Non-oriented silicon steel and preparation method thereof
By optimizing the chemical composition and process steps of non-oriented silicon steel, the problems of poor electromagnetic properties and low yield strength of non-oriented silicon steel in the prior art were solved, and high-performance silicon steels that meet the needs of new energy electric vehicles were prepared.
Patent Information
- Application Number
- CN202410921520.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The existing unoriented silicon steel has poor high-frequency electromagnetic performance and low yield strength, which cannot meet the high requirements of new energy electric vehicle drive motors.
Through the process of water-molding, continuous casting, hot rolling, regularization, cold rolling, annealing, etc., chemical composition and process parameters are controlled, including the content of Si, Al, Mn, Sn, Sb, N, P, Nb, Ti, V and Process conditions, optimize grain structure and texture, and improve electromagnetic properties and yield strength.
Non-oriented silicon steel with excellent electromagnetic properties and high yield strength was prepared to meet the high requirements of iron core materials for new energy electric vehicles, extend service life and reduce material costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, relates to a method for preparing non-oriented silicon steel, and also relates to non-oriented silicon steel prepared by the preparation method. Background Art
[0002] New energy electric vehicles can ease the dependence of automobiles on fossil fuels, reduce greenhouse gas emissions, and reduce environmental pollution, and therefore have broad market prospects.
[0003] The drive motor is the power center of the electric vehicle. The iron core is a key component for the drive motor to achieve energy conversion. Non-oriented silicon steel is often used as the iron core material for the rotor of the motor and generator working in a rotating magnetic field.
[0004] In order to improve the energy conversion efficiency and output power of the drive motor of new energy electric vehicles, extend its service life, and reduce material costs, it is necessary to prepare non-oriented silicon steel with excellent high-frequency electromagnetic properties and high yield strength. Summary of the invention
[0005] The object of the present invention is to provide a non-oriented silicon steel and a preparation method thereof, so as to solve the technical problems of poor high-frequency electromagnetic properties and low yield strength of non-oriented silicon steel in the prior art.
[0006] To achieve one of the above objectives, an embodiment of the present invention provides a method for preparing non-oriented silicon steel, comprising the steps of molten steel smelting, continuous casting, hot rolling, normalizing, cold rolling, and annealing in sequence;
[0007] The chemical composition of the molten steel finally obtained in the molten steel smelting process includes, by mass percentage, C≤0.003%, Si2.65~3.50%, Mn 0.2~0.8%, S≤0.003%, N≤0.003%, P≤0.03%, and satisfies: 3.6%≤Si+Al≤4.5%, Sn+Sb≤0.2%, Nb+Ti+V≤0.005%, and the rest is Fe and unavoidable impurities;
[0008] In the continuous casting process, electromagnetic stirring is used, and the equiaxed crystal ratio of the obtained continuous casting billet is ≥50%;
[0009] In the hot rolling process, the continuous casting slab is heated, rough rolled, finished rolled and rolled in sequence to obtain a hot rolled coil. The heating temperature is 1080-1150°C, the temperature fluctuation is controlled within ±20°C, and the heating time is ≥150min.
[0010] In the normalizing process, the normalizing temperature is 840-950° C., the normalizing holding time is 180-200 s, and the grain size of the hot-rolled coil after normalizing is 80-120 μm;
[0011] In the cold rolling process, a single cold rolling method is adopted to obtain a non-oriented silicon steel strip with a thickness t of 0.2-0.3 mm, wherein the reduction rate of the first pass is ≥30%, and the reduction rates of the remaining passes except the last pass are ≥25%;
[0012] In the annealing process, the non-oriented silicon steel strip is subjected to continuous recrystallization annealing, the annealing temperature is 950-1020° C., and the annealing holding time is 40-120 s.
[0013] In the chemical composition design scheme with a high alloy content, especially when the total content of Si and Al is 3.6-4.5%, the present application limits the Si content to 2.65-3.50%, and limits the types and contents of other chemical elements, so that not only good iron loss can be obtained, but also the finished product has good yield strength; further, by adding microalloying elements Sn or Sb, the principle that Sn or Sb is easy to be enriched on the surface of the strip can be used to avoid the formation of AlN in the annealing process of the strip, improve the annealing structure, and obtain excellent electromagnetic properties; further combined with the control of the upper limit of the content of harmful elements S, N, and P, it can be Reduce the adverse effects of harmful elements on magnetic properties and brittleness; in addition, by controlling the upper limits of Nb, Ti, and V contents, it is possible to avoid Nb, V, Ti, C, and N forming smaller carbides and nitrides to hinder grain growth, and reduce the formation of unfavorable textures; further coordinated with the control of continuous casting, hot rolling, normalizing, cold rolling, and annealing processes, a non-oriented silicon steel strip with a thickness t of 0.2 to 0.3 mm can be prepared by only one cold rolling, and the non-oriented silicon steel has excellent electromagnetic properties and high strength, which can meet the high requirements of new energy electric vehicles for core materials, and greatly shorten the production process, reduce production difficulty and manufacturing costs.
[0014] Among them, the role of each element in the chemical composition design scheme of the non-oriented silicon steel of this application is as follows:
[0015] C is a harmful element in non-oriented silicon steel. A high C content is prone to magnetic aging, which increases the iron loss of the non-oriented silicon steel product. Therefore, in this application, the C content is controlled at a relatively low level, that is, the C content is controlled to C≤0.003%.
[0016] Si can effectively increase the resistivity of non-oriented silicon steel, reduce iron loss, and effectively improve the strength of steel. However, as the Si content increases, the hardness and brittleness of the steel increase, which will increase the risk of fracture during the production process. In this application, the Si content is controlled to be 2.65~3.50%.
[0017] Al can increase the resistivity of non-oriented silicon steel and reduce eddy current loss. Since the atomic radius of Al is smaller than that of Si, increasing Al can reduce lattice distortion. Compared with the same amount of Si, the increase in brittleness and hardness of steel is small, and the processability and magnetic properties of the material can be increased. However, too high Al content will lead to poor formability of the material.
[0018] In this application, the total content of Si and Al is limited to 3.6-4.5% to reduce high-frequency iron loss, improve strength, and avoid a significant increase in material brittleness, thereby reducing the risk of fracture during the preparation process.
[0019] Mn is also one of the elements that improve resistivity, which can reduce iron loss to a certain extent, improve hot workability, and improve yield strength. Mn can also form MnS with S to prevent the formation of low-melting-point FeS along the grain boundaries and cause hot brittleness of the hot-rolled plate. In this application, the Mn content is controlled to be 0.2~0.8%.
[0020] Sn and Sb can improve annealing texture, increase magnetic induction, and reduce iron loss, but excessive addition of Sn and Sb will make the material brittle. In this application, Sn+Sb is controlled to be ≤0.2%.
[0021] When S and Mn form fine MnS, it can strongly hinder the grain growth of the non-oriented silicon steel product during annealing. An increase in the S content will lead to the deterioration of the magnetic properties of the non-oriented silicon steel. In addition, excessive MnS deposition will make the grain boundaries brittle, thereby causing hot brittleness and reducing the processing performance. In this application, the S content is controlled to be ≤0.003%.
[0022] N is a harmful element, which easily forms fine AlN particles and inhibits grain growth. When the N content exceeds 0.003%, the iron loss is likely to increase significantly. In this application, the N content is controlled to be ≤0.003%.
[0023] P has a larger atomic radius than Fe and Si, and has the effect of increasing strength and improving punching properties. However, if the P content is too high, the cold workability will deteriorate and the material will become brittle. In this application, the P content is controlled to be ≤0.03%.
[0024] Nb, Ti, and V easily form smaller carbides and nitrides, which not only hinder the growth of grains, but also promote the formation of unfavorable textures. Therefore, Nb+Ti+V is controlled to be ≤0.005%.
[0025] As a further improvement of an embodiment of the present invention, the chemical composition of the molten steel finally obtained in the molten steel smelting process includes, by mass percentage: C≤0.003%, Si 2.65~3.00%, Mn 0.2~0.8%, S≤0.003%, N≤0.003%, P≤0.03%, and satisfies: 3.6%≤Si+Al≤4.5%, Al / Si≥0.3, Sn+Sb≤0.2%, Nb+Ti+V≤0.005%, and the rest is Fe and inevitable impurities.
[0026] When the Si content is 2.65~3.00%, by controlling the Al / Si content ratio ≥0.3, the brittleness caused by too high Si content can be avoided, so that the non-oriented silicon steel has good cold and hot processing properties, and at the same time, the non-oriented silicon steel can be ensured to have excellent electromagnetic properties.
[0027] As a further improvement of an embodiment of the present invention, the chemical composition of the molten steel finally obtained in the molten steel smelting process includes, by mass percentage: C≤0.003%, Mn 0.2~0.8%, S≤0.003%, N≤0.003%, P≤0.03%, and satisfies: 3.00%<Si≤3.50%, 3.6%≤Si+Al≤4.5%, Al / Si<0.3, Sn+Sb≤0.2%, Nb+Ti+V≤0.005%, and the rest is Fe and inevitable impurities.
[0028] When 3.00%<Si≤3.50%, by controlling the Al / Si content ratio <0.3 and the total content of Si and Al, the non-oriented silicon steel can have excellent electromagnetic properties and workability at high Si content.
[0029] As a further improvement of an embodiment of the present invention, no Cu, Cr, Ni, Nb, V, Ti alloy elements are added in the molten steel smelting process;
[0030] The molten steel smelting process includes a converter smelting step and an RH refining step; in the RH refining step, ferrosilicon alloy and aluminum alloy are added simultaneously during alloying, and the RH refining time ≥30min.
[0031] By not adding Cu, Cr, Ni, Nb, V, Ti alloy elements in the molten steel smelting process, the content of these alloy elements in the chemical composition of the finally obtained molten steel can be controlled, so as to avoid the formation of small carbides and nitrides pinning the grain boundaries and hindering the grain growth, and reduce the adverse impact on the iron loss of high-grade silicon steel; further, by adding ferrosilicon alloy and aluminum alloy simultaneously during alloying in the RH refining step, the rapid formation and floating removal of Al2O3-based unfavorable inclusions can be promoted, thereby improving the cleanliness of the molten steel.
[0032] As a further improvement of one embodiment of the present invention, in the hot rolling process, the starting temperature of rough rolling is ≤1150°C, the starting temperature of finishing rolling is 950±20°C, the final rolling temperature is 830~870°C, and the coiling temperature is 610~650°C.
[0033] On the basis of the aforementioned chemical composition design scheme, the hot rolling process adopts low-temperature rolling and low-temperature coiling, combined with the control of the heating temperature and heating time of the continuous casting billet. While ensuring production efficiency, the probability of precipitation of fine AlN and MnS can be reduced, which is beneficial to the growth of organizational grains, thereby ensuring the excellent magnetic properties of the final non-oriented silicon steel product.
[0034] As a further improvement of one embodiment of the present invention, the thickness of the continuous casting billet obtained in the continuous casting step is 200-250 mm;
[0035] In the hot rolling process, the continuous casting billet is subjected to rough rolling to obtain an intermediate billet with a thickness of 35 to 40 mm, and the intermediate billet is subjected to finish rolling to obtain a hot rolled plate with a thickness of 2.0 to 2.5 mm.
[0036] By limiting the thickness of the continuous casting billet, the intermediate billet after rough rolling, and the hot rolled plate obtained after finish rolling, it is beneficial to reasonably distribute the reduction amount of each step, so that the finally prepared thin-gauge non-oriented silicon steel has good magnetic properties and strength.
[0037] As a further improvement of one embodiment of the present invention, in the annealing process, annealing is performed in a continuous annealing furnace, and an insulating coating is applied to the surface of the non-oriented silicon steel strip after annealing, and the oxygen content in the annealing furnace is controlled to be ≤20ppm. In this way, the formation of an oxide layer on the surface of the non-oriented silicon steel can be reduced, thereby reducing the adverse effects of the surface oxide layer on the electromagnetic properties.
[0038] As a further improvement of one embodiment of the present invention, in the annealing process, the protective atmosphere in the annealing furnace is a mixed gas of N2 and H2, wherein the volume fraction of H2 is ≤60%; or, the protective atmosphere in the annealing furnace is pure N2.
[0039] In this way, by controlling the protective atmosphere in the annealing furnace, the formation of an inner oxide layer and an inner nitride layer in the non-oriented silicon steel strip can be prevented, the surface quality can be improved, and the iron loss can be further reduced.
[0040] In order to achieve the above-mentioned object of the invention, one embodiment of the present invention further provides a non-oriented silicon steel, which is prepared by the preparation method of the non-oriented silicon steel as described above.
[0041] As a further improvement of one embodiment of the present invention, the iron loss P of the non-oriented silicon steel is 10 / 400 ≤(14.59-42.24t+145.9t2 )W / kg, yield strength σ 0.2 It is 400~480MPa.
[0042] That is to say, the non-oriented silicon steel prepared by the above preparation method not only has excellent electromagnetic properties, which can meet the iron loss requirements of non-oriented silicon steel thickness t under different specifications, where t is in mm, but also has excellent yield strength, which can meet the use requirements of core materials for new energy electric vehicles. When used as core materials, it can improve the energy conversion efficiency and output power of the drive motor, extend its service life, and reduce material costs. DETAILED DESCRIPTION
[0043] The present invention will be described in detail below in conjunction with specific embodiments, but these embodiments do not limit the present invention, and any structural, methodological, or functional changes made by a person skilled in the art based on these embodiments are all within the scope of protection of the present invention.
[0044] An embodiment of the present invention provides a method for preparing non-oriented silicon steel, and non-oriented silicon steel prepared by the preparation method.
[0045] In this embodiment, the chemical composition design scheme of the non-oriented silicon steel is as follows, and its chemical composition includes, by mass percentage: C≤0.003%, Si 2.65~3.50%, Mn 0.2~0.8%, S≤0.003%, N≤0.003%, P≤0.03%, and satisfies: 3.6%≤Si+Al≤4.5%, Sn+Sb≤0.2%, Nb+Ti+V≤0.005%, and the rest is Fe and unavoidable impurities.
[0046] In general, the above chemical composition design scheme can not only obtain good iron loss but also have good yield strength of the finished product; further, by adding microalloying elements Sn or Sb, the principle that Sn or Sb is easy to be enriched on the surface of the strip can be used to avoid the formation of AlN in the annealing process of the strip, improve the annealing structure, and obtain excellent elongation and electromagnetic properties; further combined with the control of the upper limit of the content of harmful elements S, N, and P, the adverse effects of harmful elements on magnetic properties and brittleness can be reduced; in addition, by controlling the upper limit of the content of Nb, Ti, and V, it is possible to avoid Nb, V, Ti and C, N forming smaller carbides and nitrides to hinder grain growth, and the formation of unfavorable textures can also be reduced.
[0047] In a preferred embodiment, the chemical composition of the non-oriented electrical steel by mass percentage includes: C ≤ 0.003%, Si 2.65 - 3.00%, Mn 0.2 - 0.8%, S ≤ 0.003%, N ≤ 0.003%, P ≤ 0.03%, and it satisfies: 3.6% ≤ Si + Al ≤ 4.5%, Al / Si ≥ 0.3, Sn + Sb ≤ 0.2%, Nb + Ti + V ≤ 0.005%, and the balance is Fe and inevitable impurities.
[0048] In another preferred embodiment, the chemical composition of the non-oriented electrical steel by mass percentage includes: C ≤ 0.003%, Mn 0.2 - 0.8%, S ≤ 0.003%, N ≤ 0.003%, P ≤ 0.03%, and it satisfies: 3.00% < Si ≤ 3.50%, 3.6% ≤ Si + Al ≤ 4.5%, Al / Si < 0.3, Sn + Sb ≤ 0.2%, Nb + Ti + V ≤ 0.005%, and the balance is Fe and inevitable impurities.
[0049] The following is a specific introduction to the preparation method of the non-oriented electrical steel, including the processes of molten steel smelting, continuous casting, hot rolling, normalizing, cold rolling, annealing, etc. carried out in sequence.
[0050] (1) Molten steel smelting
[0051] The chemical composition of the finally obtained molten steel by mass percentage includes: C ≤ 0.003%, Si 2.65 - 3.50%, Mn 0.2 - 0.8%, S ≤ 0.003%, N ≤ 0.003%, P ≤ 0.03%, and it satisfies: 3.6% ≤ Si + Al ≤ 4.5%, Sn + Sb ≤ 0.2%, Nb + Ti + V ≤ 0.005%, and the balance is Fe and inevitable impurities.
[0052] That is to say, the molten steel smelting process smelts the molten steel according to the chemical composition design scheme of the above non-oriented electrical steel, so that the chemical composition of the finally obtained molten steel is exactly the same as that of the finally prepared non-oriented electrical steel.
[0053] Preferably, no Cu, Cr, Ni, Nb, V, Ti alloy elements are added in the molten steel smelting process.
[0054] Specifically, the molten steel smelting process includes the following steps carried out in sequence:
[0055] a. Converter smelting step
[0056] The hot metal is fed into the converter and mixed with scrap steel to form molten steel and carry out dephosphorization and desiliconization.
[0057] b. RH refining step
[0058] The molten steel after converter smelting is subjected to vacuum decarburization, deoxidation, alloying, and inclusion removal using an RH vacuum circulating degassing device.
[0059] Preferably, ferrosilicon alloy and aluminum alloy are added simultaneously during the alloying process, and the RH refining time is controlled to be ≥30 min.
[0060] In a preferred embodiment, the chemical composition of the molten steel obtained in the final molten steel smelting process includes, by mass percentage: C ≤ 0.003%, Si 2.65 - 3.00%, Mn 0.2 - 0.8%, S ≤ 0.003%, N ≤ 0.003%, P ≤ 0.03%, and satisfies: 3.6% ≤ Si + Al ≤ 4.5%, Al / Si ≥ 0.3, Sn + Sb ≤ 0.2%, Nb + Ti + V ≤ 0.005%, and the rest is Fe and inevitable impurities.
[0061] In another preferred embodiment, the chemical composition of the molten steel obtained in the final molten steel smelting process includes, by mass percentage: C ≤ 0.003%, Mn 0.2 - 0.8%, S ≤ 0.003%, N ≤ 0.003%, P ≤ 0.03%, and satisfies: 3.00% < Si ≤ 3.50%, 3.6% ≤ Si + Al ≤ 4.5%, Al / Si < 0.3, Sn + Sb ≤ 0.2%, Nb + Ti + V ≤ 0.005%, and the rest is Fe and inevitable impurities.
[0062] (2) Continuous casting
[0063] The molten steel obtained in the molten steel smelting process is continuously cast into a continuous casting billet with a thickness of 200 - 250 mm using a continuous casting device. The chemical composition of the obtained continuous casting billet is consistent with that of the molten steel obtained in the final molten steel smelting process and is also exactly the same as the chemical composition of the finally prepared non-oriented silicon steel.
[0064] During continuous casting, electromagnetic stirring is used, which can not only inhibit the development of coarse columnar crystals, reduce the appearance of corrugated defects on the surface of high-grade silicon steel, but also promote the formation of favorable textures in the finished product and improve magnetic properties; the equiaxed crystal ratio of the obtained continuous casting billet is ≥50%.
[0065] (3) Hot rolling
[0066] The continuous casting billet obtained in the continuous casting process is successively passed through heating, rough rolling, finish rolling, and coiling to obtain a hot-rolled coil plate.
[0067] Among them, the heating temperature during heating is 1080 - 1150 °C, the temperature fluctuation is controlled within ±20 °C, and the heating time is ≥150 min.
[0068] By controlling the heating temperature within a lower range, the probability of precipitation of fine AlN and MnS can be reduced, and the solid solution of AlN, MnS and other precipitates in the steel during the heating process can be prevented, which is beneficial to the growth of the microstructure grains, thereby ensuring that the magnetic properties of the final non-oriented silicon steel product are excellent.
[0069] Preferably, the starting rolling temperature of the rough rolling is ≤1150°C, the starting rolling temperature of the finish rolling is 950±20°C, the final rolling temperature is 830-870°C, and the coiling temperature is 610-650°C.
[0070] Specifically, after the continuous casting billet is heated, it is sent to a rough rolling mill to obtain an intermediate billet with a thickness of 35-40 mm after multiple rough rolling. The intermediate billet is then sent to a finishing mill for multiple finishing rolling, and the total reduction rate of the finishing rolling is controlled to be ≥90% to obtain a hot-rolled plate with a thickness of 2.0-2.5 mm. The hot-rolled plate is then coiled after laminar cooling to obtain a hot-rolled coil.
[0071] Among them, the continuous casting billet can be sent to the heating furnace for heating at room temperature, then the heating rate needs to be controlled to be ≤20℃ / min, and the heating time is 200~300min to delay the heating process and extend the time of the continuous casting billet in the furnace, thereby reducing the structural cracking caused by the thermal stress inside the continuous casting billet and ensuring the uniformity of the internal and external temperatures of the continuous casting billet.
[0072] Of course, the continuous casting billet can also be hot-charged and hot-sent into the heating furnace, that is, the entry temperature of the continuous casting billet into the heating furnace is ≥350°C, and the heating time is controlled to be 150~250min. This can make the continuous casting billet have excellent hot rolling plasticity, while avoiding the degradation of magnetic properties, and can shorten the heating time and improve production efficiency.
[0073] (4) Normalization
[0074] The hot rolled coil is subjected to normalizing treatment, the normalizing temperature is 840-950°C, the normalizing holding time is 180-200s, and the grain size of the hot rolled coil after normalizing is 80-120μm.
[0075] The normalizing process can improve the structure and product magnetic properties of non-oriented silicon steel hot-rolled coil, improve the inconsistency of magnetic properties at the head, middle and tail, and control the normalizing temperature and normalizing holding time in combination with the chemical composition design of silicon steel, so that the grain size of the hot-rolled coil after normalization can be controlled to 80~120μm.
[0076] (5) Cold rolling
[0077] By adopting a single cold rolling method, the normalized hot-rolled coil is fed into a cold rolling line for multiple cold rolling passes, and the total cold rolling reduction rate is controlled to be ≥80%, so as to obtain a non-oriented silicon steel strip with a thickness t of 0.2~0.3mm.
[0078] Among them, the reduction rate of the first pass is ≥30%, and except for the last pass, the reduction rate of the remaining passes is ≥25%. The texture of non-oriented silicon steel can be improved and the electromagnetic properties can be improved by using cold rolling with a large reduction rate.
[0079] (6) Annealing
[0080] The non-oriented silicon steel strip obtained by the cold rolling process is subjected to continuous recrystallization annealing, and an insulating coating is applied to the upper and lower surfaces of the strip to obtain non-oriented silicon steel. The specific operation of the coating can be achieved by using existing feasible coating technology, which will not be described in detail here.
[0081] The annealing temperature is 950-1020°C, and the annealing holding time is 40-120s. By controlling the annealing temperature and annealing time, the non-oriented silicon steel strip is fully recrystallized.
[0082] Preferably, annealing is performed in a continuous annealing furnace, and an insulating coating is coated on the surface of the non-oriented silicon steel strip after annealing, and the oxygen content in the annealing furnace is controlled to be ≤20ppm.
[0083] Preferably, the insulating coating is a semi-organic insulating coating, which is an insulating coating mixed with organic and inorganic substances, and can improve the high temperature resistance and stamping performance of non-oriented silicon steel.
[0084] In one embodiment, the protective atmosphere in the annealing furnace is a mixed gas of N2 and H2, wherein the volume fraction of H2 is ≤60%. This protective atmosphere can prevent the non-oriented silicon steel strip from forming an inner oxide layer and an inner nitride layer, improve the surface quality, and further reduce the iron loss.
[0085] In another embodiment, the protective atmosphere in the annealing furnace is pure N2. By adopting the pure N2 protective atmosphere, the formation of nodules due to the reaction between the non-oriented silicon steel strip and the carbon sleeve furnace roller during the high temperature annealing process can be reduced.
[0086] After testing, the non-oriented silicon steel prepared by the above preparation method not only has excellent electromagnetic properties, but also the iron loss of non-oriented silicon steel with thickness t under different specifications meets the following requirements: P 10 / 400 ≤(14.59-42.24t+145.9t 2 )W / kg, t=0.2~0.3mm, and yield strength σ 0.2 It can reach 400~480MPa, which can meet the high requirements of new energy electric vehicles for core materials.
[0087] The detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
[0088] The beneficial effects of the present invention are further illustrated below by means of 9 embodiments and 10 comparative examples. Of course, these 9 embodiments are only a part of the many variations of the present invention, but not all of them.
[0089] 9 embodiments and 10 comparative examples respectively provide a non-oriented silicon steel, and the chemical compositions of the molten steel obtained by smelting molten steel, the continuous casting billet and the finally prepared non-oriented silicon steel in each embodiment are the same, and the chemical compositions of the 9 embodiments and 10 comparative examples are specifically referred to Table 1. In addition, in addition to the chemical elements shown in Table 1, in the chemical compositions of the 9 embodiments and 10 comparative examples, C≤0.003%, S≤0.003%, N≤0.003%, P≤0.03%, Nb+Ti+V≤0.005%, and the rest are Fe and unavoidable impurities.
[0090] Table 1
[0091]
[0092] The preparation method of non-oriented silicon steel comprises the following steps:
[0093] (1) Molten steel smelting
[0094] The chemical composition of the molten steel obtained by smelting is as described above, please refer to Table 1 for details.
[0095] No alloy elements Cu, Cr, Ni, Nb, V and Ti are added in the molten steel smelting process.
[0096] The molten steel smelting process specifically includes the following steps performed in sequence:
[0097] a. Converter smelting steps
[0098] The molten iron is fed into the converter and mixed with scrap steel to form molten steel, where it is dephosphorized and desiliconized.
[0099] b. RH refining steps
[0100] RH vacuum cycle degassing equipment is used to vacuum decarburize, deoxidize, alloy and remove inclusions from molten steel after converter smelting. Ferrosilicon alloy and aluminum alloy are added simultaneously during the alloying process, and the RH refining time is controlled to be ≥30min.
[0101] (2) Continuous casting
[0102] The molten steel obtained in the molten steel smelting process is continuously cast into a continuous casting billet with a thickness of 200-250 mm using a continuous casting equipment. The chemical composition of the obtained continuous casting billet is also as described above, please refer to Table 1 for details.
[0103] During the continuous casting process, electromagnetic stirring is used, and the equiaxed crystal ratio of the obtained continuous casting billet is ≥50%.
[0104] (3) Hot rolling
[0105] The continuous casting slab obtained in the continuous casting process is sequentially heated, rough rolled, finish rolled and coiled to obtain a hot rolled coil.
[0106] Among them, the heating temperature during heating is shown in Table 2, the heating temperature fluctuation is controlled within ±20°C, and the heating time is ≥150min; the starting rolling temperature of rough rolling is ≤1150°C, the starting rolling temperature of finishing rolling is 950±20°C, and the final rolling temperature and coiling temperature are shown in Table 2.
[0107] Specifically, after the continuous casting billet is heated, it is sent to a rough rolling mill to obtain an intermediate billet with a thickness of 35-40 mm after multiple rough rolling. The intermediate billet is then sent to a finishing mill for multiple finishing rolling, and the total reduction rate of the finishing rolling is controlled to be ≥90% to obtain a hot-rolled plate with a thickness of 2.0-2.5 mm. The hot-rolled plate is then coiled after laminar cooling to obtain a hot-rolled coil.
[0108] If the continuous casting billet is sent to a heating furnace for heating at room temperature, the heating rate is controlled to be ≤20°C / min, and the heating time is 200-300min.
[0109] If the temperature of the continuous casting billet when it is fed into the heating furnace is ≥350°C, the heating time is controlled to be 150-250 minutes.
[0110] (4) Normalization
[0111] The hot rolled coil is subjected to normalizing treatment, the normalizing temperature is shown in Table 2, the normalizing holding time is 180-200s, and the grain size of the hot rolled coil after normalizing is 80-120μm.
[0112] (5) Cold rolling
[0113] By adopting a single cold rolling method, the normalized hot-rolled coil is fed into a cold rolling line for multiple cold rolling passes, and the total cold rolling reduction rate is controlled to be ≥80% to obtain a non-oriented silicon steel strip. The thickness t of the non-oriented silicon steel strip is shown in Table 3.
[0114] Among them, the reduction rate of the first pass is ≥30%, and except for the last pass, the reduction rates of the remaining passes are ≥25%.
[0115] (6) Annealing
[0116] The non-oriented silicon steel strip obtained in the cold rolling process is subjected to continuous recrystallization annealing in a continuous annealing furnace, and an insulating coating is applied to the surface of the non-oriented silicon steel strip after annealing, and the oxygen content in the annealing furnace is controlled to be ≤20ppm, the annealing temperature is shown in Table 2, and the annealing holding time is 40-120s. Then, an insulating coating is applied to the upper and lower surfaces of the strip, and the specific operation of the coating can be achieved by using existing feasible coating technology, which will not be described in detail here.
[0117] The protective atmosphere in the annealing furnace is a mixed gas of N2 and H2, wherein the volume fraction of H2 is ≤60%. Alternatively, the protective atmosphere in the annealing furnace is pure N2.
[0118] Table 2
[0119]
[0120] Among them, comparative examples 2, 4, 6, and 9 cracked during cold rolling, so the subsequent annealing process was no longer carried out, and thus there were no relevant parameters for the annealing process; comparative example 8 cracked during hot rolling, so the subsequent normalizing, cold rolling, and annealing processes were no longer carried out, and there were no hot rolling final rolling temperature, coiling temperature, and relevant parameters for subsequent processes.
[0121] The electromagnetic properties and mechanical properties of the finished non-oriented silicon steel strips of the above embodiments and comparative examples were tested as follows:
[0122] <Electromagnetic performance>
[0123] The electromagnetic properties of the finished non-oriented silicon steel strip were tested according to GB / T3655-2022 standard, and the iron loss P 10 / 400 The data are shown in Table 3.
[0124] <Mechanical properties>
[0125] The mechanical properties of the finished non-oriented silicon steel strip were tested with reference to GB / T228.1-2021 standard. Specifically, the yield strength σ of the finished non-oriented silicon steel strip was tested using a tensile testing machine. 0.2 The test was carried out and the test results are shown in Table 3.
[0126] Table 3
[0127]
[0128] Among them, in the 9 embodiments, the iron loss of non-oriented silicon steel strips with different thicknesses t all meet the following requirements: P 10 / 400 ≤(14.59-42.24t+145.9t 2 )W / kg, yield strength σ 0.2 They are all within the range of 400~480MPa, which not only meets the iron loss requirements of products of different thickness specifications, but also has excellent electromagnetic properties and high strength, which can meet the high requirements of new energy electric vehicles for core materials.
[0129] Comparative Examples 2, 4, 6, and 9 cracked during cold rolling, Comparative Example 8 cracked during hot rolling, and the non-oriented silicon steel strip of Comparative Example 5 was bonded during punching. The iron loss and yield strength of Comparative Examples 1 and 3 did not meet the use requirements of the corresponding thickness specifications, and the iron loss of Comparative Examples 7 and 10 did not meet the use requirements of the corresponding thickness specifications.
[0130] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0131] The detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing non-oriented silicon steel, characterized in that: It includes the processes of molten steel smelting, continuous casting, hot rolling, normalizing, cold rolling and annealing in sequence; The chemical composition of the molten steel finally obtained in the molten steel smelting process includes, by mass percentage: C≤0.003%, Mn 0.2~0.8%, S≤0.003%, N≤0.003%, P≤0.03%, and meets: 3.6%≤Si+Al≤4.5%, Sn+Sb≤0.2%, Nb+Ti+V≤0.005%, and the rest is Fe and unavoidable impurities; and meets: Si 2.65~3.00%, Al / Si≥0.3, or meets: 3.00% <Si≤3.50%、Al / Si<0.3; In the continuous casting process, electromagnetic stirring is used, and the equiaxed crystal ratio of the obtained continuous casting billet is ≥50%; In the hot rolling process, the continuous casting slab is heated, rough rolled, finished rolled and rolled in sequence to obtain a hot rolled coil. The heating temperature is 1080-1150°C, the temperature fluctuation is controlled within ±20°C, and the heating time is ≥150min. In the normalizing process, the normalizing temperature is 840-950° C., the normalizing holding time is 180-200 s, and the grain size of the hot-rolled coil after normalizing is 80-120 μm; In the cold rolling process, a single cold rolling method is adopted to obtain a non-oriented silicon steel strip with a thickness t of 0.2-0.3 mm, wherein the reduction rate of the first pass is ≥30%, and the reduction rates of the remaining passes except the last pass are ≥25%; In the annealing process, the non-oriented silicon steel strip is subjected to continuous recrystallization annealing, the annealing temperature is 950-1020° C., and the annealing holding time is 40-120 s; The iron loss P of the obtained non-oriented silicon steel 10 / 400 ≤(14.59-42.24t+145.9t 2 )W / kg, yield strength σ 0.2 It is 400~480MPa.
2. The method for preparing non-oriented silicon steel according to claim 1, characterized in that: The alloy elements Cu, Cr, Ni, Nb, V and Ti are not added in the molten steel smelting process; The molten steel smelting process includes a converter smelting step and an RH refining step; in the RH refining step, ferrosilicon alloy and aluminum alloy are added simultaneously during the alloying process, and the RH refining time is ≥30 minutes.
3. The method for preparing non-oriented silicon steel according to claim 1, characterized in that: In the hot rolling process, the starting rolling temperature of the rough rolling is ≤1150°C, the starting rolling temperature of the finishing rolling is 950±20°C, the final rolling temperature is 830~870°C, and the coiling temperature is 610~650°C.
4. The method for preparing non-oriented silicon steel according to claim 1, characterized in that: The thickness of the continuous casting billet obtained in the continuous casting process is 200-250 mm; In the hot rolling process, the continuous casting billet is subjected to rough rolling to obtain an intermediate billet with a thickness of 35 to 40 mm, and the intermediate billet is subjected to finish rolling to obtain a hot rolled plate with a thickness of 2.0 to 2.5 mm.
5. The method for preparing non-oriented silicon steel according to claim 1, characterized in that: In the annealing process, annealing is performed in a continuous annealing furnace, and an insulating coating is coated on the surface of the non-oriented silicon steel strip after annealing, and the oxygen content in the annealing furnace is controlled to be ≤20ppm.
6. The method for preparing non-oriented silicon steel according to claim 1, characterized in that: In the annealing process, the protective atmosphere in the annealing furnace is a mixed gas of N2 and H2, wherein the volume fraction of H2 is ≤60%; or, the protective atmosphere in the annealing furnace is pure N2.
7. A non-oriented silicon steel, characterized in that: The non-oriented silicon steel is prepared by the method for preparing the non-oriented silicon steel as described in any one of claims 1 to 6.