0.1-5%, the mass fraction of the cross-linking agent is 0.1-5%, and the mass fraction of ammonium persulfate is 5-20%.

[0013] Preferably, in step (2), the preparation method of the hydrophilic monomer modified vinyl quaternary ammonium salt intermediate is:

[0014] S1. Add ethylenediamine to deionized water, stir and disperse, add 5-chlorovaleric acid thereto, stir and disperse, then add 10-20% sodium hydroxide solution thereto to adjust the pH to 9-10, stir and react at 75-90°C for 2-5h, after the reaction is completed, distill under reduced pressure and dry to obtain intermediate 1.

[0015] S2. Add intermediate 1 to methanol solvent, stir and disperse, then add 1,3-propane sultone thereto, stir and react at 60-75°C for 30-48 hours, after the reaction is completed, add sodium carbonate thereto, stir and react for 2-4 hours, after the reaction is completed, filter, distill under reduced pressure, and dry to obtain intermediate 2.

[0016] S3. Add intermediate 2 to n-butanol solvent, stir and disperse, then add 3-chloropropylene, raise the temperature to 65-80°C, stir and react for 1-4 hours, after the reaction is completed, distill under reduced pressure, wash with ether, and dry to obtain a modified vinyl quaternary ammonium salt intermediate.

[0017] Preferably, in step S1, the molar ratio of ethylenediamine to 5-chlorovaleric acid is 1:2-2.5.

[0018] Preferably, in step S2, the molar ratio of the intermediate 1, 1,3-propane sultone and sodium carbonate is 1:2-3:2-2.5.

[0019] Preferably, in step S3, the molar ratio of the intermediate 2,3-chloropropylene is 1:(2-2.5).

[0020] (III) Beneficial technical effects

[0021] The invention uses ethylenediamine, 5-chlorovaleric acid, 1,3-propane sultone, 3-chloropropylene and the like as raw materials, and obtains a modified vinyl quaternary ammonium salt intermediate through reaction, and then obtains a hydrophilic modified polyvinylidene fluoride filter membrane through graft polymerization with an alkalized polyvinylidene fluoride filter membrane and the like under the initiation of ammonium persulfate.

[0022] The modified polyvinylidene fluoride filter membrane prepared by the present invention contains more sulfonic acid groups and carboxyl groups, both of which have good hydrophilic effect on water molecules, and the modified vinyl quaternary ammonium salt intermediate prepared by the present invention contains a diene structure, which can be grafted and copolymerized with the alkalized polyvinylidene fluoride filter membrane to form a cross-linked network structure, which can hinder the action of water molecules and has a relatively excellent water retention effect, thereby improving the hydrophilic performance of the modified polyvinylidene fluoride filter membrane. In addition, the modified polyvinylidene fluoride filter membrane prepared by the present invention contains a quaternary ammonium salt structure, and when bacteria are contained on the filter membrane, the bacteria can kill the bacteria, thereby achieving a good sterilization effect.

[0023] The modified vinyl quaternary ammonium salt intermediate prepared by the present invention has a novel structure and a simple preparation process. In addition, the present invention adopts a simple and easily available modification scheme to graft a hydrophilic monomer on a polyvinylidene fluoride filter membrane, and graft a layer of hydrophilic substances on the microstructure surface of the membrane material, so that the filter membrane is permanently hydrophilic, and the hydrophilic substances will not be dissolved and released. The modified polyvinylidene fluoride filter membrane prepared by the present invention has an excellent hydrophilic effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a preparation route for modified vinyl quaternary ammonium salt intermediates. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with the accompanying drawings. The technical solution of the present invention is not limited to the specific implementations listed below, but also includes any combination of the specific implementations.

[0026] Preparation method of polyvinylidene fluoride filter membrane: dissolve PVDF powder in N, N-dimethylacetamide solvent, stir at 70°C for 5 hours, pour the mixed solution on a flat glass plate after stirring to form a wet film, immerse in 50% N, N-dimethylacetamide aqueous solution for 10 minutes, wash with deionized water after immersion, and dry to obtain a PVDF filter membrane.

[0027] Example 1

[0028] (1) 0.2 mol of ethylenediamine was added to deionized water and stirred for dispersion. 0.4 mol of 5-chlorovaleric acid was added thereto and stirred for dispersion. A 20% sodium hydroxide solution was then added thereto to adjust the pH to 10. The reaction was stirred at 75° C. for 4 h. After the reaction was completed, the reaction was carried out by vacuum distillation and drying to obtain intermediate 1.

[0029] (2) 0.1 mol of intermediate 1 was added to methanol solvent, stirred and dispersed, and then 0.25 mol of 1,3-propane sultone was added thereto. The mixture was stirred and reacted at 6°C for 48 hours. After the reaction was completed, 0.225 mol of sodium carbonate was added thereto. The mixture was stirred and reacted for 3 hours. After the reaction was completed, the mixture was filtered, distilled under reduced pressure, and dried to obtain intermediate 2.

[0030] (3) 0.1 mol of intermediate 2 was added to n-butanol solvent, stirred and dispersed, and then 0.2 mol of 3-chloropropylene was added thereto. The temperature was raised to 70° C. and stirred for reaction for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain a modified vinyl quaternary ammonium salt intermediate.

[0031] (4) Add the polyvinylidene fluoride filter membrane to an 8 mol / L sodium hydroxide solution, stir at 85° C. for 8 h, cool to room temperature, wash with deionized water, and dry to obtain an alkali-treated polyvinylidene fluoride filter membrane.

[0032] (5) Adding a hydrophilic monomer modified vinyl quaternary ammonium salt intermediate and a cross-linking agent ethylene glycol dimethacrylate to an isopropanol solvent and stirring to disperse, wherein the mass fraction of the hydrophilic monomer is 0.1% and the mass fraction of the cross-linking agent is 6%, then adding an alkali-treated polyvinylidene fluoride filter membrane thereto and soaking for 8 minutes, adding ammonium persulfate thereto at 80° C., wherein the mass fraction of the ammonium persulfate is 6%, reacting for 5 minutes, cooling to room temperature after the reaction is completed, washing with deionized water, and drying to obtain a hydrophilically modified polyvinylidene fluoride filter membrane.

[0033] Example 2

[0034] (1) 0.2 mol of ethylenediamine was added to deionized water and stirred for dispersion. 0.5 mol of 5-chlorovaleric acid was added thereto and stirred for dispersion. A 15% sodium hydroxide solution was then added thereto to adjust the pH to 10. The reaction was stirred at 80° C. for 5 h. After the reaction was completed, the reaction was carried out by vacuum distillation and drying to obtain an intermediate 1.

[0035] (2) 0.1 mol of intermediate 1 was added to methanol solvent, stirred and dispersed, and then 0.24 mol of 1,3-propane sultone was added thereto. The mixture was stirred and reacted at 75° C. for 38 hours. After the reaction was completed, 0.25 mol of sodium carbonate was added thereto. The mixture was stirred and reacted for 3 hours. After the reaction was completed, the mixture was filtered, distilled under reduced pressure, and dried to obtain intermediate 2.

[0036] (3) 0.1 mol of intermediate 2 was added to n-butanol solvent, stirred and dispersed, and then 0.24 mol of 3-chloropropylene was added thereto. The temperature was raised to 70° C. and stirred for reaction for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain a modified vinyl quaternary ammonium salt intermediate.

[0037] (4) Add the polyvinylidene fluoride filter membrane to a 6 mol / L sodium hydroxide solution, stir at 75° C. for 8 h, cool to room temperature, wash with deionized water, and dry to obtain an alkali-treated polyvinylidene fluoride filter membrane.

[0038] (5) Adding a hydrophilic monomer modified vinyl quaternary ammonium salt intermediate and a cross-linking agent ethylene glycol dimethacrylate to an isopropanol solvent and stirring to disperse, wherein the mass fraction of the hydrophilic monomer is 1% and the mass fraction of the cross-linking agent is 4%, then adding an alkali-treated polyvinylidene fluoride filter membrane thereto and soaking for 8 minutes, adding ammonium persulfate thereto at 80° C., wherein the mass fraction of the ammonium persulfate is 10%, reacting for 6 minutes, cooling to room temperature after the reaction is completed, washing with deionized water, and drying to obtain a hydrophilically modified polyvinylidene fluoride filter membrane.

[0039] Example 3

[0040] (1) 0.2 mol of ethylenediamine was added to deionized water and stirred for dispersion. 0.45 mol of 5-chlorovaleric acid was added thereto and stirred for dispersion. A 10% sodium hydroxide solution was then added thereto to adjust the pH to 9. The reaction was stirred at 90° C. for 2 h. After the reaction was completed, the reaction was carried out by vacuum distillation and drying to obtain an intermediate 1.

[0041] (2) 0.1 mol of intermediate 1 was added to methanol solvent, stirred and dispersed, and then 0.2 mol of 1,3-propane sultone was added thereto. The mixture was stirred and reacted at 75° C. for 36 hours. After the reaction was completed, 0.2 mol of sodium carbonate was added thereto. The mixture was stirred and reacted for 3 hours. After the reaction was completed, the mixture was filtered, distilled under reduced pressure, and dried to obtain intermediate 2.

[0042] (3) 0.1 mol of intermediate 2 was added to n-butanol solvent, stirred and dispersed, and then 0.25 mol of 3-chloropropylene was added thereto. The temperature was raised to 75° C. and stirred for reaction for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain a modified vinyl quaternary ammonium salt intermediate.

[0043] (4) Add the polyvinylidene fluoride filter membrane to a 6 mol / L sodium hydroxide solution, stir at 70° C. for 8 h, cool to room temperature, wash with deionized water, and dry to obtain an alkali-treated polyvinylidene fluoride filter membrane.

[0044] (5) Adding a hydrophilic monomer modified vinyl quaternary ammonium salt intermediate and a cross-linking agent ethylene glycol dimethacrylate to an isopropanol solvent and stirring to disperse, wherein the mass fraction of the hydrophilic monomer is 2% and the mass fraction of the cross-linking agent is 3%, then adding an alkali-treated polyvinylidene fluoride filter membrane and soaking for 6 minutes, adding ammonium persulfate at 60° C., wherein the mass fraction of ammonium persulfate is 20%, and reacting for 1 minute. After the reaction is completed, cooling to room temperature, washing with deionized water, and drying to obtain a hydrophilically modified polyvinylidene fluoride filter membrane.

[0045] Example 4

[0046] (1) 0.2 mol of ethylenediamine was added to deionized water and stirred for dispersion. 0.45 mol of 5-chlorovaleric acid was added thereto and stirred for dispersion. A 15% sodium hydroxide solution was then added thereto to adjust the pH to 10. The reaction was stirred at 80° C. for 4 h. After the reaction was completed, the reaction was carried out by vacuum distillation and drying to obtain an intermediate 1.

[0047] (2) 0.1 mol of intermediate 1 was added to methanol solvent, stirred and dispersed, and then 0.3 mol of 1,3-propane sultone was added thereto. The mixture was stirred and reacted at 60° C. for 48 h. After the reaction was completed, 0.25 mol of sodium carbonate was added thereto. The mixture was stirred and reacted for 4 h. After the reaction was completed, the mixture was filtered, distilled under reduced pressure, and dried to obtain intermediate 2.

[0048] (3) 0.1 mol of intermediate 2 was added to n-butanol solvent, stirred and dispersed, and then 0.22 mol of 3-chloropropylene was added thereto. The temperature was raised to 75° C. and stirred for reaction for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain a modified vinyl quaternary ammonium salt intermediate.

[0049] (4) Add the polyvinylidene fluoride filter membrane to a 5 mol / L sodium hydroxide solution, stir at 75° C. for 6 h, cool to room temperature, wash with deionized water, and dry to obtain an alkali-treated polyvinylidene fluoride filter membrane.

[0050] (5) Adding a hydrophilic monomer modified vinyl quaternary ammonium salt intermediate and a cross-linking agent ethylene glycol dimethacrylate to an isopropanol solvent and stirring to disperse, wherein the mass fraction of the hydrophilic monomer is 3.5% and the mass fraction of the cross-linking agent is 0.1%, then adding an alkali-treated polyvinylidene fluoride filter membrane thereto and soaking for 2 minutes, adding ammonium persulfate thereto at 60° C., wherein the mass fraction of the ammonium persulfate is 5%, and reacting for 10 minutes. After the reaction is completed, cooling to room temperature, washing with deionized water, and drying to obtain a hydrophilically modified polyvinylidene fluoride filter membrane.

[0051] Example 5

[0052] (1) 0.2 mol of ethylenediamine was added to deionized water and stirred for dispersion. 0.45 mol of 5-chlorovaleric acid was added thereto and stirred for dispersion. A 20% sodium hydroxide solution was then added thereto to adjust the pH to 10. The reaction was stirred at 90° C. for 5 h. After the reaction was completed, the reaction was carried out by vacuum distillation and drying to obtain an intermediate 1.

[0053] (2) 0.1 mol of intermediate 1 was added to methanol solvent, stirred and dispersed, and then 0.24 mol of 1,3-propane sultone was added thereto. The mixture was stirred and reacted at 65° C. for 30 h. After the reaction was completed, 0.22 mol of sodium carbonate was added thereto. The mixture was stirred and reacted for 2 h. After the reaction was completed, the mixture was filtered, distilled under reduced pressure, and dried to obtain intermediate 2.

[0054] (3) 0.1 mol of intermediate 2 was added to n-butanol solvent, stirred and dispersed, and then 0.24 mol of 3-chloropropylene was added thereto. The temperature was raised to 80° C. and stirred for reaction for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain a modified vinyl quaternary ammonium salt intermediate.

[0055] (4) Add the polyvinylidene fluoride filter membrane to a 10 mol / L sodium hydroxide solution, stir at 85° C. for 8 h, cool to room temperature, wash with deionized water, and dry to obtain an alkali-treated polyvinylidene fluoride filter membrane.

[0056] (5) Adding a hydrophilic monomer modified vinyl quaternary ammonium salt intermediate and a cross-linking agent ethylene glycol dimethacrylate to an isopropanol solvent and stirring to disperse the hydrophilic monomer, wherein the mass fraction of the hydrophilic monomer is 5% and the mass fraction of the cross-linking agent is 0.8%, then adding an alkali-treated polyvinylidene fluoride filter membrane thereto and soaking for 10 minutes, adding ammonium persulfate thereto at 90° C., wherein the mass fraction of the ammonium persulfate is 20%, reacting for 5 minutes, cooling to room temperature after the reaction is completed, washing with deionized water, and drying to obtain a hydrophilically modified polyvinylidene fluoride filter membrane.

[0057] Comparative Example 1

[0058] The difference between this comparative example and Example 1 is:

[0059] (5) Adding a hydrophilic monomer modified vinyl quaternary ammonium salt intermediate, triethylene glycol dimethacrylate, and a crosslinking agent ethylene glycol dimethacrylate to an isopropanol solvent, stirring and dispersing, wherein the mass fraction of the modified vinyl quaternary ammonium salt intermediate is 0.05%, the mass fraction of triethylene glycol dimethacrylate is 0.05%, and the mass fraction of the crosslinking agent is 6%, and then adding an alkali-treated polyvinylidene fluoride filter membrane thereto, soaking for 8 minutes, adding ammonium persulfate thereto at 80° C., wherein the mass fraction of the ammonium persulfate is 6%, reacting for 5 minutes, cooling to room temperature after the reaction is completed, washing with deionized water, and drying to obtain a hydrophilic modified polyvinylidene fluoride filter membrane.

[0060] Comparative Example 2

[0061] The difference between this comparative example and Example 1 is:

[0062] (5) Adding a hydrophilic monomer modified vinyl quaternary ammonium salt intermediate, tetraethylene glycol dimethacrylate, and crosslinking agent ethylene glycol dimethacrylate to an isopropanol solvent, stirring and dispersing, wherein the mass fraction of the modified vinyl quaternary ammonium salt intermediate is 0.05%, the mass fraction of tetraethylene glycol dimethacrylate is 0.05%, and the mass fraction of the crosslinking agent is 6%, and then adding an alkali-treated polyvinylidene fluoride filter membrane thereto, soaking for 8 minutes, adding ammonium persulfate thereto at 80° C., wherein the mass fraction of the ammonium persulfate is 6%, reacting for 5 minutes, cooling to room temperature after the reaction is completed, washing with deionized water, and drying to obtain a hydrophilic modified polyvinylidene fluoride filter membrane.

[0063] Comparative Example 3

[0064] The difference between this comparative example and Example 1 is:

[0065] (5) Add hydrophilic monomers triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and crosslinking agent ethylene glycol dimethacrylate to isopropanol solvent and stir to disperse, wherein the mass fraction of triethylene glycol dimethacrylate is 0.05%, the mass fraction of tetraethylene glycol dimethacrylate is 0.05%, and the mass fraction of the crosslinking agent is 6%. Then add the alkali-treated polyvinylidene fluoride filter membrane and soak for 8 minutes. Add ammonium persulfate at 80° C. and the mass fraction of ammonium persulfate is 6%. React for 5 minutes. After the reaction is completed, cool to room temperature, wash with deionized water, and dry to obtain a hydrophilic modified polyvinylidene fluoride filter membrane.

[0066] Comparative Example 4

[0067] The difference between this comparative example and Example 1 is that in step (5), no modified vinyl quaternary ammonium salt intermediate is contained.

[0068] The contact angle of the polyvinylidene fluoride filter membrane was tested using a contact angle meter.

[0069] Contact angle (°) Example 1 72.3 Example 2 68.4 Example 3 64.2 Example 4 59.2 Example 5 58.2 Comparative Example 1 76.4 Comparative Example 2 74.8 Comparative Example 3 78.1 Comparative Example 4 96.5

[0070] The smaller the contact angle, the better the hydrophilicity. As can be seen from the table, the polyvinylidene fluoride filter membrane prepared by the present invention has good hydrophilicity.

[0071] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the preparation method of the hydrophilic modified polyvinylidene fluoride filter membrane of the present invention, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a hydrophilic modified polyvinylidene fluoride filter membrane, characterized in that: The preparation method is: (1) adding the polyvinylidene fluoride filter membrane to a 5-10 mol / L sodium hydroxide solution, stirring at 70-85° C. for 6-10 hours, cooling to room temperature, washing with deionized water, and drying to obtain an alkali-treated polyvinylidene fluoride filter membrane; (2) Adding a hydrophilic monomer and a cross-linking agent to an isopropanol solvent, stirring and dispersing, then adding the alkali-treated polyvinylidene fluoride filter membrane thereto, soaking for 2-10 minutes, adding ammonium persulfate thereto at 60-90° C., reacting for 1-10 minutes, cooling to room temperature after the reaction, washing with deionized water, and drying to obtain a hydrophilically modified polyvinylidene fluoride filter membrane, wherein the preparation method of the hydrophilic monomer-modified vinyl quaternary ammonium salt intermediate is: S1, adding ethylenediamine to deionized water, stirring and dispersing, adding 5-chlorovaleric acid thereto, stirring and dispersing, and then adding 10-20% sodium hydroxide solution thereto to adjust the pH to 9-10, stirring and reacting at 75-90° C. for 2-5 hours, and after the reaction is completed, distilling under reduced pressure and drying to obtain intermediate 1; S2, adding intermediate 1 to methanol solvent, stirring and dispersing, then adding 1,3-propane sultone thereto, stirring and reacting at 60-75° C. for 30-48 hours, after the reaction is completed, adding sodium carbonate thereto, stirring and reacting for 2-4 hours, after the reaction is completed, filtering, distilling under reduced pressure, and drying to obtain intermediate 2; S3. Add intermediate 2 to n-butanol solvent, stir and disperse, then add 3-chloropropylene, raise the temperature to 65-80°C, stir and react for 1-4 hours, after the reaction is completed, distill under reduced pressure, wash with ether, and dry to obtain a modified vinyl quaternary ammonium salt intermediate.

2. The method for preparing the hydrophilic modified polyvinylidene fluoride filter membrane according to claim 1, characterized in that: In the step (2), the hydrophilic monomer further comprises one or both of triethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate.

3. The method for preparing the hydrophilic modified polyvinylidene fluoride filter membrane according to claim 1, characterized in that: In the step (2), the cross-linking agent is ethylene glycol dimethacrylate.

4. The method for preparing the hydrophilic modified polyvinylidene fluoride filter membrane according to claim 1, characterized in that: In the step (2), the mass fraction of the hydrophilic monomer is 0.1-5%, the mass fraction of the cross-linking agent is 0.1-5%, and the mass fraction of ammonium persulfate is 5-20%.

5. The method for preparing the hydrophilic modified polyvinylidene fluoride filter membrane according to claim 1, characterized in that: In the step S1, the molar ratio of ethylenediamine to 5-chlorovaleric acid is 1:2-2.

5.

6. The method for preparing the hydrophilic modified polyvinylidene fluoride filter membrane according to claim 1, characterized in that: In the step S2, the molar ratio of the intermediate 1, 1,3-propane sultone and sodium carbonate is 1:2-3:2-2.

5.

7. The method for preparing a hydrophilic modified polyvinylidene fluoride filter membrane according to claim 1, characterized in that: In the step S3, the molar ratio of the intermediate 2-chloropropylene is 1:2-2.5.