Iron-based amorphous nanocrystalline strip, magnetic core and preparation method of iron-based amorphous nanocrystalline strip

By adjusting the composition and heat treatment process of amorphous nanocrystalline magnetic cores with high magnetic permeability and anti-DC biasing capabilities, the performance attenuation of existing magnetic cores under high DC component power conditions is solved. The problem has realized the need to miniaturize and lightweight electronic components.

CN119069199APending Publication Date: 2024-12-03ADVANCED TECHNOLOGY & MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411369506.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing filtered magnetic cores have insufficient anti-DC biasing ability under high DC component power conditions, resulting in premature saturation of the magnetic cores of inductive components and cannot meet the needs of miniaturization and lightweight electronic components.

Method used

By adjusting the composition and heat treatment process of the amorphous nanocrystalline strip, an iron-based amorphous nanocrystalline strip and magnetic core are developed to improve its magnetic permeability and anti-DC biasing ability. Fe100-a-b-c-d-e-fMaCubM'cSidAe alloy is used. And improve the performance of the magnetic core through magnetic field heat treatment.

Benefits of technology

It realizes the high permeability and high anti-DC bias capability of the magnetic core under high DC component conditions, meets the needs of miniaturization and lightweighting of electronic components, and improves inductance consistency and adapts to modern power environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069199A_ABST
    Figure CN119069199A_ABST
Patent Text Reader

Abstract

The invention relates to an iron-based amorphous nanocrystalline strip, a magnetic core and a preparation method of the iron-based amorphous nanocrystalline strip, and belongs to the technical field of power electronic materials. The nanocrystalline strip and the magnetic core comprise alloys of the following elements in atomic percentage: Fe100-a-b-c-d-e-fMaCubM'cSidAeDf, M is one or two of Co or Ni elements, M'is one or more of Nb, Mo or V elements, A is one or more of B, P or C elements, D is one or two of Mn or Cr elements, c is one or more of Co, Ni, Mo, and V, and f is one or more of Co, Mo, V, B, P, and C; the atomic ratios are as follows: 0 < = a < = 0.5, 0.5 < = b < = 1.2, 1 < = c < = 3.5, 10 < = d < = 15, 6.5 < = e < = 10, 0 < = f < = 2.5, a and f are not both 0, and the total atomic ratio of Fe + M is not less than 73. The nanocrystalline strip and the magnetic core have high magnetic conductivity and high direct current resistance, are mainly applied to the field of power electronics, and are particularly suitable for high-frequency and high-direct-current-content working conditions, and the magnetic core can meet the requirements of low inductance attenuation and good consistency under the high-direct-current-content working conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of power electronic materials, and in particular relates to an iron-based amorphous nanocrystalline strip, a magnetic core and a preparation method thereof. Background Art

[0002] Amorphous nanocrystalline soft magnetic materials have high saturation magnetic induction intensity, high magnetic permeability, low coercive force and good process modulation. Since its discovery, it has been widely used in the field of power electronics. Under the same operating frequency and working magnetic field, it has a higher impedance, which can reduce the cost of electronic components and help miniaturize and lighten electronic components. With the continuous promotion of green electricity, green energy represented by photovoltaic power generation and wind power generation, while saving energy and reducing consumption, due to the difference between its power generation principle and the traditional power generation principle, the power it generates has more DC components, causing grid pollution. Traditional filter inductors work under high DC component power conditions. Due to the bias magnetic field generated by the DC component, the inductance of the inductor element is reduced, the magnetic core is saturated prematurely, and the inductor element loses its function. The filter core produced by traditional inductor materials solves this problem by reducing the magnetic permeability, but at the same time it will cause the overall size and weight of the inductor element to become larger, which is contrary to the development direction of electronic components.

[0003] In order to improve the ability of the magnetic core to resist DC bias, predecessors have mostly adopted technical solutions such as magnetic powder core or ferrite powder core, amorphous cut magnetic core, amorphous + nanocrystalline composite magnetic core, etc., by reducing the magnetic permeability of the magnetic core to improve the ability to resist DC bias. Patent CN104795195A discloses a method for preparing an iron silicon aluminum magnetic core. Although the magnetic core has a good DC bias resistance effect, its effective magnetic permeability μr is only 140, which cannot meet the requirements of large inductance working conditions. Patent CN115132479A discloses a magnetic core made of amorphous + nanocrystalline dual alloy material. It has high magnetic permeability and a certain ability to resist DC bias. However, during the implementation of this technical solution, two types of materials need to be used in combination, and the production efficiency is low.

[0004] In summary, there are currently two commonly used solutions for filter cores with high DC bias resistance. The first is to use low permeability powder cores or ferrite cores, but this solution results in too low product inductance. To ensure the filtering effect, the core size needs to be increased, which leads to problems such as increased weight, increased cost, and reduced application convenience. The second is to use nanocrystalline cores with air gaps to reduce their permeability, which results in the same result as powder cores or ferrite cores.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention intends to improve the ability of the filter core to resist DC bias and improve the inductance consistency by adjusting the composition of the nanocrystalline strip and the heat treatment process of the nanocrystalline core, thereby adapting to the current power environment and providing a more optimized filter core solution.

[0007] Therefore, the present invention aims to provide an iron-based amorphous nanocrystalline strip, a magnetic core and a preparation method thereof. One of the purposes is to provide a nanocrystalline magnetic core with high resistance to DC bias, which can have high magnetic permeability and high linearity while working under high DC component conditions, thereby meeting the needs of miniaturization and lightweight use of electronic components.

[0008] The technical problem to be solved by the present invention is to obtain a strip and a nanocrystalline magnetic core having both high magnetic permeability and high DC bias resistance by adjusting the composition of amorphous nanocrystalline strips and the heat treatment process of amorphous nanocrystalline magnetic cores, and to provide a preparation process of the strip and the magnetic core. This solves the problem of performance attenuation of amorphous nanocrystalline magnetic cores working under high DC components, and the problem of increased size and weight of inductor components caused by the use of magnetic powder cores and ferrites.

[0009] The technical solution of the present invention is as follows:

[0010] In a first aspect, an iron-based amorphous nanocrystalline strip comprises an alloy having an atomic percentage of elements as shown in formula (I): Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I)

[0011] Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements;

[0012] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73.

[0013] Further, the atomic ratios are: 0<a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0<f≤2.5, a and f are not 0, and the remainder is iron; further, the atomic ratios are: 0.4≤a≤0.5, 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, 1.2≤f≤2, and the remainder is iron; further, the atomic ratios are: a=0.5, b=1.0, c=3.0, d=13, e=8, f=1.5, and the remainder is iron.

[0014] Alternatively, the atomic ratios are: 0<a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, f is 0, and the remainder is iron; further, the atomic ratios are: 0.4≤a≤0.5, 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, and the remainder is iron; further, the atomic ratios are: a=0.5, b=1.0, c=3.0, d=13, e=8, f=0, and the remainder is iron;

[0015] Alternatively, the atomic ratios are: 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0<f≤2.5, a is 0, and the remainder is iron; further, the atomic ratios are: 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, 1.2≤f≤2, and the remainder is iron; further, the atomic ratios are: a=0, b=1.0, c=3.0, d=13, e=8, f=1.5, and the remainder is iron.

[0016] Furthermore, the initial crystallization temperature of the iron-based amorphous nanocrystalline ribbon is: the starting temperature is 490-495°C, and the peak temperature is 510-520°C;

[0017] and / or, the iron-based amorphous nanocrystalline strip has a thickness of 8 to 26 micrometers, a width of 2 to 200 millimeters, and a lamination coefficient of ≥80%;

[0018] And / or, the iron-based amorphous nanocrystalline strip is subjected to 30 consecutive thickness tests every 1 meter in the length direction, and the maximum thickness range is ≤ 2 microns;

[0019] And / or, the iron-based amorphous nanocrystalline strip is continuously tested at intervals of 5 mm in the width direction, and the number of test points varies according to the width of the strip, so that the thickness range of the continuous test points is ≤ 2 μm;

[0020] And / or, the iron-based amorphous nanocrystalline strip has a width tolerance of ≤0.2 mm.

[0021] In a second aspect, a method for preparing an iron-based amorphous nanocrystalline ribbon comprises the following steps:

[0022] 2) According to Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The raw materials are mixed according to the alloy composition, and the raw materials are remelted to obtain molten steel;

[0023] Alloy Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f In the formula, M is one or both of Co and Ni, M' is one or both of Nb, Mo or V, A is one or both of B, P or C, and D is one or both of Mn or Cr;

[0024] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73;

[0025] 2) The molten steel obtained in 1) is processed into a strip by a single-roller rapid quenching method to obtain an iron-based amorphous nanocrystalline strip.

[0026] Further, the iron-based amorphous nanocrystalline ribbon is the iron-based amorphous nanocrystalline ribbon described in the first aspect;

[0027] and / or, in step 1), the pouring temperature of the molten steel is ≤1450°C; and / or, the mass fraction of Al in the molten steel is ≤0.002%, the mass fraction of Ti is ≤0.03%, and O is less than 20ppm;

[0028] And / or, in step 2), the temperature of the molten steel for strip making is 1100-1350°C; preferably, the temperature of the molten steel for strip making is 1150-1320°C.

[0029] In a third aspect, an iron-based amorphous nanocrystalline magnetic core is prepared by an iron-based amorphous nanocrystalline strip, wherein the iron-based amorphous nanocrystalline strip comprises an alloy having an atomic percentage content of elements as shown in formula (I): Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I)

[0030] Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements;

[0031] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73.

[0032] Further, the iron-based amorphous nanocrystalline ribbon is the iron-based amorphous nanocrystalline ribbon described in the first aspect, or the iron-based amorphous nanocrystalline ribbon prepared by the preparation method described in the second aspect;

[0033] And / or, the iron-based amorphous nanocrystalline magnetic core has high magnetic permeability and high DC resistance: μ r @20kHz, 0A / m≥50000; μ r @20kHz, 5A / m≥40000; μ r @20kHz, 10A / m≥15000.

[0034] In a fourth aspect, a method for preparing an iron-based amorphous nanocrystalline magnetic core comprises the following steps:

[0035] 1) Winding an iron-based amorphous nanocrystalline strip into a magnetic core, wherein the iron-based amorphous nanocrystalline strip comprises an alloy having an atomic percentage of elements as shown in formula (I): Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I)

[0036] Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements;

[0037] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73;

[0038] 3) subjecting the magnetic core obtained in step 1) to heat treatment, wherein the heat treatment comprises a temperature rising section, a temperature keeping section and a temperature falling section, wherein the temperature of the temperature keeping section is higher than the crystallization starting temperature.

[0039] Furthermore, the iron-based amorphous nanocrystalline ribbon is the iron-based amorphous nanocrystalline ribbon described in the first aspect, or the iron-based amorphous nanocrystalline ribbon prepared by the preparation method described in the second aspect, or the magnetic core is the iron-based amorphous nanocrystalline magnetic core described in the third aspect.

[0040] Furthermore, the heat treatment includes general heat treatment and magnetic field heat treatment, preferably magnetic field heat treatment; further, the magnetic field heat treatment is transverse magnetic field heat treatment, that is, the direction of the applied magnetic field is parallel to the width direction of the strip.

[0041] The present invention relates to an iron-based amorphous nanocrystalline strip, a magnetic core and a preparation method thereof. The iron-based amorphous nanocrystalline strip and the magnetic core have high magnetic permeability and high DC resistance, and are mainly used in the field of power electronics, especially in high-frequency and high DC content working conditions. Under high DC content working conditions, the magnetic core has reduced inductance decay and good consistency. Compared with the prior art, the present invention has the following beneficial effects:

[0042] 1. The iron-based amorphous nanocrystalline strip of the present invention has excellent electromagnetic properties. At the same time, the material allows industrial long-term continuous preparation and has stable quality.

[0043] 2. The iron-based amorphous nanocrystalline strip of the present invention is tested for thickness at 30 points every 1 meter in the length direction, and the maximum thickness range is ≤2 microns. In the width direction, continuous testing is performed at intervals of 5 mm, and the number of test points varies according to the width of the strip, which can meet the requirement of a thickness range of ≤2 microns at continuous testing points. The strip width is 2-200 mm, and the width tolerance is ≤0.2 mm. The strip thickness can meet the requirement of 8-26 microns. The strip lamination coefficient is ≥80%.

[0044] 3. The magnetic core prepared by the iron-based amorphous nanocrystalline strip of the present invention has high magnetic permeability and high DC bias resistance. By adjusting the strip alloy composition and the core heat treatment process, especially the composition adjustment, based on FeCu b M' c Si d A e Alloy, M (Co, Ni) and D (Mn, Cr) elements are optionally added to improve the magnetic permeability and DC bias resistance of the strip, thereby improving the DC bias resistance of the filter core and improving the inductance consistency. It can adapt to the current power environment and work under high DC component conditions while having high magnetic permeability and high linearity, thereby meeting the use requirements of miniaturization and lightweight of electronic components.

[0045] 4. The iron-based amorphous nanocrystalline strip and its preparation method of the present invention have low requirements for preparation conditions and a simple method. The hundred-kilogram-level gravity strip production equipment, hundred-kilogram-level pressure strip production equipment, ton-level gravity production equipment, and other types of amorphous nanocrystalline strip production equipment currently used in industrial production can be used to produce the above-mentioned strip.

[0046] 5. The iron-based amorphous nanocrystalline magnetic core of the present invention has high magnetic permeability and high DC resistance: μ r @20kHz, 0A / m≥50000; μ r @20kHz, 5A / m≥40000; μ r @20kHz, 10A / m≥15000.

[0047] 6. The preparation process of the iron-based amorphous nanocrystalline magnetic core of the present invention can meet the equipment requirements for the current industrial production of magnetic cores, has the conditions for mass production, and can maintain stable product quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 It is the process curve diagram of heat treatment scheme 1;

[0049] Figure 2 This is the process curve diagram of heat treatment scheme 2;

[0050] The unit of the vertical axis temperature is: ℃; the unit of the horizontal axis time is: min, and the unit length is 30min. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0052] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0053] In the present invention, unless otherwise specified and / or described, all values ​​involving content are "atomic percentages" from beginning to end. The process parameters of the following examples without specific conditions are usually based on conventional conditions. The raw materials described in the following examples can all be obtained from public commercial channels.

[0054] The present invention provides an iron-based amorphous nanocrystalline ribbon with high magnetic permeability and high DC resistance, a magnetic core and a preparation method thereof. The iron-based amorphous nanocrystalline ribbon of the present invention has excellent electromagnetic properties, and the ribbon allows industrial long-term continuous preparation with stable quality.

[0055] According to the first aspect of the present invention, the present invention provides an iron-based amorphous nanocrystalline strip with high magnetic permeability and high DC resistance, and the specific technical scheme is as follows:

[0056] An iron-based amorphous nanocrystalline strip, comprising an alloy having an atomic percentage content of elements as shown in formula (I): Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I)

[0057] Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements;

[0058] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73.

[0059] The iron-based amorphous nanocrystalline ribbon of the present invention has the following characteristics or advantages: (1) It has excellent electromagnetic properties, high magnetic permeability, and high resistance to direct current bias.

[0060] (2) In the longitudinal direction, continuous 30-point thickness testing is performed every 1 meter to ensure that the maximum thickness deviation is ≤ 2 microns.

[0061] (3) In the width direction of the strip, continuous testing is performed at intervals of 5 mm. The number of test points varies according to the width of the strip, and the thickness range of the continuous test points can be ≤ 2 μm.

[0062] (4) Strip width is 2-200 mm, and the width tolerance is ≤0.2 mm.

[0063] (5) The strip thickness can be 8-26 microns.

[0064] (6) Strip lamination coefficient ≥ 80%.

[0065] (7) The preparation conditions of the strips are low. The 100-kilogram-class gravity strip making equipment, 100-kilogram-class pressure strip making equipment, ton-class gravity production equipment, and other types of amorphous nanocrystalline strip production equipment currently used in industrial production can all be used to produce the above-mentioned strips.

[0066] The component system of traditional nanocrystalline materials is five elements: Fe, Si, B, Cu, and Nb. The performance adjustment of nanocrystalline strips is often achieved by adjusting the content of these five elements to change the performance. In order to reduce the magnetic permeability of nanocrystalline strips and provide better linearity, the purpose of reducing the magnetic permeability of the strips can be achieved by adding Ni and Co elements to the above component system, but it will lead to low inductance of magnetic rings of the same size, which does not meet the requirements of filtering and noise reduction. The iron-based amorphous nanocrystalline strip of the present invention first optimizes the alloy composition to improve the ability of the filter core to resist DC bias and improve the consistency of inductance, thereby adapting to the current power environment and providing a more optimized filter core solution.

[0067] Among the alloy components, Fe, Co, and Ni are ferromagnetic elements and are the main carriers of the magnetism of iron-based amorphous and nanocrystalline strips. A relatively high total content of Fe, Co, and Ni elements is an important guarantee for the amorphous nanocrystalline strips to have a high saturation magnetic flux density value, in order to ensure that the saturation magnetic flux density of the nanocrystalline strips described in the present invention is similar to that of the traditional nanocrystalline strips, so as to prevent the magnetic core from being easily saturated due to the low saturation magnetic flux density. At the same time, the addition of Co and Ni elements will increase the complexity of the total component system and improve the fluidity of the molten steel. In summary, in the alloy component system designed by the present invention, the total amount of Fe+M atomic ratio is not less than 73%.

[0068] A (B, P, C) elements are amorphous forming elements, and their content is controlled to be 6.5≤e≤10. When the content is less than 6.5, the amorphous forming ability is poor, the strip is not easy to form during the preparation process, the strip is seriously broken, and the prepared strip is prone to surface crystallization, which deteriorates the soft magnetic properties. When the content is higher than 10, the content of other elements will be reduced, resulting in a decrease in the saturation magnetic induction intensity of the alloy.

[0069] Si is also an amorphous element, which improves the amorphous forming ability of the alloy. In particular, Si can reduce the melting point of the alloy and is a core element for improving the processability of the nanocrystalline alloy system. Its atomic ratio is controlled at: 10.0≤d≤15.0.

[0070] In the nanocrystalline component system, the Cu element provides a nucleation site for rapid nucleation during the heat treatment of nanocrystalline strips and is an indispensable element in the nanocrystalline alloy system. Its atomic proportion is controlled at 0.5-1.2%, which can ensure that a sufficient number of α-Fe nanocrystals are formed during the heat treatment process. In the embodiment of the present invention, when the Cu element exceeds 1.2, the content of other elements will decrease.

[0071] The main function of the M' (Nb, Mo, V) element is to prevent the growth of the nucleated nano-sized grains to obtain an excellent amorphous + nanocrystalline dual-phase coupling effect. In the present invention, the total atomic content of Nb+Mo+V is controlled at 1-3.5%.

[0072] Studies have shown that the addition of D (Mn, Cr) elements can stabilize the state of magnetic domains and reduce the energy intensity of the magnetic domain pinning field after magnetic field heat treatment, so that when the magnetic chips are affected by an external magnetic field, the magnetic domain rotation requires less energy and has lower losses, thereby improving the material's magnetic permeability and ability to resist DC bias.

[0073] The iron-based amorphous nanocrystalline strip of the present invention is mainly prepared by b M' c Si d A e On the basis of the alloy, M and D are optionally added to improve the magnetic permeability and DC bias resistance of the strip. During the research and development process, the inventor found that, on the one hand, when the D element is not added and only the M element is added to optimize the alloy, when Co and Ni are optionally added, for the simultaneous improvement of magnetic permeability and DC bias resistance under high working magnetic field, when magnetic field heat treatment is performed, the effect of Ni added alone is better than the effect of Co and Ni added at the same time, and when general heat treatment is performed, that is, heat treatment is performed without adding a magnetic field, the effect of Ni added alone is equivalent to the effect of Co and Ni added at the same time. On the other hand, when the M element is not added and only the D element is added to optimize the alloy, for the simultaneous improvement of magnetic permeability and DC bias resistance under high working magnetic field, its effect is better than the effect of adding only the M element, even the effect after general heat treatment is better than the effect of adding only the M element and performing magnetic field heat treatment; in addition, the effect of using Mn element alone as the D element is equivalent to the effect of adding Co and Cr as the M element and adding Cr as the D element, and is better than the effect of adding Co and Mn as the D element, especially after magnetic field heat treatment. When D and M elements are added simultaneously for optimization, the Co+Cr combination has a better improvement effect on the magnetic permeability and DC bias resistance under high working magnetic fields than the Co+Mn combination.

[0074] Therefore, as an optional embodiment of the iron-based amorphous nanocrystalline strip of the present invention, the atomic ratios are: 0<a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0<f≤2.5, a and f are not 0, and the remainder is iron; further, the atomic ratios are: 0.4≤a≤0.5, 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, 1.2≤f≤2, and the remainder is iron; further, the atomic ratios are: a=0.5, b=1.0, c=3.0, d=13, e=8, f=1.5, and the remainder is iron;

[0075] Alternatively, the atomic ratios are: 0<a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, f is 0, and the remainder is iron; further, the atomic ratios are: 0.4≤a≤0.5, 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, and the remainder is iron; further, the atomic ratios are: a=0.5, b=1.0, c=3.0, d=13, e=8, f=0, and the remainder is iron;

[0076] Alternatively, the atomic ratios are: 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0<f≤2.5, a is 0, and the remainder is iron; further, the atomic ratios are: 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, 1.2≤f≤2, and the remainder is iron; further, the atomic ratios are: a=0, b=1.0, c=3.0, d=13, e=8, f=1.5, and the remainder is iron.

[0077] As an optional implementation of the iron-based amorphous nanocrystalline ribbon of the present invention, the initial crystallization temperature of the iron-based amorphous nanocrystalline ribbon is: the starting temperature is 490-495°C, and the peak temperature is 510-520°C.

[0078] According to a second aspect of the present invention, a method for preparing an iron-based amorphous nanocrystalline ribbon, that is, the method for preparing an iron-based amorphous nanocrystalline ribbon according to the first aspect, comprises the following steps:

[0079] 1) According to Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The raw materials are mixed according to the alloy composition, and the raw materials are remelted to obtain molten steel;

[0080] Alloy Fe 100-a-b-c-d-e-f M a Cub M' c Si d A e D f In the formula, M is one or both of Co and Ni, M' is one or both of Nb, Mo or V, A is one or both of B, P or C, and D is one or both of Mn or Cr;

[0081] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73;

[0082] 2) The molten steel obtained in 1) is processed into a strip by a single-roller rapid quenching method to obtain an iron-based amorphous nanocrystalline strip.

[0083] The strip preparation process of the present invention has low requirements, can meet the equipment requirements for the current industrial production of nanocrystalline strips, has batch production conditions, and can maintain stable strip quality. Specifically, the 100-kilogram-level gravity strip production equipment, 100-kilogram-level pressure strip production equipment, ton-level gravity production equipment, and other types of amorphous nanocrystalline strip production equipment currently used in industrial production can all be used for production.

[0084] The strip preparation process of the present invention has a strip with a width of 2-200 mm, a width tolerance of ≤0.2 mm, a thickness of 8-26 μm, and a strip lamination of ≥80%. In the length direction, 30 consecutive thickness tests are performed every 1 meter, which can satisfy a maximum thickness range of ≤2 μm. In the width direction, continuous tests are performed every 5 mm, and the number of test points varies according to the width of the strip, which can satisfy a thickness range of ≤2 μm at consecutive test points.

[0085] As an optional implementation of the method for preparing the iron-based amorphous nanocrystalline strip of the present invention, in step 1), the pouring temperature of the molten steel is ≤1450°C;

[0086] And / or, the mass fraction of Al in the molten steel is ≤0.002%, the mass fraction of Ti is ≤0.03%, and O is less than 20 ppm.

[0087] In the present invention, the single-roller rapid quenching method is also called a single-plane flow casting method. The implementation of this method can be achieved through existing technical equipment, such as the aforementioned strip production equipment, which will not be elaborated here one by one. As an optional embodiment, the cooling roller of the single-plane flow casting method includes a water inlet channel and a water outlet channel, a plurality of water inlet outlets are arranged in the vertical direction of the water inlet channel, a plurality of water outlet outlets are arranged in the vertical direction of the water outlet channel, and the water inlet outlet and the water outlet outlet are connected through a cooling water trough; further, the thermal conductivity of the cooling roller is 130-250W / mK, preferably, the thermal conductivity of the cooling roller is 200-250W / mK; the inlet water temperature of the cooling roller is 20-35°C, and the temperature difference between the inlet water temperature and the outlet water temperature is ≤4°C; preferably, the inlet water temperature of the cooling roller is 23-30°C, and the temperature difference between the inlet water temperature and the outlet water temperature is ≤2°C; the cooling roller rotation speed is 18-30m / s; preferably, the cooling roller rotation speed is 23-28m / s.

[0088] As an optional implementation of the method for preparing the iron-based amorphous nanocrystalline strip of the present invention, in step 2), the temperature of the molten steel for making the strip is 1100-1350°C; preferably, the temperature of the molten steel for making the strip is 1150-1320°C.

[0089] According to a third aspect of the present invention, an iron-based amorphous nanocrystalline magnetic core is prepared by an iron-based amorphous nanocrystalline strip, wherein the iron-based amorphous nanocrystalline strip comprises an alloy having an atomic percentage of elements as shown in formula (I): Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I)

[0090] Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements;

[0091] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73.

[0092] That is, the iron-based amorphous nanoscale magnetic core described in the third aspect is a magnetic core prepared from the iron-based amorphous nanocrystalline strip described in the first aspect or the iron-based amorphous nanocrystalline alloy strip prepared by the preparation method described in the second aspect.

[0093] The magnetic core of the present invention has high magnetic permeability and high DC resistance: μr @20kHz, 0A / m≥50000; μ r @20kHz, 5A / m≥40000; μ r @20kHz, 10A / m≥15000.

[0094] In the present invention, μ r It is the relative magnetic permeability, which is equivalent to the effective magnetic permeability, so it is also the effective magnetic permeability.

[0095] According to a fourth aspect of the present invention, a method for preparing an iron-based amorphous nanocrystalline magnetic core comprises the following steps:

[0096] 1) Winding an iron-based amorphous nanocrystalline strip into a magnetic core, wherein the iron-based amorphous nanocrystalline strip comprises an alloy having an atomic percentage of elements as shown in formula (I): Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I)

[0097] Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements;

[0098] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73;

[0099] 2) subjecting the magnetic core obtained in step 1) to heat treatment, wherein the heat treatment comprises a temperature rising section, a temperature keeping section and a temperature falling section, wherein the temperature of the temperature keeping section is higher than the crystallization starting temperature.

[0100] As an optional embodiment of the method for preparing the iron-based amorphous nanocrystalline magnetic core of the present invention, the heat treatment includes general heat treatment and magnetic field heat treatment, preferably magnetic field heat treatment. Further, the magnetic field heat treatment is a transverse magnetic field heat treatment, that is, the direction of the applied magnetic field is parallel to the width direction of the strip.

[0101] Studies have shown that different heat treatment systems have a greater impact on the amorphous + nanocrystalline dual-phase coupling structure after heat treatment, which in turn affects the magnetic domain structure. Different heat treatment temperatures and magnetic field application methods have a greater impact on the magnetic permeability and DC bias resistance of materials and magnetic cores. The present invention obtains magnetic cores with different magnetic permeabilities and DC bias resistance by adjusting different heat treatment systems and magnetic field application methods. As an optional embodiment, the method for preparing the iron-based amorphous nanocrystalline magnetic core includes the following steps:

[0102] 1) According to the nanocrystalline ribbon provided in the first aspect, the nanocrystalline ribbon is wound into a magnetic core. According to the DSC test results, a heat treatment scheme is designed, which includes a heating section, a heat preservation section and a cooling section. According to the performance modulation principle of the nanocrystalline ribbon and the DSC test results, a heat treatment is performed, and specifically, a magnetic field heat treatment (heat treatment scheme 1) or a general heat treatment (heat treatment scheme 2) can be selected.

[0103] 2) The heating stage of the heat treatment process may include multiple stages with different temperatures, the temperature difference between the connected stages is ≥15°C, and the insulation time of each stage is 10-70min. The highest temperature of the heating stage is less than the highest temperature of the insulation stage, and the difference is greater than 20°C. Specifically, Figure 1 , 2 As shown, the temperature rising section contains a stage, the highest temperature of the stage is 400°C, and the holding time is 65min.

[0104] 3) The temperature of the insulation section is higher than the crystallization starting temperature, the difference is greater than 25°C, and lower than 60°C. The initial crystallization starting temperature is 490-495°C, and the peak temperature is 510-520°C.

[0105] Preferably, the temperature of the insulation section is higher than the crystallization starting temperature, the difference is greater than 30°C, and is not higher than 70°C.

[0106] Specifically, Figure 1 , 2 As shown, the temperature of the insulation section is 560°C, and the insulation time is 70 minutes, which is higher than the highest temperature of 400°C in the heating section, with a difference of 160°C. It is also higher than the crystallization starting temperature of 490-495°C, with a difference of 65-70°C.

[0107] 4) The temperature reduction section is from the end of the heat preservation section to the furnace discharge temperature, the furnace discharge temperature is less than 200°C, preferably, the furnace discharge temperature is less than 100°C.

[0108] 5) The magnetic field heat treatment described above applies a transverse magnetic field, and the application time starts from when the furnace temperature is increased to 400° C. until the magnetic core is taken out of the furnace.

[0109] Preferably, the magnetic field is applied from the time the furnace temperature is raised to 400° C. to the end of the core insulation period.

[0110] The magnetic field heat treatment has a magnetic field strength of 200-1500 GS, preferably 400-1200 GS.

[0111] The thickness of the nanocrystalline ribbon of the present invention is 8-26 microns, the width of the ribbon is 2-200 millimeters, and the lamination is greater than 80%. r@20kHz, 0A / m≥55000; μ r @20kHz, 5A / m≥40000; μ r @20kHz, 10A / m≥15000, with high magnetic permeability and high DC resistance. With the continuous deepening of new energy grid connection, the continuous increase in the market share of new energy vehicles, and the increasingly complex electromagnetic environment in other application fields. The strip and magnetic core described in the present invention have very broad application prospects. The preparation process of the strip and magnetic core described in the present invention can meet the current equipment requirements for the industrial production of nanocrystalline strips and magnetic cores, have mass production conditions, and can maintain stable product quality.

[0112] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0113] The methods for preparing the iron-based amorphous nanocrystalline ribbon and magnetic core in the embodiments of the present invention and the comparative examples are as follows:

[0114] 1) The alloy components of the embodiments and comparative examples were prepared.

[0115] Wherein, the embodiment is according to Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The alloy is prepared, wherein M is one or two of Co or Ni elements, M' is one or more of Nb, Mo or V elements, A is one or more of B, P or C elements, and D is one or two of Mn or Cr elements;

[0116] The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73.

[0117] The specific alloy ingredients of each embodiment and comparative example can be seen in Table 1, which is as follows:

[0118] Table 1 Alloy composition and heat treatment process system of each embodiment and comparative example

[0119] project Alloy composition Heat treatment process system Example 1 <![CDATA[Fe 74.5 (NiCo) 0.5 Yes 13 B8Cu1Nb3]]> Heat treatment solution 1 Example 2 <![CDATA[Fe 74.5 (NiCo) 0.5 Yes 13 B8Cu1Nb3]]> Heat treatment solution 2 Example 3 <![CDATA[Fe 74.5 In 0.5 To 13 B8Cu1Nb3]]> Heat treatment solution 1 Example 4 <![CDATA[Fe 74.5 In 0.5 To 13 B8Cu1Nb3]]> Heat treatment solution 2 Example 5 <![CDATA[Fe 73 What 0.5 You 13 B8Cu1Nb3Mn 1.5 ]]> Heat treatment solution 1 Example 6 <![CDATA[Fe 73 What 0.5 You 13 B8Cu1Nb3Mn 1.5 ]]> Heat treatment solution 2 Example 7 <![CDATA[Fe 73 What 0.5 You 13 B8Cu1Nb3Cr 1.5 ]]> Heat treatment solution 1 Example 8 <![CDATA[Fe 73 What 0.5 You 13 B8Cu1Nb3Cr 1.5 ]]> Heat treatment solution 2 Example 9 <h2 style=";text-align:left;direction:ltr"><![CDATA[Fe <h2 style=";text-align:left;direction:ltr"> 73.5 <h2 style=";text-align:left;direction:ltr"> Yes<h2 style=";text-align:left;direction:ltr"> 13 <h2 style=";text-align:left;direction:ltr"> B8Cu1Nb3Mn<h2 style=";text-align:left;direction:ltr"> 1.5 <h2 style=";text-align:left;direction:ltr"> ]]><h2 style=";text-align:left;direction:ltr"> Heat treatment solution 1 Example 10 <h2 style=";text-align:left;direction:ltr"><![CDATA[Fe <h2 style=";text-align:left;direction:ltr"> 73.5 <h2 style=";text-align:left;direction:ltr"> Yes<h2 style=";text-align:left;direction:ltr"> 13 <h2 style=";text-align:left;direction:ltr"> B8Cu1Nb3Mn<h2 style=";text-align:left;direction:ltr"> 1.5 <h2 style=";text-align:left;direction:ltr"> ]]><h2 style=";text-align:left;direction:ltr"> Heat treatment solution 2 Comparative Example 1 <![CDATA[Fe 74 Are you 13 B9Cu1Nb3]]> Heat treatment solution 1 Comparative Example 2 <![CDATA[Fe 75 What 0.5 You 13 B6Cu 1.5 Nb3Mn 1.5 ]]> Heat treatment solution 1

[0120] 2) using a medium frequency smelting furnace to remelt raw materials with different proportions, after smelting, the mass fraction of Al in the molten steel is ≤0.002%, the mass fraction of Ti is ≤0.03%, and O is less than 20ppm, the pouring temperature is ≤1450°C and then the steel is tapped into a tundish, and after heating, insulation and quenching, a single-roller rapid quenching method is used to prepare an iron-based amorphous nanocrystalline strip with a width of 62mm and a thickness of 18-20μm, and the molten steel temperature for strip making is 1100-1350°C, preferably, the molten steel temperature for strip making is 1150-1320°C.

[0121] The raw materials include but are not limited to pure iron, metallic silicon, ferroboron, ferroniobium, ferromanganese, ferrochrome, electrolytic nickel, electrolytic cobalt, electrolytic copper, etc.;

[0122] The single-roller rapid quenching method is a single-plane flow casting method. The cooling roller of the single-plane flow casting method includes a water inlet channel and a water outlet channel. A plurality of water inlet outlets are arranged in the vertical direction of the water inlet channel, and a plurality of water outlet outlets are arranged in the vertical direction of the water outlet channel. The water inlet outlet and the water outlet outlet are connected through a cooling water trough. Further, the thermal conductivity of the cooling roller is 130-250W / mK. Preferably, the thermal conductivity of the cooling roller is 200-250W / mK. The inlet water temperature of the cooling roller is 20-35°C, and the temperature difference between the inlet water temperature and the outlet water temperature is ≤4°C. Preferably, the inlet water temperature of the cooling roller is 23-30°C, and the temperature difference between the inlet water temperature and the outlet water temperature is ≤2°C. The rotation speed of the cooling roller is 18-30m / s. Preferably, the rotation speed of the cooling roller is 23-28m / s.

[0123] 3) The iron-based amorphous nanocrystalline strip obtained in step 2) is rolled into 10 mm and rolled into a magnetic core with an outer diameter of 30 mm, an inner diameter of 20 mm and a height of 10 mm, and then Figure 1 or Figure 2 The heat treatment scheme is used to heat treat the iron-based amorphous nanocrystalline magnetic core. The specific heat treatment process system used in the embodiment and the comparative example can be seen in Table 1.

[0124] Specifically, according to the performance modulation principle of nanocrystalline ribbons and the DSC test results, the initial crystallization temperature of the ribbon is 490-495°C, and the peak temperature is 510-520°C. A heat treatment scheme is designed, and magnetic field heat treatment (heat treatment scheme 1) or general heat treatment (heat treatment scheme 2) can be selected. Both heat treatment schemes include a heating section, a heat preservation section, and a cooling section. Figure 1 , 2 As shown:

[0125] The heating stage of magnetic field heat treatment and general heat treatment contains a stage, the highest temperature of the stage is 400℃, and the holding time is 65min.

[0126] The temperature of the insulation section is 560°C, and the insulation time is 70 minutes, which is higher than the highest temperature of 400°C in the heating section, with a difference of 160°C. It is also higher than the crystallization starting temperature of 490-495°C, with a difference of 65-70°C.

[0127] The temperature reduction stage is from the end of the heat preservation stage to the furnace discharge temperature, and the furnace discharge temperature is less than 100°C.

[0128] If the magnetic field heat treatment is used, a transverse magnetic field is applied, and the application time starts from when the furnace temperature rises to 400°C until the end of the core insulation period. During the magnetic field heat treatment, the magnetic field intensity is 400-1200GS.

[0129] A more detailed description is given below, including but not limited to a description of the main differences.

[0130] Example 1

[0131] In this embodiment, Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The alloy composition is formulated.

[0132] Where M is Ni+Co, M' is Nb, A is B, a=0.5, b=1, c=3, d=13, e=8, f=0, and the rest is iron, that is, the alloy is Fe 74.5 (NiCo) 0.5 Si 13 B8Cu1Nb3;

[0133] Use a medium frequency smelting furnace to remelt raw materials such as pure iron, metallic silicon, ferroboron, ferroniobium, electrolytic nickel, electrolytic cobalt, and electrolytic copper in different proportions. After smelting, the steel is tapped into the tundish. After heating and cooling, a single-roller rapid quenching method is used to prepare an iron-based nanocrystalline strip with a width of 62mm and a thickness of 18-20μm. The nanocrystalline strip is roll-cut to 10mm and wound into a magnetic core with an outer diameter of 30mm, an inner diameter of 20mm, and a height of 10mm. This magnetic core is cut according to Figure 1 Heat treatment system for processing.

[0134] Example 2

[0135] Take the nanocrystalline ribbon prepared in Example 1, roll cut the nanocrystalline ribbon into 10 mm pieces, and roll it into a magnetic core with an outer diameter of 30 mm, an inner diameter of 20 mm, and a height of 10 mm. Figure 2 Heat treatment system for processing.

[0136] Example 3

[0137] In this embodiment, Fe100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The alloy composition is formulated.

[0138] Wherein M is Ni, M' is Nb, A is B. a=0.5, b=1, c=3, d=13, e=8, f=0, and the remainder is iron.

[0139] Use a medium frequency smelting furnace to remelt raw materials such as pure iron, electrolytic nickel, metallic silicon, ferroboron, ferroniobium, and electrolytic copper in different proportions. After smelting, the steel is tapped into the tundish. After heating and cooling, a single-roller rapid quenching method is used to prepare an iron-based nanocrystalline strip with a width of 62mm and a thickness of 18-20μm. The nanocrystalline strip is roll-cut to 10mm and wound into a magnetic core with an outer diameter of 30mm, an inner diameter of 20mm, and a height of 10mm. This magnetic core is placed according to Figure 1 Heat treatment system for processing.

[0140] Example 4

[0141] Take the nanocrystalline ribbon prepared in Example 3, roll cut the nanocrystalline ribbon into 10 mm pieces, and roll it into a magnetic core with an outer diameter of 30 mm, an inner diameter of 20 mm, and a height of 10 mm. Figure 2 Heat treatment system for processing.

[0142] Example 5

[0143] In this embodiment, Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The alloy composition is formulated.

[0144] Wherein M is Co, M' is Nb, A is B, D is Mn, a=0.5, b=1, c=3, d=13, e=8, f=1.5, and the remainder is iron.

[0145] Use a medium frequency smelting furnace to remelt raw materials such as pure iron, electrolytic cobalt, metallic silicon, ferroboron, ferroniobium, electrolytic copper, and ferromanganese in different proportions. After smelting, the steel is tapped into the tundish. After heating and cooling, a single-roller rapid quenching method is used to prepare an iron-based nanocrystalline strip with a width of 62mm and a thickness of 18-20μm. The nanocrystalline strip is roll-cut to 10mm and wound into a magnetic core with an outer diameter of 30mm, an inner diameter of 20mm, and a height of 10mm. This magnetic core is placed according to Figure 1 Heat treatment system for processing.

[0146] Example 6

[0147] Take the nanocrystalline ribbon prepared in Example 5, roll cut the nanocrystalline ribbon into 10 mm pieces, and roll it into a magnetic core with an outer diameter of 30 mm, an inner diameter of 20 mm, and a height of 10 mm. Figure 2 Heat treatment system for processing.

[0148] Example 7

[0149] In this embodiment, Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The alloy composition is formulated.

[0150] Wherein M is Co, M' is Nb, A is B, D is Cr, a=0.5, b=1, c=3, d=13, e=8, f=1.5, and the remainder is iron.

[0151] Use a medium frequency smelting furnace to remelt raw materials such as pure iron, electrolytic cobalt, metallic silicon, ferroboron, ferroniobium, ferrochrome, and electrolytic copper in different proportions. After smelting, the steel is tapped into the tundish. After heating and cooling, a single-roller rapid quenching method is used to prepare an iron-based nanocrystalline strip with a width of 62mm and a thickness of 18-20μm. The nanocrystalline strip is roll-cut to 10mm and wound into a magnetic core with an outer diameter of 30mm, an inner diameter of 20mm, and a height of 10mm. This magnetic core is cut according to Figure 1 Heat treatment system for processing.

[0152] Example 8

[0153] Take the nanocrystalline ribbon prepared in Example 7, roll cut the nanocrystalline ribbon into 10 mm pieces, and roll it into a magnetic core with an outer diameter of 30 mm, an inner diameter of 20 mm, and a height of 10 mm. Figure 2 Heat treatment system for processing.

[0154] Example 9

[0155] In this embodiment, Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The alloy composition is formulated.

[0156] Wherein M' is Nb, A is B, D is Mn, a=0, b=1, c=3, d=13, e=8, f=1.5, and the remainder is iron.

[0157] Use a medium frequency smelting furnace to remelt raw materials such as pure iron, metallic silicon, ferroboron, ferroniobium, ferromanganese, and electrolytic copper in different proportions. After smelting, the steel is tapped into the tundish. After heating and keeping calm, a single-roller rapid quenching method is used to prepare an iron-based nanocrystalline strip with a width of 62mm and a thickness of 18-20μm. The nanocrystalline strip is roll-cut to 10mm and wound into a magnetic core with an outer diameter of 30mm, an inner diameter of 20mm, and a height of 10mm. This magnetic core is cut according to Figure 1 Heat treatment system for processing.

[0158] Example 10

[0159] Take the nanocrystalline ribbon prepared in Example 9, roll cut the nanocrystalline ribbon into 10 mm pieces, and roll it into a magnetic core with an outer diameter of 30 mm, an inner diameter of 20 mm, and a height of 10 mm. Figure 2 Heat treatment system for processing.

[0160] Comparative Example 1

[0161] In this comparative example 1, Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The alloy composition is formulated.

[0162] Wherein M' is Nb, A is B, a=0, b=1, c=3, d=13, e=9, f=0, and the remainder is iron.

[0163] Use a medium frequency smelting furnace to remelt raw materials such as pure iron, metallic silicon, ferroboron, ferroniobium, and electrolytic copper in different proportions. After smelting, the steel is tapped into the tundish. After heating and cooling, a single-roller rapid quenching method is used to prepare an iron-based nanocrystalline strip with a width of 62mm and a thickness of 18-20μm. The nanocrystalline strip is roll-cut to 10mm and wound into a magnetic core with an outer diameter of 30mm, an inner diameter of 20mm, and a height of 10mm. This magnetic core is cut according to Figure 1 Heat treatment system for processing.

[0164] Comparative Example 2

[0165] In this comparative example 2, Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The alloy composition is formulated.

[0166] Wherein M is Co, M' is Nb, A is B, D is Mn, a=0.5, b=1.5, c=3, d=13, e=6, f=1.5, and the rest is iron.

[0167] Use a medium frequency smelting furnace to remelt raw materials such as pure iron, metallic silicon, ferroboron, ferroniobium, and electrolytic copper in different proportions. After smelting, the steel is tapped into the tundish. After heating and keeping calm, a single-roller rapid quenching method is used to prepare an iron-based nanocrystalline strip with a width of 62mm and a thickness of 18-20μm. The strip cannot be formed continuously during the preparation process. The nanocrystalline strip is roll-sheared to 10mm. The strip breaks severely during the roll-shearing process and is wound into a magnetic core with an outer diameter of 30mm, an inner diameter of 20mm, and a height of 10mm. This magnetic core is made according to Figure 1 Heat treatment system for processing.

[0168] Testing and result analysis

[0169] The iron-based amorphous nanocrystalline magnetic cores obtained in Examples 1-10 and Comparative Examples 1-2 were subjected to inductance tests under the conditions of Table 2 (i.e., 0 A / m, 5 A / m, and 10 A / m at 20 kHz) using an inductance test device of model Agilent 4284A with DC bias test capability. The effective magnetic permeability was obtained according to the inductance and effective magnetic permeability conversion formula: μ r =Lle / (N 2 Ae), where μ r is the effective magnetic permeability; L is the inductance; N is the number of coil turns; Ae is the effective magnetic path cross-sectional area; le is the effective magnetic path length.

[0170] The results are shown in Table 2:

[0171] Table 2 Core performance of each embodiment and comparative example

[0172]

[0173]

[0174] By comparing Example 1 with Example 2, as well as comparing Example 3 with Example 4, as well as comparing Example 5 with Example 6, as well as comparing Example 7 with Example 8, and comparing Example 8 with Example 9, it can be found that the heat treatment process system of applying a transverse magnetic field during the heat treatment process adopted in Example 1, Example 3, Example 5, Example 7, and Example 9 can effectively improve the magnetic permeability under high external magnetic field conditions at the same frequency.

[0175] By comparing Examples 1-4 with Comparative Example 1, it can be found that under the same composition system, the addition of Co and Ni elements can reduce the magnetic permeability under the same frequency and low working magnetic field, but can increase the magnetic permeability under the same frequency and high working magnetic field. Further, by comparing Examples 1-4, it can be found that when only M element is added without adding D element, when Co and Ni are optionally added, for the simultaneous improvement of magnetic permeability and DC bias resistance under high working magnetic field, when magnetic field heat treatment is performed, the effect of Ni added alone is better than the effect of Co and Ni added at the same time, and when general heat treatment is performed, that is, heat treatment is performed without adding a magnetic field, the effect of Ni added alone is equivalent to the effect of Co and Ni added at the same time.

[0176] By comparing Comparative Example 1 with Examples 5-10, it can be found that the addition of Mn and Cr elements can effectively improve the magnetic permeability under the same frequency and high working magnetic field. And further, by comparing Examples 5-8, it can be found that when the D element and the M element are added at the same time for optimization, the Co+Cr combination has a better improvement effect on the magnetic permeability and DC bias resistance under high working magnetic field than the Co+Mn combination, that is, in the presence of the D element, the addition of Cr can better improve the magnetic permeability under the same frequency and high working magnetic field than the addition of Mn. And by comparing Examples 9 and 10 with Examples 1-4, it can be found that when the M element is not added and only the D element is added for alloy optimization, the effect of improving the magnetic permeability and DC bias resistance under high working magnetic field is better than that of adding only the M element, and even the effect after general heat treatment is better than that of adding only the M element and performing magnetic field heat treatment. In addition, by comparing Examples 5 and 7 with Example 9, and by comparing Examples 6 and 8 with Example 10, it can be found that the effect of selecting only Mn as the D element is equivalent to the effect of adding Co as the M element and Cr as the D element at the same time, and is better than the effect of adding Co as the M element and Mn as the D element at the same time, especially after magnetic field heat treatment.

[0177] By testing the performance of the strip prepared in Comparative Example 2, it was found that r @20kHz, the magnetic permeability under 0A / m conditions is only 26,000. Further analysis of the strip shows that the surface of the strip is severely crystallized. The reason is that the Cu content exceeds the standard and the B content is low, resulting in insufficient amorphous forming ability of the material when prepared under atmospheric environment. The manifestation of insufficient amorphous forming ability is difficult preparation, poor strip toughness, broken strip during roller shearing, and low magnetic permeability. It is consistent with the process manifestation of Comparative Example 2. By comparing Comparative Example 2 with Example 5 and Comparative Example 1, it can be found that through the introduction of Co+Mn, although the magnetic permeability of the material is also reduced under the same frequency and high working magnetic field, the reduction is small, which can further illustrate the role of Co+Mn.

[0178] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.

Claims

1. An iron-based amorphous nanocrystalline strip, characterized in that: An alloy comprising the elements represented by formula (I) in atomic percentage: Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I) Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements; The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73.

2. The iron-based amorphous nanocrystalline strip according to claim 1, characterized in that: The atomic ratios are: 0<a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0<f≤2.5, a and f are not 0, and the remainder is iron; further, the atomic ratios are: 0.4≤a≤0.5, 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, 1.2≤f≤2, and the remainder is iron; further, the atomic ratios are: a=0.5, b=1.0, c=3.0, d=13, e=8, f=1.5, and the remainder is iron; Alternatively, the atomic ratios are: 0<a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, f is 0, and the remainder is iron; further, the atomic ratios are: 0.4≤a≤0.5, 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, and the remainder is iron; further, the atomic ratios are: a=0.5, b=1.0, c=3.0, d=13, e=8, f=0, and the remainder is iron; Alternatively, the atomic ratios are: 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0<f≤2.5, a is 0, and the remainder is iron; further, the atomic ratios are: 0.7≤b≤1.1, 2.5≤c≤3.5, 12≤d≤14, 7≤e≤9, 1.2≤f≤2, and the remainder is iron; further, the atomic ratios are: a=0, b=1.0, c=3.0, d=13, e=8, f=1.5, and the remainder is iron.

3. The iron-based amorphous nanocrystalline strip according to claim 1 or 2, characterized in that: The initial crystallization temperature of the iron-based amorphous nanocrystalline ribbon is: the starting temperature is 490-495°C, and the peak temperature is 510-520°C; and / or, the iron-based amorphous nanocrystalline strip has a thickness of 8 to 26 micrometers, a width of 2 to 200 millimeters, and a lamination coefficient of ≥80%; And / or, the iron-based amorphous nanocrystalline strip is subjected to 30 consecutive thickness tests every 1 meter in the length direction, and the maximum thickness range is ≤ 2 microns; And / or, the iron-based amorphous nanocrystalline strip is continuously tested at intervals of 5 mm in the width direction, and the number of test points varies according to the width of the strip, so that the thickness range of the continuous test points is ≤ 2 μm; And / or, the iron-based amorphous nanocrystalline strip has a width tolerance of ≤0.2 mm.

4. A method for preparing an iron-based amorphous nanocrystalline ribbon, characterized in that: The following steps are involved: 1) According to Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f The raw materials are mixed according to the alloy composition, and the raw materials are remelted to obtain molten steel; Alloy Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f In the formula, M is one or both of Co and Ni, M' is one or both of Nb, Mo or V, A is one or both of B, P or C, and D is one or both of Mn or Cr; The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73; 2) The molten steel obtained in 1) is processed into a strip by a single-roller rapid quenching method to obtain an iron-based amorphous nanocrystalline strip.

5. The method for preparing the iron-based amorphous nanocrystalline ribbon according to claim 4, characterized in that: The iron-based amorphous nanocrystalline strip is the iron-based amorphous nanocrystalline strip as claimed in any one of claims 1 to 3; and / or, in step 1), the pouring temperature of the molten steel is ≤1450°C; and / or, the mass fraction of Al in the molten steel is ≤0.002%, the mass fraction of Ti is ≤0.03%, and O is less than 20ppm; And / or, in step 2), the temperature of the molten steel for strip making is 1100-1350°C; preferably, the temperature of the molten steel for strip making is 1150-1320°C.

6. An iron-based amorphous nanocrystalline magnetic core, characterized in that: The iron-based amorphous nanocrystalline magnetic core is prepared by an iron-based amorphous nanocrystalline strip, wherein the iron-based amorphous nanocrystalline strip comprises an alloy having an atomic percentage content of elements as shown in formula (I): Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I) Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements; The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73.

7. The iron-based amorphous nanocrystalline magnetic core according to claim 6, characterized in that: The iron-based amorphous nanocrystalline strip is the iron-based amorphous nanocrystalline strip described in any one of claims 1 to 3, or the iron-based amorphous nanocrystalline strip prepared by the preparation method described in any one of claims 4 to 5; And / or, the iron-based amorphous nanocrystalline magnetic core has high magnetic permeability and high DC resistance: μ r @20kHz, 0A / m≥50000; μ r @20kHz, 5A / m≥40000; μ r @20kHz, 10A / m≥15000.

8. A method for preparing an iron-based amorphous nanocrystalline magnetic core, characterized in that: The following steps are involved: 1) Winding an iron-based amorphous nanocrystalline strip into a magnetic core, wherein the iron-based amorphous nanocrystalline strip comprises an alloy having an atomic percentage of elements as shown in formula (I): Fe 100-a-b-c-d-e-f M a Cu b M' c Si d A e D f (I) Wherein, M is one or both of Co and Ni elements, M' is one or both of Nb, Mo or V elements, A is one or both of B, P or C elements, and D is one or both of Mn or Cr elements; The atomic ratios are: 0≤a≤0.5, 0.5≤b≤1.2, 1≤c≤3.5, 10≤d≤15, 6.5≤e≤10, 0≤f≤2.5, a and f are not all 0, and the total atomic ratio of Fe+M is not less than 73; 2) subjecting the magnetic core obtained in step 1) to heat treatment, wherein the heat treatment comprises a temperature rising section, a temperature keeping section and a temperature falling section, wherein the temperature of the temperature keeping section is higher than the crystallization starting temperature.

9. The method for preparing an iron-based amorphous nanocrystalline magnetic core according to claim 8, characterized in that: The iron-based amorphous nanocrystalline strip is any one of the iron-based amorphous nanocrystalline strips in claims 1-3, or an iron-based amorphous nanocrystalline strip prepared by any one of the preparation methods in claims 4-5, or the magnetic core is any one of the iron-based amorphous nanocrystalline magnetic cores in claims 6-7.

10. The method for preparing the iron-based amorphous nanocrystalline magnetic core according to claim 8 or 9, characterized in that: The heat treatment includes general heat treatment and magnetic field heat treatment, preferably magnetic field heat treatment; further, the magnetic field heat treatment is transverse magnetic field heat treatment, that is, the direction of applying the magnetic field is parallel to the width direction of the strip.

Citation Information

Patent Citations

  • Sendust magnetic powder core

    CN104795195A

  • Manufacturing method of single direct-current-component-resistant magnetic core

    CN115132479A