Elastomer toughened modified polycarbonate and preparation method
By introducing carbonate-based polyurethane elastomer into polycarbonate, the similar compatibility between the polyether flexible soft segment and the bisphenol A carbonate hard segment is used to form an alloy-like phase, which solves the insufficient toughness and heat resistance of polycarbonate. The problem of high toughness and heat resistance has been improved.
Patent Information
- Application Number
- CN202410921757.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Polycarbonate has poor toughness and poor heat resistance, which cannot meet the higher requirements for material performance in industrial manufacturing.
Carbonate-based polyurethane elastomer is used as toughening agent to prepare carbonate-based polyurethane with high toughness and heat resistance by reacting with polyether polyol, isophorone diisocyanate and naphthyl carbonate chain extender The elastomer is formed through a combined process of a twin-screw extruder and an injection molding machine to form an elastomer toughened modified polycarbonate.
It significantly improves the toughness, elasticity and heat resistance of polycarbonate, with elongation of break reaching 94.5-139.4%, impact strength reaches 68.5-95.1kJ/m2, bending strength reaches 88.3-107.0MPa, and improves the thermal decomposition of the material. temperature.
Smart Images

Figure CN118459965B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polycarbonate, in particular to an elastomer toughened and modified polycarbonate and a preparation method thereof. Background Art
[0002] Polycarbonate PC has excellent flame retardancy, good wear resistance, and high mechanical properties. It is widely used in glass assembly, automobile industry, electronic and electrical industries. With the rapid development of industry, traditional polycarbonate can no longer meet the needs of industrial manufacturing, and higher requirements are placed on the toughness, strength, heat resistance and other properties of polycarbonate. The use of rubber elastomers, plastics, nanomaterials, etc. to toughen polycarbonate is a research hotspot.
[0003] Materials such as polyurethane plastics and elastomers have excellent elasticity, toughness and strength, and the preparation method is simple, the cost is low, and the application is very wide. Chinese patent CN111205616B discloses a halogen-free flame-retardant polycarbonate alloy resistant to hot and cold alternation and its preparation method, using polycarbonate, modified polyurethane, polysiloxane-polycarbonate copolymer as raw materials, and silicon-containing core-shell structure acrylic polymer as toughening agent. The obtained polycarbonate alloy has good cold resistance, heat resistance, flame retardancy and other properties. However, the raw materials of this patent are relatively complex, and raw materials such as polysiloxane-polycarbonate copolymer and silicon-containing core-shell structure acrylic polymer need to be added, and the toughening effect on polycarbonate materials is not good. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] The invention solves the problems of poor toughness and poor heat resistance of polycarbonate.
[0006] (II) Technical solution
[0007] An elastomer toughened and modified polycarbonate comprises the following raw materials: 65-90 parts by weight of polycarbonate, 10-35 parts by weight of carbonate-based polyurethane elastomer, and 0.2-0.5 parts by weight of antioxidant.
[0008] The preparation method of carbonate-based polyurethane elastomer is:
[0009] Add polyether polyol into a flask, vacuum dehydrate, then add isophorone diisocyanate, heat to 60-70°C, react for 3-4h, then add naphthyl carbonate chain extender and dibutyltin dilaurate, quickly stir and mix for 40-50s, then pour into a preheated mold, and perform aging treatment after reaching the gel point to obtain a carbonate-based polyurethane elastomer.
[0010] The structural formula of naphthyl carbonate chain extender is as follows:
[0011] .
[0012] Furthermore, the molar ratio of polyether polyol, isophorone diisocyanate and naphthyl carbonate chain extender is 1:(2.5-2.8):(1.1-1.3); the polyether polyol includes polyethylene glycol and / or polypropylene glycol.
[0013] Furthermore, the aging treatment is first performed at 110-120°C for 12-24 hours and then at 20-30°C for 5-7 days.
[0014] Further, the preparation method of the naphthyl carbonate chain extender is:
[0015] (1) Place a flask in an ice bath, add dichloromethane, bisphenol A, pyridine, and p-bromophenyl chloroformate, and stir at 15-25°C for 4-10 hours. After filtering, rotary evaporate the filtrate, and separate it by chromatography to obtain bisphenol A carbonate bromobenzene monomer.
[0016] (2) Add N,N-dimethylformamide, bisphenol A carbonate bromobenzene monomer, 6-hydroxynaphthalene-2-boric acid, (1,1'-bis(diphenylphosphino)ferrocene) palladium dichloride, potassium carbonate and deionized water into a flask, stir and react at 110-130°C for 12-18h, add ethyl acetate and deionized water, mix well and allow to stand to separate, separate the dehydrated phase, dry the ethyl acetate organic phase to remove water, rotary evaporate, and separate by chromatography to obtain a naphthyl carbonate chain extender.
[0017] Furthermore, the molar ratio of bisphenol A, pyridine and p-bromochlorophenylformate in (1) is 1:(2-2.2):(2-2.2).
[0018] Furthermore, in (2), the molar ratio of bisphenol A carbonate bromobenzene monomer, 6-hydroxynaphthalene-2-boric acid, (1,1'-bis(diphenylphosphino)ferrocene)palladium dichloride, and potassium carbonate is 1:(2.3-2.6):(0.044-0.058):(3.4-4.2).
[0019] Furthermore, the preparation method of the elastomer toughened modified polycarbonate is to place the polycarbonate, carbonate-based polyurethane elastomer, and antioxidant in a mixer and mix them evenly, then extrude and granulate them in a twin-screw extruder, the temperature of zones 1-6 is 210-260°C, and finally injection mold them in an injection molding machine, the injection molding pressure is 80-90MPa, and the temperature is 270-280°C to obtain the elastomer toughened modified polycarbonate.
[0020] (III) Beneficial technical effects: The present invention utilizes bisphenol A to react with phenyl p-bromochloroformate and 6-hydroxynaphthalene-2-boric acid in sequence to obtain a novel naphthyl carbonate chain extender; and then polymerizes it with polyether polyol and isophorone diisocyanate to obtain a carbonate-based polyurethane elastomer.
[0021] The present invention uses carbonate-based polyurethane elastomer as a toughening agent to blend and modify polycarbonate. The polyurethane elastomer contains a polyether flexible soft segment and has high mechanical properties such as toughness and elasticity. At the same time, it contains a hard segment of a bisphenol A carbonate structural unit, which has strong similar compatibility with the carbonate structural unit in the polycarbonate, significantly improving the compatibility between the polyurethane elastomer and the polycarbonate matrix. The two form an alloy-like phase, so that the polyurethane elastomer has a better toughening effect. The elongation at break of the polycarbonate reaches 94.5-139.4%, and the impact strength reaches 68.5-95.1 kJ / m 2 , the bending strength reaches 88.3-107.0MPa.
[0022] The carbonate-based polyurethane elastomer of the present invention contains naphthalene rings and multiple benzene rings in its hard segment, has strong heat resistance, has little effect on the heat resistance of polycarbonate, and when added in an appropriate amount, can increase the thermal decomposition temperature of the polycarbonate material, making the polycarbonate exhibit higher heat resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the reaction formula for preparing naphthyl carbonate chain extender. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.
[0025] The polycarbonate model in the embodiment of the present invention is bisphenol A polycarbonate.
[0026] Embodiment 1:
[0027] (1) Place a flask in an ice bath, add 80 mL of dichloromethane, 15 mmol of bisphenol A, 30 mmol of pyridine, and 33 mmol of p-bromochlorophenyl formate, and stir at 15°C for 6 h. After filtering, the filtrate is rotary evaporated and separated by chromatography. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 5:1 to obtain bisphenol A carbonate bromobenzene monomer; the yield is 8.12 g.
[0028] (2) Add 60 mL of N,N-dimethylformamide, 10 mmol of bisphenol A carbonate bromobenzene monomer, 26 mmol of 6-hydroxynaphthalene-2-boric acid, 0.44 mmol of (1,1'-bis(diphenylphosphino)ferrocene) palladium dichloride, 34 mmol of potassium carbonate, and 20 mL of deionized water to a flask, stir and react at 110°C for 18 h, add ethyl acetate and deionized water, mix well, and then stand to separate the layers. Separate the deionized phase, dry the ethyl acetate organic phase to remove water, rotary evaporate, and perform chromatography column separation. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 3:1 to obtain a naphthyl carbonate chain extender. The yield is 4.07 g.
[0029] (3) Add 20 mmol of polyethylene glycol 1000 into a flask and dehydrate under vacuum. Then add 50 mmol of isophorone diisocyanate and heat to 60 °C for reaction for 4 h. Then add 22 mmol of naphthyl carbonate chain extender and 0.12 g of dibutyltin dilaurate. Mix rapidly for 40 s and pour into a preheated mold (temperature is 110 °C). After reaching the gel point, first mature at 120 °C for 12 h and then mature at 25 °C for 7 days to obtain a carbonate-based polyurethane elastomer.
[0030] (4) 900 g of polycarbonate, 100 g of carbonate-based polyurethane elastomer, and 2.8 g of antioxidant 1010 were placed in a mixer and mixed uniformly, and then extruded into granules in a twin-screw extruder. The temperatures in zones 1-6 were 210°C, 240°C, 250°C, 260°C, 260°C, and 255°C. Finally, the mixture was injection molded in an injection molding machine at an injection pressure of 80 MPa and a temperature of 280°C to obtain an elastomer-toughened modified polycarbonate.
[0031] Embodiment 2:
[0032] (1) Place a flask in an ice bath, add 80 mL of dichloromethane, 15 mmol of bisphenol A, 30 mmol of pyridine, and 32 mmol of p-bromochlorophenyl formate, and stir at 25°C for 4 h. After filtering, the filtrate is rotary evaporated and separated by chromatography. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 5:1 to obtain bisphenol A carbonate bromobenzene monomer; the yield is 8.04 g.
[0033] (2) Add 80 mL of N,N-dimethylformamide, 10 mmol of bisphenol A carbonate bromobenzene monomer, 26 mmol of 6-hydroxynaphthalene-2-boric acid, 0.58 mmol of (1,1'-bis(diphenylphosphino)ferrocene) palladium dichloride, 34 mmol of potassium carbonate, and 30 mL of deionized water to a flask, stir and react at 120°C for 12 h, add ethyl acetate and deionized water, mix well, and then stand to separate the layers. Separate the deionized phase, dry the ethyl acetate organic phase to remove water, rotary evaporate, and perform chromatography column separation. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 3:1 to obtain a naphthyl carbonate chain extender. The yield is 4.62 g.
[0034] (3) Add 20 mmol of polyethylene glycol 1000 into a flask and dehydrate under vacuum. Then add 56 mmol of isophorone diisocyanate and heat to 60°C for reaction for 4 h. Then add 24 mmol of naphthyl carbonate chain extender and 0.13 g of dibutyltin dilaurate. Mix rapidly for 50 s and pour into a preheated mold (temperature is 110°C). After reaching the gel point, first mature at 110°C for 24 h and then mature at 20°C for 7 days to obtain a carbonate-based polyurethane elastomer.
[0035] (4) 850 g of polycarbonate, 150 g of carbonate-based polyurethane elastomer, and 2 g of antioxidant 1010 were placed in a mixer and mixed evenly. The mixture was then extruded and granulated in a twin-screw extruder. The temperatures in zones 1-6 were 210°C, 240°C, 250°C, 260°C, 260°C, and 255°C. The mixture was then injection molded in an injection molding machine at a pressure of 80 MPa and a temperature of 270°C to obtain an elastomer-toughened modified polycarbonate.
[0036] Embodiment 3:
[0037] (1) Place a flask in an ice bath, add 100 mL of dichloromethane, 15 mmol of bisphenol A, 33 mmol of pyridine, and 33 mmol of p-bromochlorophenyl formate, and stir at 25°C for 4 h. After filtering, rotary evaporate the filtrate and separate it by chromatography. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 5:1 to obtain bisphenol A carbonate bromobenzene monomer; the yield is 7.73 g.
[0038] (2) Add 70 mL of N,N-dimethylformamide, 10 mmol of bisphenol A carbonate bromobenzene monomer, 25 mmol of 6-hydroxynaphthalene-2-boric acid, 0.48 mmol of (1,1'-bis(diphenylphosphino)ferrocene) palladium dichloride, 34 mmol of potassium carbonate, and 20 mL of deionized water to a flask, stir and react at 130°C for 1 hour, add ethyl acetate and deionized water, mix well, and then stand to separate the layers. Separate the deionized phase, dry the ethyl acetate organic phase to remove water, rotary evaporate, and perform chromatography column separation. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 3:1 to obtain a naphthyl carbonate chain extender. The yield is 4.21 g.
[0039] (3) Add 20 mmol of polypropylene glycol 1000 into a flask and dehydrate it under vacuum. Then add 50 mmol of isophorone diisocyanate and heat it to 60°C. React for 4 h. Then add 22 mmol of naphthyl carbonate chain extender and 0.11 g of dibutyltin dilaurate. Mix them by rapid stirring for 40 s. Then pour it into a preheated mold (temperature is 110°C). After reaching the gel point, first mature it at 110°C for 24 h and then mature it at 20°C for 7 days to obtain a carbonate-based polyurethane elastomer.
[0040] (4) 780 g of polycarbonate, 220 g of carbonate-based polyurethane elastomer, and 5 g of antioxidant 1010 were placed in a mixer and mixed evenly. The mixture was then extruded and granulated in a twin-screw extruder. The temperatures in zones 1-6 were 210°C, 240°C, 250°C, 260°C, 260°C, and 255°C. The mixture was then injection molded in an injection molding machine at a pressure of 80 MPa and a temperature of 270°C to obtain an elastomer-toughened modified polycarbonate.
[0041] Embodiment 4:
[0042] (1) Place a flask in an ice bath, add 80 mL of dichloromethane, 15 mmol of bisphenol A, 30 mmol of pyridine, and 33 mmol of p-bromochlorophenyl formate, and stir at 20°C for 10 h. After filtering, rotary evaporate the filtrate and separate it by chromatography. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 5:1 to obtain bisphenol A carbonate bromobenzene monomer; the yield is 7.82 g.
[0043] (2) Add 80 mL of N,N-dimethylformamide, 10 mmol of bisphenol A carbonate bromobenzene monomer, 23 mmol of 6-hydroxynaphthalene-2-boric acid, 0.58 mmol of (1,1'-bis(diphenylphosphino)ferrocene) palladium dichloride, 38 mmol of potassium carbonate, and 25 mL of deionized water to a flask, stir and react at 110°C for 18 h, add ethyl acetate and deionized water, mix well, and then stand to separate the layers. Separate the deionized phase, dry the ethyl acetate organic phase to remove water, rotary evaporate, and perform chromatography column separation. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 3:1 to obtain a naphthyl carbonate chain extender. The yield is 3.87 g.
[0044] (3) Add 20 mmol of polyethylene glycol 1000 into a flask and dehydrate under vacuum. Then add 56 mmol of isophorone diisocyanate and heat to 65 °C for 4 h. Then add 26 mmol of naphthyl carbonate chain extender and 0.13 g of dibutyltin dilaurate. Mix rapidly for 40 s and pour into a preheated mold (temperature is 110 °C). After reaching the gel point, first mature at 110 °C for 24 h and then mature at 30 °C for 5 days to obtain a carbonate-based polyurethane elastomer.
[0045] (4) 720 g of polycarbonate, 280 g of carbonate-based polyurethane elastomer, and 4 g of antioxidant 1010 were placed in a mixer and mixed evenly. The mixture was then extruded and granulated in a twin-screw extruder. The temperatures in zones 1-6 were 210°C, 240°C, 250°C, 260°C, 260°C, and 255°C. The mixture was then injection molded in an injection molding machine at a pressure of 90 MPa and a temperature of 270°C to obtain an elastomer-toughened modified polycarbonate.
[0046] Embodiment 5:
[0047] (1) Place a flask in an ice bath, add 100 mL of dichloromethane, 15 mmol of bisphenol A, 32 mmol of pyridine, and 32 mmol of p-bromochlorophenyl formate, and stir at 20°C for 6 h. After filtering, rotary evaporate the filtrate and separate it by chromatography. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 5:1 to obtain bisphenol A carbonate bromobenzene monomer; the yield is 8.39 g.
[0048] (2) Add 80 mL of N,N-dimethylformamide, 10 mmol of bisphenol A carbonate bromobenzene monomer, 26 mmol of 6-hydroxynaphthalene-2-boric acid, 0.44 mmol of (1,1'-bis(diphenylphosphino)ferrocene) palladium dichloride, 42 mmol of potassium carbonate, and 30 mL of deionized water to a flask. Stir and react at 120°C for 12 h. Add ethyl acetate and deionized water, mix well, and let stand to separate the layers. Separate the deionized phase, dry the ethyl acetate organic phase to remove water, rotary evaporate, and perform column separation. The eluent is a solution of n-hexane and ethyl acetate in a volume ratio of 3:1 to obtain a naphthyl carbonate chain extender. The yield is 4.07 g.
[0049] (3) Add 20 mmol of polypropylene glycol 1000 into a flask and dehydrate it under vacuum. Then add 52 mmol of isophorone diisocyanate and heat it to 70°C. React for 3 h. Then add 24 mmol of naphthyl carbonate chain extender and 0.12 g of dibutyltin dilaurate. Mix them by rapid stirring for 40 s. Then pour it into a preheated mold (temperature is 110°C). After reaching the gel point, first mature it at 110°C for 24 h and then mature it at 25°C for 7 days to obtain a carbonate-based polyurethane elastomer.
[0050] (4) 650 g of polycarbonate, 350 g of carbonate-based polyurethane elastomer, and 4 g of antioxidant 1010 were placed in a mixer and mixed evenly, and then extruded into granules in a twin-screw extruder. The temperatures in zones 1-6 were 210°C, 240°C, 250°C, 260°C, 260°C, and 255°C. Finally, injection molding was performed in an injection molding machine at an injection molding pressure of 80 MPa and a temperature of 280°C to obtain an elastomer-toughened modified polycarbonate.
[0051] Comparative Example 1
[0052] (1) 900 g of polycarbonate and 2.8 g of antioxidant 1010 were placed in a mixer and mixed, and then extruded into granules in a twin-screw extruder. The temperatures in zones 1-6 were 210°C, 240°C, 250°C, 260°C, 260°C, and 255°C. Finally, the polycarbonate material was obtained by injection molding in an injection molding machine at an injection pressure of 80 MPa and a temperature of 280°C.
[0053] Comparative Example 2
[0054] (1) Add 20 mmol of polyethylene glycol 1000 into a flask, dehydrate under vacuum, then add 50 mmol of isophorone diisocyanate, heat to 60°C, react for 4 h, then add 22 mmol of bisphenol A and 0.12 g of dibutyltin dilaurate, stir rapidly for 40 s, then pour into a preheated mold (temperature is 110°C), after reaching the gel point, first mature at 120°C for 12 h, then mature at 25°C for 7 days to obtain a polyurethane elastomer.
[0055] (2) 900 g of polycarbonate, 100 g of polyurethane elastomer, and 2.8 g of antioxidant 1010 were placed in a mixer and mixed uniformly, and then extruded into granules in a twin-screw extruder. The temperatures in zones 1-6 were 210°C, 240°C, 250°C, 260°C, 260°C, and 255°C. Finally, injection molding was performed in an injection molding machine at an injection molding pressure of 80 MPa and a temperature of 280°C to obtain an elastomer-toughened modified polycarbonate.
[0056] Comparative Example 3
[0057] (1) Add 20 mmol of polycarbonate diol 1000 into a flask and dehydrate under vacuum. Then add 50 mmol of isophorone diisocyanate and heat to 60°C to react for 4 h. Then add 22 mmol of bisphenol A and 0.12 g of dibutyltin dilaurate and stir rapidly for 40 seconds. Then pour into a preheated mold (temperature is 110°C). After reaching the gel point, first mature at 120°C for 12 h and then mature at 25°C for 7 days to obtain a carbonate-based polyurethane elastomer.
[0058] (2) 900 g of polycarbonate, 100 g of carbonate-based polyurethane elastomer, and 2.8 g of antioxidant 1010 were placed in a mixer and mixed uniformly, and then extruded into granules in a twin-screw extruder. The temperatures in zones 1-6 were 210°C, 240°C, 250°C, 260°C, 260°C, and 255°C. Finally, the mixture was injection molded in an injection molding machine at an injection pressure of 80 MPa and a temperature of 280°C to obtain an elastomer-toughened modified polycarbonate.
[0059] The tensile properties of polycarbonate are tested according to GB / T 1040.1-2018; the bending properties are tested according to GB / T 9341-2008; and the impact properties are tested according to GB / T 1843-2008.
[0060] Table 1 Polycarbonate performance test table
[0061] Tensile strength (MPa) Elongation at break (%) <![CDATA[Impact strength (kJ / m 2 ).]]> Bending strength (MPa) Example 1 50.6 94.5 68.5 88.3 Example 2 62.4 112.7 73.2 96.1 Example 3 60.3 135.0 79.7 104.5 Example 4 54.8 139.4 95.1 107.0 Example 5 48.9 127.5 92.4 99.3 Comparative Example 1 46.2 31.9 28.5 61.6 Comparative Example 2 44.6 58.2 43.8 68.9 Comparative Example 3 55.7 77.3 60.1 79.0
[0062] The thermal properties of polycarbonate were tested by thermogravimetric analyzer, with nitrogen as the test atmosphere and the test temperature range from room temperature to 800°C. 5% is the temperature at which 5% of the mass is lost. 50% is the temperature at which 50% of the mass is lost.
[0063] Table 2 Polycarbonate thermal decomposition temperature test
[0064] <![CDATA[T 5% (℃)]]> <![CDATA[T 50% (℃)]]> Example 1 453.5 501.2 Example 2 458.8 505.9 Example 3 460.1 503.0 Example 4 454.3 501.6 Example 5 452.5 498.8 Comparative Example 1 456.2 502.3 Comparative Example 2 428.0 467.4 Comparative Example 3 439.7 478.8
[0065] As shown in Table 1 and Table 2, the polycarbonate of Comparative Example 1 has no polyurethane elastomer added, and its tensile strength is 46.2MPa, elongation at break is 31.9%, and impact strength is 28.5kJ / m 2 , the bending strength is 61.6MPa.
[0066] The polycarbonate in Examples 1-5 is added with a carbonate-based polyurethane elastomer, which contains a polyether flexible soft segment and has high mechanical properties such as toughness and elasticity; and also contains a bisphenol A carbonate structural unit ( ) has a strong similar compatibility with the carbonate structural unit in polycarbonate, which significantly improves the compatibility between polyurethane elastomer and polycarbonate matrix. The two form an alloy-like phase, which makes the polyurethane elastomer have a good toughening effect. The elongation at break of polycarbonate reaches 94.5-139.4%, and the impact strength reaches 68.5-95.1kJ / m 2 , the bending strength reaches 88.3-107.0MPa. In addition, the hard segment of the polyurethane elastomer contains naphthalene rings and multiple benzene rings, which have strong heat resistance and little effect on the heat resistance of polycarbonate. When added in an appropriate amount, it can increase the thermal decomposition temperature of the polycarbonate material, making the polycarbonate show higher heat resistance.
[0067] Compared with Example 1, the difference of Comparative Example 2 is that bisphenol A is used as a chain extender when preparing the polyurethane elastomer, and the obtained polyurethane elastomer does not contain carbonate structural units, resulting in poor compatibility between the polyurethane elastomer and polycarbonate, poor toughening effect, and the tensile properties, impact strength, bending strength and other properties of the polycarbonate are all lower than those of Example 1. In addition, the thermal decomposition temperature is low and the heat resistance is poor.
[0068] In comparative example 3, when preparing a polyurethane elastomer, polycarbonate diol was used as the soft segment, and the obtained polyurethane elastomer was also very compatible with polycarbonate, and the tensile strength of polycarbonate was significantly improved. However, the polyurethane elastomer was a polyester polyurethane, did not contain a flexible polyether segment, and had lower elasticity and toughness than the polyether polyurethane elastomers of Examples 1-5, resulting in poor toughening effect. The elongation at break, impact strength, flexural strength and other properties of the polycarbonate were all lower than those of Example 1. In addition, the thermal decomposition temperature was low, and the heat resistance was poor.
[0069] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. An elastomer toughened modified polycarbonate, characterized in that: The method comprises the following raw materials: 65-90 parts by weight of polycarbonate, 10-35 parts by weight of carbonate-based polyurethane elastomer, and 0.2-0.5 parts by weight of antioxidant; The preparation method of the carbonate-based polyurethane elastomer is: Add polyether polyol into a flask, vacuum dehydrate, then add isophorone diisocyanate, heat to 60-70°C, react for 3-4h, then add naphthyl carbonate chain extender and dibutyltin dilaurate, quickly stir and mix for 40-50s, then pour into a preheated mold, and perform aging treatment after reaching the gel point to obtain a carbonate-based polyurethane elastomer; The molar ratio of the polyether polyol, isophorone diisocyanate and naphthyl carbonate chain extender is 1:(2.5-2.8):(1.1-1.3); the polyether polyol includes polyethylene glycol and / or polypropylene glycol; The preparation method of the naphthyl carbonate chain extender is: (1) placing a flask in an ice bath, adding dichloromethane, bisphenol A, pyridine, and p-bromophenyl chloroformate, stirring to react, filtering, rotary evaporating the filtrate, and performing column chromatography separation to obtain bisphenol A carbonate bromobenzene monomer; (2) Add N,N-dimethylformamide, bisphenol A carbonate bromobenzene monomer, 6-hydroxynaphthalene-2-boric acid, (1,1'-bis(diphenylphosphino)ferrocene) palladium dichloride, potassium carbonate, and deionized water into a flask, stir to react, add ethyl acetate and deionized water, mix well, let stand to separate, separate the dehydrated phase, dry the ethyl acetate organic phase to remove water, rotary evaporate, and separate by chromatography to obtain a naphthyl carbonate chain extender; The molar ratio of bisphenol A, pyridine and p-bromochlorophenylformate in (1) is 1:(2-2.2):(2-2.2); The molar ratio of bisphenol A carbonate bromobenzene monomer, 6-hydroxynaphthalene-2-boric acid, (1,1'-bis(diphenylphosphino)ferrocene)palladium dichloride and potassium carbonate in (2) is 1:(2.3-2.6):(0.044-0.058):(3.4-4.2).
2. The elastomer toughened modified polycarbonate according to claim 1, characterized in that: The aging treatment is firstly aging at 110-120° C. for 12-24 hours, and then aging at 20-30° C. for 5-7 days.
3. The elastomer toughened modified polycarbonate according to claim 1, characterized in that: The reaction temperature in (1) is 15-25°C and the reaction time is 4-10h.
4. The elastomer toughened modified polycarbonate according to claim 1, characterized in that: The reaction temperature in (2) is 110-130°C and the reaction time is 12-18h.
5. A method for preparing an elastomer toughened modified polycarbonate according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: placing polycarbonate, carbonate-based polyurethane elastomer and antioxidant in a mixer and mixing them evenly; then extruding and granulating them in a twin-screw extruder; and finally injection molding them in an injection molding machine to obtain elastomer toughened and modified polycarbonate.
6. The method for preparing the elastomer toughened modified polycarbonate according to claim 5, characterized in that: The twin-screw extruder is used for extrusion granulation, and the temperature of zones 1-6 is 210-260° C.; the injection molding pressure of the injection molding machine is 80-90 MPa, and the temperature is 270-280° C.