A stable dispersed nano calcium carbonate early strength agent and its preparation method and application

Through the combination of anhydrous sodium carbonate, calcium nitrate tetrahydrate, metal salts, organic acids and organic alcohol amines, the problem of nano-calcium carbonate agglomeration in aqueous solution is solved, its stable dispersion in cementitious materials is achieved, and the concrete is improved. early and late strength and durability properties.

CN118459139BActive Publication Date: 2024-10-01SHIJIAZHUANG CHANGAN YUCAI BUILDING MATERIALS +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410911439.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

Nano-calcium carbonate easily agglomerates in aqueous solution, resulting in uneven dispersion in cementitious materials and affecting the hydration efficiency and durability of cement.

Method used

Using a combination of anhydrous sodium carbonate, calcium nitrate tetrahydrate, metal salts, organic acids, organic alcohol amines and dispersants, through complex coordination and surface modification methods, the interface energy and surface free energy of nano-calcium carbonate are reduced and their surface free energy is improved. Dispersion stability in aqueous solutions.

Benefits of technology

It achieves stable dispersion of nano-calcium carbonate, improves the early and late strength of concrete, enhances the durability of cement mortar, and simplifies the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a stably dispersed nano calcium carbonate early strength agent and a preparation method and application thereof, belonging to the technical field of chemical additives for building materials, comprising the following raw materials by weight: 5 parts of anhydrous sodium carbonate, 10 parts of calcium nitrate tetrahydrate, 4-16 parts of metal salt, 1-4 parts of organic acid, 1-8 parts of organic alcohol amine, 6-12 parts of dispersant and 400-500 parts of water. Its preparation method comprises the following steps: adding metal salt and organic alcohol amine to an organic acid solution and fully stirring and dispersing, then adding a dispersant and calcium nitrate tetrahydrate and continuing to stir and disperse, and then dropping a sodium carbonate solution to obtain the nano calcium carbonate early strength agent. The present invention solves the problem of rapid agglomeration of nano calcium carbonate in an aqueous solution, so that calcium carbonate can be used in a cementitious material at a nanometer scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical additives for building materials, and in particular relates to a stably dispersed nano calcium carbonate early strength agent and a preparation method and application thereof. Background Art

[0002] One of the priority areas of modern construction production is the introduction of high-performance high-speed concrete with improved technical and construction technology properties for the design, installation and repair of engineering structures and structures of residential, public and industrial buildings, in order to ensure the commissioning of operational objects and their reliable operation throughout their life cycle. In the early and design stages of innovative structural materials, the high performance and durability of concrete mixes determine their technical efficiency.

[0003] Since the beginning of this century, with the growing demand for ultra-high performance concrete, the application of nanotechnology in concrete has begun. Nanomaterials have important effects on the physical and chemical properties and microstructure of cement-based materials due to their characteristics such as micro-aggregate effect and nucleation effect. When nano calcium carbonate is introduced into concrete, it can react with tricalcium aluminate to form hydrated calcium carbonate aluminate, providing nucleation sites for CSH, accelerating the hydration rate of cement, shortening the cement setting time and rapidly improving the early strength. It is a nanomaterial with more potential in cement than nano CSH. In addition, nano calcium carbonate can produce higher density concrete by refining the intersection area of ​​cement, thereby achieving excellent filling effect and improving the durability of concrete.

[0004] Although the application of nano calcium carbonate in cement brings many advantages, it also has some limitations. First, the dispersion of nano calcium carbonate is an important challenge. Due to its ultra-high surface energy and chemical activity, nano calcium carbonate is prone to agglomeration. This makes it difficult to completely fill the pores of cement-based materials at the nanoscale in practical applications. The agglomeration phenomenon not only reduces the actual surface area of ​​nano calcium carbonate, but also reduces its Ca 2+ The physical and chemical adsorption of C3S particles affects the Ca 2+ The concentration of nano-calcium carbonate further slows down the hydration process of C3S, thus affecting the hydration efficiency of cement. At present, the research on the effect of nano-calcium carbonate on the chemical properties and microstructure of cement-based materials is relatively limited. The main reason is that the high surface energy of nano-CaCO3 makes nano-CaCO3 agglomerate rapidly in aqueous solution, which limits its application in cementitious materials.

[0005] Therefore, how to provide a nano-calcium carbonate that can be stably dispersed in an aqueous solution is a technical problem that those skilled in the art need to solve urgently. Summary of the invention

[0006] In order to solve the above technical problems, the present invention proposes a stably dispersed nano calcium carbonate early strength agent and a preparation method and application thereof.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A stably dispersed nano calcium carbonate early strength agent comprises the following raw materials in parts by weight:

[0009] 5 parts of anhydrous sodium carbonate, 10 parts of calcium nitrate tetrahydrate, 4-16 parts of metal salt, 1-4 parts of organic acid, 1-8 parts of organic alcohol amine, 6-12 parts of dispersant and 400-500 parts of water.

[0010] Beneficial effect: The dispersant in the present invention is Ca in aqueous solution. 2+ Providing adsorption sites and steric hindrance, organic alcohol amines are used as surface modification methods to weaken the surface free energy of nano-calcium carbonate. Metal salts and organic acids work synergistically to reduce the interfacial energy of nano-calcium carbonate through complexation and coordination, while increasing the absolute value of the surface Zeta potential, thereby achieving the goal of improving the dispersion degree and dispersion stability of nano-calcium carbonate.

[0011] Preferably, the metal salt is magnesium chloride and / or aluminum nitrate.

[0012] More preferably, the aluminum nitrate is aluminum nitrate tetrahydrate.

[0013] Beneficial effects: The aluminum ions and magnesium ions in the present invention can coordinate with organic acids to produce positively charged complexes, which selectively chemically adsorb CO3 on the surface of calcite in the form of single hydrogen free radicals. 2- sites, causing the zeta potential on its surface to change positively, inhibiting the aggregation of nano-calcium carbonate.

[0014] Preferably, the organic acid is citric acid and / or lactic acid.

[0015] Beneficial effects: The organic acid in the present invention acts on the surface of nano-calcium carbonate particles through the functional groups (such as carboxyl) in its molecules, and the lone pair of electrons on the oxygen atom in the carboxyl group forms a coordination bond with the calcium ion to form an organic adsorption layer. This adsorption layer reduces the surface energy of the nano-calcium carbonate particles and reduces the tendency of agglomeration between the particles, thereby improving the dispersibility of the nano-calcium carbonate.

[0016] Preferably, the organic alcohol amine is diethanolamine and / or triethanolamine.

[0017] Beneficial effects: The organic alcohol amine in the present invention interacts with the surface of nano-calcium carbonate through its polar functional groups (hydroxyl and amino groups), such as hydrogen bonding and electrostatic interaction. This interaction can change the charge distribution and surface energy of the surface of nano-calcium carbonate, thereby facilitating its dispersion and stability in the solution. However, different alcohol amines, reaction conditions, and dosages can also lead to the formation of calcium carbonate with different morphologies.

[0018] Preferably, the dispersant is polycarboxylate water reducer D4.

[0019] Beneficial effects: The carboxylic acid groups in the polycarboxylic acid molecules of the present invention can be adsorbed on the surface of nano-calcium carbonate particles to form a protective film. This adsorption changes the charge distribution and surface energy on the surface of the nano-calcium carbonate particles, making them easier to disperse in aqueous solution. The polycarboxylic acid molecular chains stretch in the aqueous solution to form a certain steric hindrance, which can prevent the agglomeration of the nano-calcium carbonate particles and keep them in a dispersed state. The calcium carbonate generated by the reaction of calcium nitrate tetrahydrate and anhydrous sodium carbonate in the present invention is widely used in the construction industry, and has the advantages of low output and cost, good safety, environmental protection, and mild and easy-to-control reaction conditions.

[0020] A method for preparing a stably dispersed nano calcium carbonate early strength agent comprises the following steps:

[0021] The nano calcium carbonate early strength agent is obtained by adding metal salt and organic alcohol amine to the organic acid solution, stirring and dispersing them fully, then adding dispersant and calcium nitrate tetrahydrate and continuing to stir and disperse them, and then dropping sodium carbonate solution.

[0022] Beneficial effects: The metal salt and calcium nitrate tetrahydrate used in the present invention are both strong acid and weak base salts, and step-by-step addition can better avoid the generation of metal hydroxides due to pH adjustment, which affects the reaction process.

[0023] Preferably, the organic acid solution is obtained by mixing an organic acid with a portion of water;

[0024] The sodium carbonate solution is obtained by mixing anhydrous sodium carbonate with residual water.

[0025] Beneficial effect: Since the process conditions in the present invention require the pH value to be regulated, in order to avoid the generation of metal hydroxides that affect the reaction when sodium hydroxide solution is added to adjust the pH due to the solution being too acidic before dropwise addition, the pH of the organic acid solution needs to be adjusted to 7-8.

[0026] Preferably, the stirring and dispersing is performed at a rotation speed of 3000-8000 rpm and for a time of 10-30 min.

[0027] Preferably, the step of continuing the stirring and dispersing further comprises adjusting the pH, wherein the pH is adjusted to 7-8 using a sodium hydroxide solution;

[0028] More preferably, the mass concentration of the sodium hydroxide solution is 30%.

[0029] Beneficial effects: Under neutral conditions (i.e. pH value of about 7), the complex formed by citric acid and calcium carbonate has high stability. This is because in a neutral environment, the charge balance state of citrate ions and calcium ions is relatively stable and is not easily affected by external factors (such as acidity or alkalinity).

[0030] During the process of adding the sodium carbonate solution, the pH value is adjusted to 7-8 by using the hydrochloric acid solution;

[0031] More preferably, the mass concentration of the hydrochloric acid solution is 30%.

[0032] Beneficial effects: The sodium carbonate aqueous solution in the present invention is alkaline. To ensure that its pH is 7-8, a hydrochloric acid solution is used to control the pH value of the sodium carbonate aqueous solution during the dropwise addition process.

[0033] Application of a stably dispersed nano calcium carbonate early strength agent in building materials.

[0034] Beneficial effects: The nano calcium carbonate early strength agent in the present invention has a particle size of less than 100nm, and only one thousandth of the proportion of the adhesive can quickly improve the early strength of cement mortar, and also improve the late strength of cement mortar. It can react with tricalcium aluminate to generate hydrated calcium carbonate aluminate, and provide nucleation sites for CSH, accelerate cement hydration, shorten cement setting time and quickly improve early strength.

[0035] Compared with the prior art, the present invention has the following advantages and technical effects:

[0036] The present invention provides a stably dispersed nano calcium carbonate early strength agent and a preparation method and application thereof, which solves the problem of rapid agglomeration of nano calcium carbonate in aqueous solution, enables calcium carbonate to be applied in cementitious materials at a nanometer scale, realizes the application of nano calcium carbonate in concrete at a nanometer scale, not only realizes the purpose of rapid strength development of concrete within hours, but also greatly improves the late strength of concrete. At the same time, the present invention provides a preparation method for the study of the influence of nano calcium carbonate on the hydration degree of minerals in cement and the chemical properties and microstructure of cement-based materials, which can be quantified by specific data. Finally, the production raw material types of the nano calcium carbonate early strength agent provided by the present invention are small, the preparation process is simple, and the required production equipment is small, which is convenient for popularization and application. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods.

[0039] The embodiment of the present invention provides a stably dispersed nano calcium carbonate early strength agent, comprising the following raw materials in parts by weight:

[0040] 5 parts of anhydrous sodium carbonate, 10 parts of calcium nitrate tetrahydrate, 4-16 parts of metal salt, 1-4 parts of organic acid, 1-8 parts of organic alcohol amine, 6-12 parts of dispersant and 400-500 parts of water.

[0041] In a preferred embodiment, the metal salt is magnesium chloride and / or aluminum nitrate.

[0042] In a more preferred embodiment, the aluminum nitrate is aluminum nitrate nonahydrate.

[0043] In a preferred embodiment, the organic acid is citric acid and / or lactic acid.

[0044] In a preferred embodiment, the organic alcohol amine is diethanolamine and / or triethanolamine.

[0045] In a preferred embodiment, the dispersant is polycarboxylate water reducer D4.

[0046] The embodiment of the present invention also provides a method for preparing a stably dispersed nano calcium carbonate early strength agent, comprising the following steps:

[0047] The nano calcium carbonate early strength agent is obtained by adding metal salt and organic alcohol amine to the organic acid solution, stirring and dispersing them fully, then adding dispersant and calcium nitrate tetrahydrate and continuing to stir and disperse them, and then dropping sodium carbonate solution.

[0048] In a preferred embodiment, the organic acid solution is obtained by mixing an organic acid with a portion of water;

[0049] The sodium carbonate solution is obtained by mixing anhydrous sodium carbonate with residual water.

[0050] In a preferred embodiment, the stirring and dispersing is performed at a speed of 3000-8000 rpm and for a time of 10-30 min.

[0051] In a preferred embodiment, the stirring and dispersing and the continuing stirring and dispersing both further include adjusting the pH, wherein the pH is adjusted to 7-8 using a sodium hydroxide solution;

[0052] In a more preferred embodiment, the mass concentration of the sodium hydroxide solution is 30%.

[0053] During the process of adding the sodium carbonate solution, the pH value is adjusted to 7-8 by using the hydrochloric acid solution;

[0054] In a more preferred embodiment, the mass concentration of the hydrochloric acid solution is 30%.

[0055] The embodiment of the present invention also provides an application of a stably dispersed nano calcium carbonate early strength agent in building materials.

[0056] The raw materials in the embodiments of the present invention are all purchased from commercial sources;

[0057] Among them, the mass concentration of sodium hydroxide solution is 30%, and the mass concentration of hydrochloric acid solution is 30%.

[0058] Unless otherwise specified, "parts" in the embodiments of the present invention refer to parts by weight.

[0059] Example 1

[0060] A method for preparing a stably dispersed nano calcium carbonate early strength agent comprises the following steps:

[0061] (1) Add 400 parts of deionized water and 2 parts of citric acid to a 2L stainless steel stirring vessel. After fully dissolving, adjust the pH to 7 with sodium hydroxide solution to obtain an organic acid solution. Then add 4 parts of aluminum nitrate nonahydrate and 2 parts of diethanolamine, start a high-speed disperser, and stir and disperse for 10 minutes at a speed of 5000 rpm to obtain a first dispersion;

[0062] (2) Add 10 parts of polycarboxylate water-reducing agent D4 as a dispersant to the first dispersion, and then add 10 parts of calcium nitrate tetrahydrate. After fully dissolving, adjust the pH to 7 with sodium hydroxide solution, start the high-speed disperser, and continue stirring and dispersing at a speed of 5000 rpm for 10 minutes to obtain a second dispersion;

[0063] (3) Dissolve 5 parts of anhydrous sodium carbonate in 100 parts of deionized water to obtain a sodium carbonate solution, and add the solution dropwise to the second dispersion obtained in step (2) at a dropping rate of 300 g / h. In addition, during the dropping process, a hydrochloric acid solution is used to maintain the pH value of the dispersion at 8. After the reaction is completed, a stably dispersed nano-calcium carbonate early strength agent is obtained.

[0064] Example 2

[0065] A method for preparing a stably dispersed nano calcium carbonate early strength agent comprises the following steps:

[0066] (1) Add 400 parts of deionized water and 4 parts of citric acid to a 2L stainless steel stirring vessel. After fully dissolving, adjust the pH to 7 with sodium hydroxide solution to obtain an organic acid solution. Then add 8 parts of aluminum nitrate nonahydrate and 4 parts of diethanolamine, start a high-speed disperser, and stir and disperse at a speed of 5000 rpm for 10 minutes to obtain a first dispersion;

[0067] (2) Add 10 parts of polycarboxylate water-reducing agent D4 as a dispersant to the first dispersion, and then add 10 parts of calcium nitrate tetrahydrate. After fully dissolving, adjust the pH to 7 with sodium hydroxide solution, start the high-speed disperser, and continue stirring and dispersing at a speed of 5000 rpm for 10 minutes to obtain a second dispersion;

[0068] (3) Dissolve 5 parts of anhydrous sodium carbonate in 100 parts of deionized water to obtain a sodium carbonate solution, and add the solution dropwise to the second dispersion obtained in step (2) at a dropping rate of 300 g / h. In addition, during the dropping process, a hydrochloric acid solution is used to maintain the pH value of the dispersion at 8. After the reaction is completed, a stably dispersed nano-calcium carbonate early strength agent is obtained.

[0069] Example 3

[0070] A method for preparing a stably dispersed nano calcium carbonate early strength agent comprises the following steps:

[0071] (1) Add 350 parts of deionized water and 4 parts of citric acid to a 2 L stainless steel stirring vessel. After fully dissolving, adjust the pH to 7 with a sodium hydroxide solution, then add 8 parts of aluminum nitrate nonahydrate and 4 parts of diethanolamine, start a high-speed disperser, and stir and disperse for 10 minutes at a speed of 5000 rpm to obtain a first dispersion;

[0072] (2) Add 12 parts of polycarboxylate water-reducing agent D4 as a dispersant to the first dispersion, and then add 10 parts of calcium nitrate tetrahydrate. After fully dissolving, adjust the pH to 7 with sodium hydroxide solution, start the high-speed disperser, and continue stirring and dispersing at a speed of 5000 rpm for 10 minutes to obtain a second dispersion;

[0073] (3) Dissolve 5 parts of anhydrous sodium carbonate in 150 parts of deionized water to obtain a sodium carbonate solution, and add the solution dropwise to the second dispersion obtained in step (2) at a dropping rate of 450 g / h. In addition, during the dropping process, a hydrochloric acid solution is used to maintain the pH value of the dispersion at 8. After the reaction is completed, a stably dispersed nano-calcium carbonate early strength agent is obtained.

[0074] Example 4

[0075] A method for preparing a stably dispersed nano calcium carbonate early strength agent comprises the following steps:

[0076] (1) Add 400 parts of deionized water and 2 parts of organic acid (citric acid and lactic acid mixed in a mass ratio of 2:1) to a 2L stainless steel stirring vessel. After fully dissolved, adjust the pH to 7 with sodium hydroxide solution to obtain an organic acid solution. Then add 4 parts of aluminum nitrate nonahydrate and 2 parts of organic alcohol amine (triethanolamine and diethanolamine mixed in a mass ratio of 2:1), start the high-speed disperser, and stir and disperse for 10 minutes at a speed of 5000 rpm to obtain a first dispersion;

[0077] (2) Add 6 parts of polycarboxylate water-reducing agent D4 as a dispersant to the first dispersion, and then add 10 parts of calcium nitrate tetrahydrate. After fully dissolving, adjust the pH to 7 with sodium hydroxide solution, start the high-speed disperser, and continue stirring and dispersing at a speed of 3000 rpm for 10 minutes to obtain a second dispersion;

[0078] (3) Dissolve 5 parts of anhydrous sodium carbonate in 100 parts of deionized water to obtain a sodium carbonate solution, and add the solution dropwise to the second dispersion obtained in step (2) at a dropping rate of 300 g / h. In addition, during the dropping process, a hydrochloric acid solution is used to maintain the pH value of the dispersion at 8. After the reaction is completed, a stably dispersed nano-calcium carbonate early strength agent is obtained.

[0079] Comparative Example 1

[0080] A method for preparing a nano calcium carbonate early strength agent comprises the following steps:

[0081] (1) Add 400 parts of deionized water, 10 parts of polycarboxylate water-reducing agent D4 as a dispersant and 10 parts of calcium nitrate tetrahydrate to a 2L stainless steel stirring vessel. After fully dissolving, adjust the pH to 7 with sodium hydroxide solution, turn on the high-speed disperser, and stir and disperse at a speed of 5000 rpm for 10 minutes.

[0082] (2) Dissolve 5 parts of anhydrous sodium carbonate in 100 parts of deionized water to obtain a sodium carbonate solution, and add the solution dropwise to the solution obtained in step (1) at a dropping rate of 300 g / h. After the reaction is completed, a nano calcium carbonate early strength agent is obtained.

[0083] Comparative Example 2

[0084] A method for preparing a nano calcium carbonate early strength agent, which differs from Example 1 only in that hydrochloric acid solution is not used to adjust the pH value in step (3), and other process steps and parameters are the same as those in Example 1.

[0085] Comparative Example 3

[0086] A method for preparing a nano calcium carbonate early strength agent, which differs from Example 1 only in that diethanolamine is not added in step (1), and the other process steps and parameters are the same as those in Example 1.

[0087] Comparative Example 4

[0088] A method for preparing a nano calcium carbonate early strength agent, which differs from Example 1 only in that aluminum nitrate nonahydrate is not added in step (1), and other process steps and parameters are the same as those in Example 1.

[0089] Technical effects:

[0090] 1. The nano calcium carbonate early strength agents of Examples 1-4 and Comparative Examples 1-4 were subjected to particle size analysis and stability analysis. The results are shown in Table 1.

[0091] Table 1 Particle size and stability of highly dispersed nano calcium carbonate

[0092]

[0093] It can be seen that the particle sizes of the nano calcium carbonate in Examples 1-4 are all controlled below 100 nm, and the dispersion in water is relatively stable.

[0094] 2. According to the "Test Method for Strength of Cement Mortar" GB / T 17671-2021, the nano calcium carbonate early strength agent obtained in Examples 1-4 and Comparative Examples 1-4 was added as an additive to cement mortar, and cubic test blocks were prepared. The blocks were cured for 8h, 1d and 28d under standard curing conditions, and the mechanical properties were tested.

[0095] The cement mortar formula is: 900g cement, 1350g sand, 234g water, 90g nano calcium carbonate early strength agent, and 72g accelerator. The accelerator model is GK-3B (see patent application CN 202110916790.8 for detailed preparation method).

[0096] Table 2 shows the mechanical property test results of cement mortar test blocks prepared using the nano calcium carbonate early strength agent obtained in Examples 1-4 and Comparative Examples 1-4.

[0097] Among them, the only difference between the blank group and the above-mentioned cement mortar formula is that the nano calcium carbonate early strength agent is not included, and the other raw materials, addition amounts and preparation methods are the same as those of the above-mentioned cement mortar.

[0098] Table 2 Mechanical properties test of cement mortar

[0099]

[0100] It can be seen from Table 2 that, under the condition that the proportion of nano-calcium carbonate obtained in Examples 1-4 and Comparative Examples 1-4 to the adhesive material is consistent, which is 0.1%wt, the 8h, 1d and 28d strengths of Example 1 are about 38%, 36% and 12% higher than those of the blank group, respectively; the 8h, 1d and 28d strengths of Example 2 are about 72%, 39% and 14% higher than those of the blank group, respectively; the 8h, 1d and 28d strengths of Example 3 are about 78%, 45% and 19% higher than those of the blank group, respectively. The smaller the particle size of the nano-calcium carbonate, the more obvious the improvement in mortar strength. This is because the micro-aggregate effect and crystal nucleus effect of nano-calcium carbonate have a significant effect on the early strength improvement, and its unique chemical effect runs through the cement hydration cycle, and is also obvious to the later strength improvement. However, compared with the blank group, the comparative example 1 had a negative impact on the 8h and 1d strengths. Compared with the blank group, the comparative examples 2, 3 and 4 had improved 8h strengths, but the 1d strength and 28d strengths were not much different from the benchmark, indicating that the agglomeration of nano-calcium carbonate not only reduced the actual surface area of ​​nano-calcium carbonate, but also reduced its 2+ The physical and chemical adsorption of C3S particles affects the Ca 2+ The concentration further slows down the hydration process of C3S, thus affecting the hydration efficiency of cement. The nano calcium carbonate in the early strength agent accounts for 0.1%wt of the adhesive material, which has a significant early strength effect and a permanent effect of improving the later strength.

[0101] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A stably dispersed nano calcium carbonate early strength agent, characterized in that: The invention comprises the following raw materials in parts by weight: 5 parts of anhydrous sodium carbonate, 10 parts of calcium nitrate tetrahydrate, 4-16 parts of metal salt, 1-4 parts of organic acid, 1-8 parts of organic alcohol amine, 6-12 parts of dispersant and 400-500 parts of water; The metal salt is magnesium chloride and / or aluminum nitrate; The organic acid is citric acid and / or lactic acid; The preparation method of the stably dispersed nano calcium carbonate early strength agent comprises the following steps: Add metal salt and organic alcohol amine to the organic acid solution, stir and disperse them thoroughly, then add dispersant and calcium nitrate tetrahydrate, continue to stir and disperse, and then drop sodium carbonate solution to obtain the nano calcium carbonate early strength agent; The step of continuing to stir and disperse further includes adjusting the pH, wherein the pH is adjusted to 7-8 using a sodium hydroxide solution; During the process of adding the sodium carbonate solution, the pH value is adjusted to 7-8 by using the hydrochloric acid solution.

2. A stably dispersed nano calcium carbonate early strength agent according to claim 1, characterized in that: The organic alcohol amine is diethanolamine and / or triethanolamine.

3. A stably dispersed nano calcium carbonate early strength agent according to claim 1, characterized in that: The dispersant is polycarboxylate water reducer D4.

4. A method for preparing a stably dispersed nano calcium carbonate early strength agent as described in any one of claims 1 to 3, characterized in that: The following steps are involved: The nano calcium carbonate early strength agent is obtained by adding metal salt and organic alcohol amine to the organic acid solution, stirring and dispersing them fully, then adding dispersant and calcium nitrate tetrahydrate and continuing to stir and disperse them, and then dropping sodium carbonate solution.

5. The method for preparing a stably dispersed nano calcium carbonate early strength agent according to claim 4, characterized in that: The organic acid solution is obtained by mixing an organic acid with a portion of water; The sodium carbonate solution is obtained by mixing anhydrous sodium carbonate with residual water.

6. The method for preparing a stably dispersed nano calcium carbonate early strength agent according to claim 4, characterized in that: The rotation speed of the stirring and dispersing is 3000-8000 rpm, and the time is 10-30 min.