A production method for continuous casting billet for high-grade silicon steel and the produced silicon steel continuous casting billet
By controlling the parameters of continuous casting machines and crystallizers, combined with the second cold zone electromagnetic stirring technology, the production process of high-grade silicon steel continuous casting billets is optimized, and the problems of large bulging on the narrow side and low isometric crystallization rate are solved, and the product quality is improved Continuous casting machine production avoids equipment damage.
Patent Information
- Application Number
- CN202410921455.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-10
AI Technical Summary
High-grade silicon steel continuous casting billets have problems such as large bulge on narrow side and low isometric crystallinity in the center, which affects surface quality and stability. The existing technology is difficult to effectively solve, resulting in reduced production capacity and equipment damage.
By controlling the continuous casting machine pulling speed, crystallizer water volume, second cold water volume, taper and other parameters, a reasonable design of the roller slots of the foot roller section, zero section and fan section, combined with the second cold zone electromagnetic stirring technology, the production of silicon steel continuous casting billets is optimized. Process, the bulging volume on the narrow side is less than or equal to 2mm, and the central isometric crystallinity is more than or equal to 70%.
In the absence of equipment transformation, the continuous casting machine output and product quality are improved, the narrow side bulge amount is reduced, and the central isometric crystal ratio is improved, avoiding other quality defects and equipment damage problems.
Abstract
Description
Technical Field
[0001] The invention relates to a production method of a continuous casting billet for high-grade silicon steel and the produced silicon steel continuous casting billet, belonging to the technical field of iron and steel metallurgy. Background Art
[0002] High-grade silicon steel is a widely used functional soft magnetic material. Due to its complex manufacturing process and high technical difficulty, it is mainly used in the iron core manufacturing of various motors and electrical appliances. With the improvement of automation in various industries and the development of high-efficiency motors, excellent and stable surface quality has become the development trend of this type of product. What affects the surface quality and stability of silicon steel is the quality of high-grade silicon steel continuous casting billets. At present, there are two main quality problems with high-grade silicon steel continuous casting billets, namely, large bulging on the narrow side of the continuous casting billet and low equiaxed crystal rate in the center.
[0003] Regarding the bulging problem, due to the high silicon content in high-grade silicon steel, the thermal conductivity of the matrix is poor. When the ingot shell thickness is small when it comes out of the crystallizer during the pouring process, the narrow side of the ingot will bulge under the static pressure of the molten steel, the temperature recovery and the contraction of the wide roll gap. The bulging has a great impact on the surface and internal quality of the ingot. First, due to the bulging, there must be molten steel replenished to the narrow side. The reduction of molten steel at the replenished position will cause the surface of that position to shrink, thereby causing the surface quality of that position to deteriorate, such as horizontal and vertical cracks on the surface; secondly, due to the bulging, the surface cooling of the narrow side of the ingot is uneven, and the thermal stress at the solidification front of the ingot causes internal cracks in the ingot.
[0004] In the prior art, the method to solve the bulging problem of the narrow side of the continuous casting billet is mainly to reduce the continuous casting pulling speed, so that the molten steel inside the billet can solidify quickly, accelerate the formation of the billet shell, and increase the thickness to resist the pressure brought by the middle molten steel. However, the reduction in pulling speed will lead to a reduction in the production capacity of the continuous casting machine, and due to poor thermal conductivity, the pulling speed of high-grade silicon steel is already low. Further reducing the pulling speed will cause the molten steel to be overcooled in the crystallizer, resulting in adhesion between the molten steel and the crystallizer, and damage to the copper plate of the crystallizer. For example, the application with publication number CN101992275A adopts the method of spraying water to cool the narrow side of the continuous casting billet within 48m below the foot roller of the continuous casting machine to improve the cooling strength of the narrow side to solve the bulging problem of the narrow side of the continuous casting billet; however, this method will cause the corners of the billet to be overcooled, and the corner temperature will be low during the straightening section, resulting in defects such as transverse cracks in the corners. The application with publication number CN102303104A controls the bulging deformation by designing the size, position and roller spacing of the supporting guide rollers and rollers; however, as the wide roller gap of the fan-shaped segment shrinks, the ingot will be widened in the lateral direction, which will increase the friction resistance between the narrow side supporting guide rollers and the ingot, resulting in defects such as scratches and abrasions on the surface of the ingot. The application with announcement number CN114734007B controls the bulging of the narrow side of the ingot by adding a hydraulic foot roller to the foot roller section of the continuous casting machine so that the foot roller pressure is equal to the static pressure of the molten steel, and then combines the continuous casting process parameters. However, this method requires the addition of auxiliary equipment, which has a high investment cost, and the foot roller section is a high-temperature area, the equipment is easily damaged, and maintenance is difficult, which affects steel production.
[0005] Regarding the central equiaxed crystal rate, its control level plays a key role in the quality stability of high-grade silicon steel. When the equiaxed crystal rate of the ingot is low, the columnar crystals are developed, and the deformation during the rolling process produces obvious directionality, resulting in corrugated defects. Regarding the control of the equiaxed crystal rate, the application with the announcement number CN101164720B improves the equiaxed crystal rate by controlling the superheat, the crystallizer and the secondary cooling intensity, and the electromagnetic stirring. However, since the overall control mainly relies on the electromagnetic stirring equipment, the fine control of factors such as temperature and cooling water flow is not ideal, and the equiaxed crystal rate is only increased to more than 45%. The application with the announcement number CN115283634B controls the equiaxed crystal rate of the continuous casting ingot to more than 65% by controlling the RH steel-out temperature, the crystallizer water volume, the secondary cooling water volume and the electromagnetic stirring parameters based on the Si content in the steel. However, this method reduces the secondary cooling water volume of the full roller section, which is not conducive to the control of the narrow side bulging of the continuous casting ingot.
[0006] Therefore, it is urgent to design a continuous casting billet production method for high-grade silicon steel, which can effectively reduce the narrow side bulging of the continuous casting billet and increase the central equiaxed crystal rate. Summary of the invention
[0007] The present invention provides a production method of a continuous casting billet for high-grade silicon steel and the silicon steel continuous casting billet produced. According to the cross-sectional size of the continuous casting billet, by controlling the pulling speed of a continuous casting machine, the amount of water in a crystallizer, the amount of water in a secondary cooling water, the taper and other parameters, a reasonable full roll segment, a zero segment and a fan-shaped segment roll gap are designed, and combined with the electromagnetic stirring technology in the secondary cooling zone, the narrow side bulging amount of the continuous casting billet for high-grade silicon steel is controlled to be less than or equal to 2 mm, and the central equiaxed crystal rate is controlled to be greater than or equal to 70%, thereby effectively reducing the narrow side bulging amount of the continuous casting billet and improving the central equiaxed crystal rate.
[0008] The technical solution adopted by the present invention to solve its technical problem is:
[0009] A method for producing a continuous casting billet for high-grade silicon steel, specifically comprising the following steps:
[0010] Step S1: pre-desulfurization of molten iron, mechanically stirring the molten iron, and spraying a desulfurizer for desulfurization, the temperature of the molten iron before desulfurization is ≥1450°C, S≤0.03%, the temperature of the molten iron after desulfurization is ≥1350°C, S≤0.0010%, and the slag removal rate is ≥98%;
[0011] Step S2: Converter smelting, pouring the desulfurized molten iron into the converter, adding 20-25% scrap steel, adding lime and blowing oxygen to slag for dephosphorization, heating and decarbonization, the T.Fe in the slag at the end of converter smelting is ≤20%, and the temperature is 1650-1680℃;
[0012] The components in the molten steel are as follows in terms of mass percentage: 0.03%≤C≤0.05%, 0.05%≤O≤0.07%, S≤0.0015%;
[0013] Step S3: RH refining, deep decarburization of molten steel, adding metal aluminum after decarburization, and then adding alloys, adjusting the composition of molten steel to the preset target composition, and then performing net circulation treatment. After the net circulation treatment, steel is tapped, and the tapping temperature is defined as ;
[0014] Step S4: Slab continuous casting, define the liquidus temperature of high grade silicon steel as According to the difference between the steel tapping temperature and the liquidus temperature of high-grade silicon steel, the current of the induction heating tundish is set, and the current control range is 0-1800A; the temperature range of the molten steel in the tundish is controlled to be 10-15℃;
[0015] The pulling speed, crystallizer and secondary cooling water volume are set according to the cross-sectional dimensions of the high-grade silicon steel continuous casting billet. At the same time, the current and frequency of the crystallizer electromagnetic and secondary cooling electromagnetic stirring are set based on the set pulling speed, crystallizer and secondary cooling water volume. The secondary cooling water volume ranges from 0.4-0.7L / kg.
[0016] According to the cross-sectional dimensions of the high-grade silicon steel continuous casting billet, the mold taper, the number of narrow side foot roller pairs and the roller spacing are set. The mold taper range is 1.15-1.25, the number of narrow side foot roller pairs ranges from 3 to 5 pairs, and the roller spacing is 30-50 mm.
[0017] Finally, the equiaxed crystal rate of silicon steel continuous casting billet is controlled to be ≥70%, and the bulging amount of the narrow side of silicon steel continuous casting billet is ≤2mm;
[0018] As a further preferred embodiment of the present invention, in step S1, a desulfurization agent is used for desulfurization treatment, the desulfurization agent includes lime powder and fluorite injected, CaO:CaF in the desulfurization agent is 9:1, and the desulfurization agent consumes 5-7kg of iron per ton;
[0019] As a further preferred embodiment of the present invention, in step S2, the scrap iron is made of low-sulfur silicon steel cutting waste;
[0020] As a further preferred embodiment of the present invention, in step S3, during RH vacuum refining, the vacuum degree is set to ≤ 0.67 bar; the duration of the net circulation treatment is ≥ 12 min;
[0021] As a further preferred embodiment of the present invention, in step S4, according to the steel tapping temperature Liquidus temperature of high grade silicon steel The difference between the values of , sets the current of the induction heating tundish, specifically:
[0022] when When the induction heating tundish is turned on, the current value is 0-600A;
[0023] when When the induction heating tundish is turned on, the current value is 600-1200A;
[0024] when When the induction heating tundish is turned on, the current value is 1200-1800A;
[0025] As a further preferred embodiment of the present invention, in step S4, when the cross-sectional size of the silicon steel continuous casting billet is (800-1000) mm×220 mm, the pulling speed is 1.10-1.20 m / min, the water volume of the wide surface of the crystallizer is 3400-3500 L / min, the water volume of the narrow surface of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.6-0.7 L / kg, the crystallizer electromagnetic stirring parameters are current 500-550 A, frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 400-450 A, frequency 4 Hz;
[0026] As a further preferred embodiment of the present invention, when the cross-sectional size of the silicon steel continuous casting billet is (800-1000) mm×220 mm, the taper of the crystallizer is 1.15, the number of narrow side foot rollers is 3 pairs, and the roller spacing is 50 mm;
[0027] As a further preferred embodiment of the present invention, in step S4, when the cross-sectional size of the silicon steel continuous casting billet is (1001-1200) mm×220 mm, the pulling speed is 1.00-1.10 m / min, the water volume of the wide surface of the crystallizer is 3500-3600 L / min, the water volume of the narrow surface of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.5-0.6 L / kg, the crystallizer electromagnetic stirring parameters are current 550-600 A, frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 450-500 A, frequency 4 Hz;
[0028] As a further preferred embodiment of the present invention, when the cross-sectional size of the silicon steel continuous casting billet is (1001-1200) mm×220 mm, the taper of the crystallizer is 1.20, the number of narrow side foot rollers is 4 pairs, and the roller spacing is 40 mm;
[0029] As a further preferred embodiment of the present invention, in step S4, when the cross-sectional size of the silicon steel continuous casting billet is (1201-1400) mm×220 mm, the pulling speed is 0.90-1.00 m / min, the water volume of the wide surface of the crystallizer is 3600-3700 L / min, the water volume of the narrow surface of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.4-0.5 L / kg, the crystallizer electromagnetic stirring parameters are current 600-650 A, frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 500-550 A, frequency 4 Hz;
[0030] As a further preferred embodiment of the present invention, when the cross-sectional size of the silicon steel continuous casting billet is (1201-1400) mm×220 mm, the taper of the crystallizer is 1.25, the number of narrow side foot rollers is 5 pairs, and the roller spacing is 30 mm;
[0031] As a further preferred embodiment of the present invention, in step S4, the secondary cooling zone includes a full roll section, a zero section and a fan section, the water volume of the full roll section accounts for 8-12% of the secondary cooling water volume, and the water volume of the zero section accounts for 52-64% of the secondary cooling water volume;
[0032] The foot roll section is divided into the narrow side and wide side of the silicon steel continuous casting billet. The narrow side accounts for 30-40% of the water volume in the foot roll section, and the wide side accounts for 60-70% of the water volume in the foot roll section.
[0033] As a further preferred embodiment of the present invention, the wide side length of the foot roller segment is 0.52 m, and two pairs of rollers are distributed;
[0034] The zero section length is 3m, with 10 pairs of rollers;
[0035] There are 12 fan-shaped segments, numbered 1#-12#, with a length of 2.4m, and 7 pairs of rollers distributed in each fan-shaped segment;
[0036] Control the gap between the crystallizer and the roller, and set the change of the roller gap contraction amount to positive, negative, and positive;
[0037] As a further preferred embodiment of the present invention, the shrinkage of the roll gap in the full roll section and the zero section is 0-0.2 mm;
[0038] The shrinkage of the roller gap of the fan-shaped segments numbered 1#-6# is -0.2--0.1mm;
[0039] The shrinkage of the roller gap of the fan-shaped segments numbered 7#-12# is 0.2-0.4mm;
[0040] As a further preferred embodiment of the present invention, the length of the crystallizer is 1000 mm, and the electromagnetic force at the center of the meniscus of the molten steel in the crystallizer is 20-25 N;
[0041] There are 2 pairs of electromagnetic stirring rollers for the secondary cooling, which are installed at the exit of the zero section and the entrance of the 1# sector section, 4.3m and 4.5m away from the meniscus of the molten steel in the crystallizer respectively;
[0042] Silicon steel continuous casting billets are produced according to the production method. The chemical composition of the silicon steel continuous casting billets, measured in mass percentage, includes: C≤0.0020%, 2.5%≤Si≤3.5%, 0.10%≤Mn≤0.30%, 0.010%≤P≤0.020%, S≤0.0020%, 0.5%≤Al≤0.8%, Ti≤0.0010%, and the balance is Fe and other inevitable impurities.
[0043] Through the above technical solution, compared with the prior art, the present invention has the following beneficial effects:
[0044] 1. The production method of the continuous casting billet for high-grade silicon steel provided by the present invention does not involve equipment modification, does not reduce the casting speed of the continuous casting machine, and therefore does not affect the output of the continuous casting machine, and the continuous casting billet has no other quality defects at low multiples;
[0045] 2. The production method of the continuous casting billet for high-grade silicon steel provided by the present invention increases the thickness of the billet shell on the narrow side of the continuous casting machine by setting parameters such as the continuous casting pulling speed, the water flow rate of the crystallizer, the amount of secondary cooling water, and the taper, so as to improve the strength and stability of the narrow side and better resist the static pressure of the molten steel. At the same time, the thickness of the wide billet shell is relatively thinned, so that the solidification of the molten steel in the wide direction is relatively delayed, which is conducive to more uniform solidification of the billet shell in the crystallizer and avoids defects caused by premature solidification. At the same time, it can also match the state of the narrow side billet shell to achieve reasonable regulation and optimization of the overall solidification process;
[0046] 3. The production method of continuous casting billets for high-grade silicon steel provided by the present invention adjusts the pulling speed of the continuous casting machine, the taper of the crystallizer and the number of narrow side foot rollers according to the different cross-sectional sizes of the continuous casting billets. By controlling the shrinkage of the roll gap in the foot roller section, zero section and fan-shaped section, in the early, middle and late stages of solidification of the continuous casting billets, it can avoid bulging of the narrow side of the continuous casting billets while ensuring good center quality. DETAILED DESCRIPTION
[0047] As described in the background technology, in order to avoid the problems of reduced capacity of the continuous casting machine caused by reducing the pulling speed, adhesion of the molten steel to the crystallizer, and other problems, the prior art solves the two main quality problems of large bulging on the narrow side of the continuous casting billet for high-grade silicon steel and low equiaxed crystal rate in the center. For example, water spray cooling is implemented on the narrow side of the continuous casting billet, various parameters of the supporting guide rollers are designed, and foot rollers are added to the foot roller section of the continuous casting machine. In terms of improving the center equiaxed crystal rate, electromagnetic stirring equipment and control of various parameters such as RH steel-out temperature are relied upon to avoid it. However, the implementation of the improved parts of the prior art will inevitably bring other problems. Solving the bulging problem will produce defects such as transverse cracks in the corners; adding foot rollers means that auxiliary equipment needs to be added, and the direct impact is that the investment cost becomes higher; excessive reliance on electromagnetic stirring equipment will result in unsatisfactory control effects of other parameters. If the relevant parameters are controlled, the water volume of the equipment cannot be controlled, and the bulging problem will reappear.
[0048] In order to achieve the above objectives at the same time, the present application provides a method for producing continuous casting billets for high-grade silicon steel, specifically, according to the cross-sectional size of the continuous casting billet, by controlling the casting speed of the continuous casting machine, the amount of water in the crystallizer, the amount of water in the secondary cooling water, the taper and other parameters, a reasonable full roll segment, zero segment and fan-shaped segment roll gap are designed, and the electromagnetic stirring technology of the secondary cooling zone is combined. The production method of the present application does not involve equipment modification, does not need to reduce the casting speed of the continuous casting machine, and therefore does not affect the output of the continuous casting machine, and the continuous casting billet has no other quality defects at low multiples.
[0049] Next, the production method provided in this application is specifically described. The production process includes molten iron pre-desulfurization → converter smelting → RH refining → continuous casting to produce the continuous casting billet, which specifically includes the following steps:
[0050] Step S1: Pre-desulfurization of molten iron: mechanically stir the molten iron and spray a desulfurizer for desulfurization. The desulfurizers usually used include lime powder and fluorite. To achieve the best desulfurization effect, the CaO:CaF ratio in the desulfurizer is 9:1, and the desulfurizer consumption per ton of iron is 5-7kg.
[0051] After the KR treatment in step S1, the molten iron temperature before desulfurization is ≥1450°C, S≤0.03%, the molten iron temperature after desulfurization is ≥1350°C, S≤0.0010%, and the slag removal rate is ≥98%.
[0052] Step S2: Converter smelting, pouring the desulfurized molten iron into the converter, adding scrap steel, adding lime and blowing oxygen to slag for dephosphorization, heating and decarbonization, the T.Fe content of the slag at the end of converter smelting is ≤20%, and the temperature is 1650-1680℃;
[0053] In the converter smelting process, adding scrap steel can firstly reduce the steelmaking cost. The price of scrap steel is lower than that of pig iron or other steelmaking raw materials. Adding an appropriate amount of scrap steel can reduce the demand for original molten iron, thereby reducing production costs. Secondly, the addition of scrap steel absorbs part of the heat of the molten iron, controls the temperature of the molten steel in the converter, and avoids excessive temperature. Finally, scrap steel contains some beneficial alloy elements. Adding an appropriate amount of scrap steel can adjust the alloy composition of the molten steel to meet the requirements of different steel grades.
[0054] Preferably, the scrap steel added in the present application is low-sulfur silicon steel cutting scrap, and the added amount accounts for 20-25%. After oxygen blowing, heating, decarburization and dephosphorization operations, the components in the molten steel obtained are respectively calculated in mass percentage as follows: 0.03%≤C≤0.05%, 0.05%≤O≤0.07%, S≤0.0015%.
[0055] Step S3: RH refining, control the vacuum degree ≤ 0.67 bar, perform deep decarburization on the molten steel, add metal aluminum after decarburization, add alloy, adjust the composition of the molten steel to the preset target composition, and then perform net circulation treatment. The duration of net circulation treatment is ≥ 12 minutes. After the net circulation treatment, the steel is tapped. The tapping temperature is defined as The tapping temperature here is based on the liquidus temperature of the steel grade. Make matching control adjustments.
[0056] After the coordinated processing of step S1 to step S3, molten steel with composition and cleanliness meeting the requirements can be provided. The next step is step S4, slab continuous casting.
[0057] In the slab continuous casting process, it is first necessary to use the tundish molten steel for high superheat pouring (control the tundish molten steel temperature range to be 10-15°C), and the current value of the induction heating tundish is determined by the difference between the steel tapping temperature and the liquidus temperature of the high-grade silicon steel, specifically:
[0058] when When the induction heating tundish is turned on, the current value is 0-600A;
[0059] when When the induction heating tundish is turned on, the current value is 600-1200A;
[0060] when When the induction heating middle package is turned on, the current value is 1200-1800A.
[0061] Then, high continuous casting speed, small water flow in the crystallizer, large taper on the narrow side to reduce the air gap between the billet shell and the crystallizer wall, and increased cooling water flow on the narrow side of the foot roll section were set. The design of small water flow in the crystallizer and large taper on the narrow side reduced the air gap between the billet shell and the crystallizer wall, which is beneficial to the uniform growth of the billet shell and enhance its stability. Combined with increasing the cooling water flow on the narrow side of the foot roll section, the thickness of the narrow side billet shell of the continuous casting billet at the crystallizer outlet is increased. The increase in the thickness of the narrow side billet shell improves the strength and stability of the narrow side, can increase the ability of the narrow side billet shell to resist the static pressure of molten steel, and reduce the risk of deformation, rupture and other problems of the billet shell due to force, which helps to ensure the quality of the billet and the smooth progress of the continuous casting process.
[0062] The above-mentioned means can also make the shell thickness of the wide side of the continuous casting billet at the crystallizer outlet relatively thin, which can control the balance between heat transfer and solidification rate to a certain extent. The thinner wide shell can relatively delay the solidification of the molten steel in the wide direction, which is beneficial to more uniform solidification of the shell in the crystallizer and avoid defects caused by premature solidification. At the same time, it can also match the state of the narrow side shell to achieve reasonable regulation and optimization of the overall solidification process.
[0063] Specifically, the pulling speed of the continuous casting machine, the water volume on the wide surface of the crystallizer, the water volume on the narrow surface of the crystallizer, the secondary cooling water volume, the electromagnetic stirring parameters of the crystallizer and the secondary cooling electromagnetic stirring parameters are all related to the cross-sectional dimensions of the silicon steel continuous casting billet. In the preferred embodiment, three cross-sectional dimensions are selected, namely (800-1000) mm×220mm, (1001-1200) mm×220mm and (1201-1400) mm×220mm. These three dimensions cover almost all models for the research on high-grade silicon steel in this application.
[0064] Specifically, when the cross-sectional size of the silicon steel continuous casting billet is (800-1000) mm×220 mm, the pulling speed is 1.10-1.20 m / min, the water volume on the wide surface of the crystallizer is 3400-3500 L / min, the water volume on the narrow surface of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.6-0.7 L / kg, the crystallizer electromagnetic stirring parameters are current 500-550 A, frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 400-450 A, frequency 4 Hz.
[0065] When the cross-sectional size of the silicon steel continuous casting billet is (1001-1200) mm×220 mm, the pulling speed is 1.00-1.10 m / min, the water volume on the wide surface of the crystallizer is 3500-3600 L / min, the water volume on the narrow surface of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.5-0.6 L / kg, the crystallizer electromagnetic stirring parameters are current 550-600 A, frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 450-500 A, frequency 4 Hz.
[0066] When the cross-sectional size of the silicon steel continuous casting billet is (1201-1400) mm×220 mm, the pulling speed is 0.90-1.00 m / min, the water volume on the wide surface of the crystallizer is 3600-3700 L / min, the water volume on the narrow surface of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.4-0.5 L / kg, the crystallizer electromagnetic stirring parameters are current 600-650 A and frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 500-550 A and frequency 4 Hz.
[0067] Regarding the above distribution of secondary cooling water volume, the water volume of the full roll section and the zero section included in the continuous casting secondary cooling zone are specifically allocated. The entire secondary cooling water volume range is controlled at 0.4-0.7L / kg, the full roll section water volume accounts for 8-12% of the secondary cooling water volume, and the zero section water volume accounts for 52-64% of the secondary cooling water volume; the full roll section is divided into the narrow side and the wide side of the silicon steel continuous casting billet, the narrow side accounts for 30-40% of the water volume of the full roll section, and the wide side accounts for 60-70% of the water volume of the full roll section.
[0068] According to the cross-sectional dimensions of high-grade silicon steel continuous casting billets, the crystallizer taper, the number of narrow side foot roller pairs and the roller spacing are also set. It should be noted that the crystallizer taper range is 1.15-1.25, the number of narrow side foot roller pairs ranges from 3 to 5 pairs, and the roller spacing is 30-50mm. When the cross-sectional dimensions of the silicon steel continuous casting billet are (800-1000) mm×220mm, the crystallizer taper is 1.15, the narrow side foot rollers are 3 pairs, and the roller spacing is 50mm. When the cross-sectional dimensions of the silicon steel continuous casting billet are (1001-1200) mm×220mm, the crystallizer taper is 1.20, the narrow side foot rollers are 4 pairs, and the roller spacing is 40mm. When the cross-sectional dimensions of the silicon steel continuous casting billet are (1201-1400) mm×220mm, the crystallizer taper is 1.25, the narrow side foot rollers are 5 pairs, and the roller spacing is 30mm.
[0069] Regarding the continuous casting secondary cooling zone, the length and roller settings of the full roller segment, zero segment and fan-shaped segment are also optimized. The wide length of the full roller segment is 0.52m, with 2 pairs of rollers; the length of the zero segment is 3m, with 10 pairs of rollers; the fan-shaped segments include 12, numbered 1#-12# respectively, the length of the fan-shaped segments 1#-12# is 2.4m, and each fan-shaped segment has 7 pairs of rollers.
[0070] Regarding the design of the roll gap shrinkage in the continuous casting process, it is the change in the gap between the crystallizer and the roller during the continuous casting process. As an important parameter, this application adopts positive → negative → positive. The roll gap shrinkage in the full roll segment and the zero segment is 0-0.2mm; the roll gap shrinkage of the fan-shaped segment numbered 1#-6# is -0.2--0.1mm; the roll gap shrinkage of the fan-shaped segment numbered 7#-12# is 0.2-0.4mm.
[0071] When the roll gap shrinkage is positive, a smaller roll gap shrinkage is set in the early stage of solidification of the continuous casting billet (in the foot roll section and the zero section roll), combined with increasing the cooling water flow of the foot roll section on the narrow side of the crystallizer, increasing the billet shell thickness and increasing the narrow side taper of the crystallizer, which can not only reduce the pressure of the roll gap shrinkage on the wide surface of the continuous casting billet to prevent the narrow side of the continuous casting billet from bulging, but also prevent the wide surface of the continuous casting billet from bulging under the static pressure of the molten steel, resulting in the formation of middle cracks. Secondly, the thin billet shell thickness on the wide surface of the continuous casting billet at the outlet of the crystallizer and the setting of a smaller roll gap shrinkage in the early stage of solidification of the continuous casting billet are conducive to reducing the billet shell thickness of the continuous casting billet at the position of the secondary cooling electromagnetic stirrer, and under the action of the electromagnetic stirring force, it is conducive to increasing the proportion of equiaxed crystals.
[0072] When the roll gap shrinkage is negative, in the middle stage of solidification of the continuous casting billet (sector-shaped sections numbered 1#-6#), the billet shell on the wide surface of the continuous casting billet has a certain thickness and can resist the static pressure of the molten steel. The roll gap shrinkage is controlled to a negative value to reduce the pressure of the roll gap shrinkage on the wide surface of the continuous casting billet and prevent the narrow side of the continuous casting billet from bulging.
[0073] When the roll gap shrinkage is positive again, in the later stage of solidification of the continuous casting billet (sector segments numbered 7#-12#), the solidification shrinkage is large. In order to ensure good center quality, the larger roll gap shrinkage is controlled.
[0074] Finally, the electromagnetic stirring technology in the secondary cooling zone is combined. That is, for the crystallizer, its length is set to 1000mm, and the electromagnetic force at the center of the meniscus of the molten steel in the crystallizer is 20-25N; there are 2 pairs of electromagnetic stirring rollers in the secondary cooling zone, which are installed at the zero section outlet and the 1# fan-shaped section inlet, and are 4.3m and 4.5m away from the meniscus of the molten steel in the crystallizer respectively.
[0075] As mentioned above, by controlling the continuous casting machine pulling speed, crystallizer water volume, secondary cooling water volume, taper and other parameters, designing reasonable full roll segment, zero segment and fan-shaped segment roll gaps, and combining the secondary cooling zone electromagnetic stirring technology, the narrow side bulge of the continuous casting billet for high-grade silicon steel is controlled to ≤2mm, and the central equiaxed crystal rate is controlled to ≥70%.
[0076] The silicon steel continuous casting billet obtained by this method is tested and its composition fully meets the use requirements. Specifically, in terms of mass percentage, the chemical composition of the silicon steel continuous casting billet includes: C≤0.0020%, 2.5%≤Si≤3.5%, 0.10%≤Mn≤0.30%, 0.010%≤P≤0.020%, S≤0.0020%, 0.5%≤Al≤0.8%, Ti≤0.0010%, and the balance is Fe and other unavoidable impurities.
[0077] In order to demonstrate that the silicon steel continuous casting billets produced by the production method for high-grade silicon steel continuous casting billets provided in the present application fully meet the preset expected values, the present application provides the following three embodiments. Example
[0078] Embodiment 1:
[0079] The steel grade is WV2000, the liquidus temperature is 1512℃, the cross-sectional size of the continuous casting billet is 900 mm×220 mm, the length of the crystallizer is 1000 mm, and the continuous casting secondary cooling zone includes a full roller section, a zero section and 12 fan-shaped sections. The wide surface length of the full roller section is 0.52 m, with 2 pairs of rollers distributed; the length of the zero section is 3 m, with 10 pairs of rollers distributed; the length of the fan-shaped sections numbered 1#~12# is 2.4 m, and each fan-shaped section has 7 pairs of rollers distributed. There are 2 pairs of secondary cooling electromagnetic stirring rollers, which are installed at the outlet of the zero section and the inlet of the 1# fan-shaped section, and are 4.3 m and 4.5 m away from the meniscus of the molten steel in the crystallizer respectively.
[0080] The provided method for producing a continuous casting billet for high-grade silicon steel specifically comprises the following steps:
[0081] The first step is the hot metal pretreatment process. Before desulfurization, the hot metal temperature is 1460℃, S is 0.028%, the mass ratio of CaO to CaF in the desulfurizer is 9:1, the amount of desulfurizer added per ton of iron is 5kg, the desulfurization treatment time is 35min, the hot metal temperature after desulfurization is 1360℃, S is 0.0010%, and the slag removal rate is 98%, and low-sulfur hot metal is obtained;
[0082] The second step is to add low-S content silicon steel scraps in the converter smelting process, and then add low-sulfur molten iron into the converter, wherein the scrap ratio is 20%, add lime and blow oxygen to make slag dephosphorization, temperature increase, and decarbonization. The T.Fe content in the slag at the end of the converter smelting is 15%, the C content in the molten steel is 0.05%, the O content is 0.05%, the S content is 0.0015%, and the temperature is 1650℃;
[0083] The third step is the RH refining process, in which the vacuum degree is 0.67 bar, and the molten steel is deeply decarburized. After decarburization, metallic aluminum is added first, and then the remaining alloys are added. The composition of the molten steel is 0.0020% C, 2.6% Si, 0.15% Mn, 0.018% P, 0.0019% S, 0.55% Al, 0.0009% Ti, and the remainder is Fe and other inevitable impurities. Then, a net circulation treatment is carried out, and the net circulation time is 12 minutes. The RH tapping temperature is 1558°C.
[0084] In the fourth step, during the continuous casting process, the ladle is hoisted to the continuous casting platform for protective pouring, and the induction heating tundish is turned on. The current value is 300A, the superheat of the molten steel in the tundish is 15°C, and the molten steel flows into the crystallizer from the tundish through the immersed water nozzle. The taper of the crystallizer is 1.15, there are 3 pairs of narrow side foot rollers, the roller spacing is 50mm, the continuous casting speed is 1.15m / min, the water volume on the wide side of the crystallizer is 3450L / min, the water volume on the narrow side of the crystallizer is 575L / min, and the electromagnetic stirring parameters of the crystallizer are current 500 A. Frequency is 5Hz, the electromagnetic force at the center of the meniscus of the molten steel in the crystallizer is 20N, the secondary cooling electromagnetic stirring parameters are current 400A, frequency 4Hz, secondary cooling water volume is 0.65L / kg, of which the water volume of the full roll section and the zero section accounts for 12% and 64% respectively, the water volume of the narrow side and the wide side of the full roll section accounts for 40% and 60% respectively, the roll gap contraction of the full roll section and the zero section is 0mm, the roll gap contraction of the fan-shaped sections No. 1#~6# is -0.1mm, and the roll gap contraction of the fan-shaped sections No. 7#~12# is 0.2mm.
[0085] Finally, a low-magnification sample was taken from the continuous casting billet to measure the bulging amount on the narrow side of the continuous casting billet and the central equiaxed crystal rate. The bulging amount on the narrow side of the continuous casting billet was 1 mm, and the central equiaxed crystal rate was 70%.
[0086] Calculated in mass percentage, the chemical composition of silicon steel continuous casting billet includes: C≤0.0020%, 2.5%≤Si≤2.8%, 0.10%≤Mn≤0.20%, 0.010%≤P≤0.020%, S≤0.0020%, 0.5%≤Al≤0.6%, Ti≤0.0010%, and the balance is Fe and other inevitable impurities.
[0087] Embodiment 2:
[0088] The steel grade is WV1500, the liquidus temperature is 1510℃, the cross-sectional size of the continuous casting billet is 1100 mm×220 mm, the length of the crystallizer is 1000 mm, and the continuous casting secondary cooling zone includes a full roller section, a zero section and 12 fan-shaped sections. The wide surface length of the full roller section is 0.52 m, with 2 pairs of rollers distributed; the length of the zero section is 3 m, with 10 pairs of rollers distributed; the length of the fan-shaped sections numbered 1#~12# is 2.4 m, and each fan-shaped section has 7 pairs of rollers distributed. There are 2 pairs of secondary cooling electromagnetic stirring rollers, which are installed at the outlet of the zero section and the inlet of the 1# fan-shaped section, and are 4.3 m and 4.5 m away from the meniscus of the molten steel in the crystallizer respectively.
[0089] The provided method for producing a continuous casting billet for high-grade silicon steel specifically comprises the following steps:
[0090] The first step is the hot metal pretreatment process. Before desulfurization, the hot metal temperature is 1480℃, S is 0.025%, the mass ratio of CaO to CaF in the desulfurizer is 9:1, the amount of desulfurizer added per ton of iron is 6kg, the desulfurization treatment time is 30min, the hot metal temperature after desulfurization is 1380℃, S is 0.0008%, and the slag removal rate is 99%, and low-sulfur hot metal is obtained;
[0091] The second step is to add low-S content silicon steel scrap in the converter smelting process, and then add low-sulfur molten iron into the converter, wherein the scrap steel ratio is 23%, add lime and blow oxygen to make slag dephosphorization, temperature increase, and decarbonization. The T.Fe content in the slag at the end of converter smelting is 18%, the C content in the molten steel is 0.04%, the O content is 0.06%, the S content is 0.0012%, and the temperature is 1660℃;
[0092] The third step is the RH refining process, in which the vacuum degree is 0.67 bar, and the molten steel is deeply decarburized. After decarburization, metallic aluminum is added first, and then the remaining alloys are added. The composition of the molten steel is 0.0018% C, 3.0% Si, 0.20% Mn, 0.016% P, 0.0017% S, 0.65% Al, 0.0008% Ti, and the remainder is Fe and other inevitable impurities. Then, a net circulation treatment is carried out, and the net circulation time is 12 minutes. The RH tapping temperature is 1553°C.
[0093] In the fourth step, during the continuous casting process, the ladle is hoisted to the continuous casting platform for protective pouring, and the induction heating tundish is turned on. The current value is 900A, the superheat of the molten steel in the tundish is 13°C, and the molten steel flows into the crystallizer from the tundish through the immersed water nozzle. The taper of the crystallizer is 1.20, there are 4 pairs of narrow side foot rollers, the roller spacing is 40mm, the continuous casting speed is 1.05m / min, the water volume on the wide side of the crystallizer is 3550L / min, the water volume on the narrow side of the crystallizer is 575L / min, and the electromagnetic stirring parameters of the crystallizer are current 550A, The frequency is 5Hz, the electromagnetic force at the center of the meniscus of the molten steel in the crystallizer is 22N, the secondary cooling electromagnetic stirring parameters are current 450A, frequency 4Hz, and secondary cooling water volume 0.55L / kg, of which the water volume of the full roll section and the zero section accounts for 10% and 58% respectively, and the water volume of the narrow side and the wide side of the full roll section accounts for 35% and 65% respectively, the roll gap contraction of the full roll section and the zero section is 0.1mm, the roll gap contraction of the fan-shaped sections No. 1#~6# is -0.15mm, and the roll gap contraction of the fan-shaped sections No. 7#~12# is 0.3mm.
[0094] Finally, a low-magnification sample was taken from the continuous casting billet to measure the bulging amount on the narrow side and the central equiaxed crystal ratio. The bulging amount on the narrow side of the continuous casting billet was 1 mm, and the central equiaxed crystal ratio was 73%.
[0095] Measured in mass percentage, the chemical composition of silicon steel continuous casting billet includes: C≤0.0020%, 2.8%≤Si≤3.2%, 0.15%≤Mn≤0.25%, 0.010%≤P≤0.020%, S≤0.0020%, 0.6%≤Al≤0.7%, Ti≤0.0010%, and the balance is Fe and other inevitable impurities.
[0096] Embodiment 3:
[0097] The steel grade is WV1000, the liquidus temperature is 1508℃, the cross-sectional size of the continuous casting billet is 1300 mm×220 mm, the length of the crystallizer is 1000 mm, and the continuous casting secondary cooling zone includes a full roller section, a zero section and 12 fan-shaped sections. The wide surface length of the full roller section is 0.52 m, with 2 pairs of rollers distributed; the length of the zero section is 3 m, with 10 pairs of rollers distributed; the length of the fan-shaped sections numbered 1#~12# is 2.4 m, and each fan-shaped section has 7 pairs of rollers distributed. There are 2 pairs of secondary cooling electromagnetic stirring rollers, which are installed at the outlet of the zero section and the inlet of the 1# fan-shaped section, and are 4.3 m and 4.5 m away from the meniscus of the molten steel in the crystallizer respectively.
[0098] The provided method for producing a continuous casting billet for high-grade silicon steel specifically comprises the following steps:
[0099] The first step is the hot metal pretreatment process. Before desulfurization, the hot metal temperature is 1470℃, S is 0.025%, the mass ratio of CaO to CaF in the desulfurizer is 9:1, the amount of desulfurizer added per ton of iron is 7kg, the desulfurization treatment time is 28min, the hot metal temperature after desulfurization is 1370℃, S is 0.0007%, and the slag removal rate is 99%, and low-sulfur hot metal is obtained;
[0100] The second step is to add low-S content silicon steel scrap in the converter smelting process, and then add low-sulfur molten iron into the converter, wherein the scrap steel ratio is 25%, add lime and blow oxygen to make slag dephosphorization, temperature rise, and decarbonization. The T.Fe content in the slag at the end of converter smelting is 20%, the C content in the molten steel is 0.03%, the O content is 0.07%, the S content is 0.0010%, and the temperature is 1680℃;
[0101] The third step is the RH refining process, in which the vacuum degree is 0.67 bar, and the molten steel is deeply decarburized. After decarburization, metallic aluminum is added first, and then the remaining alloys are added. The composition of the molten steel is 0.0016% C, 3.4% Si, 0.25% Mn, 0.013% P, 0.0015% S, 0.65% Al, 0.0007% Ti, and the remainder is Fe and other inevitable impurities. Then, a net circulation treatment is carried out, and the net circulation time is 12 minutes. The RH tapping temperature is 1545°C.
[0102] In the fourth step, during the continuous casting process, the ladle is hoisted to the continuous casting platform for protective pouring, and the induction heating tundish is turned on. The current value is 1500A, the superheat of the molten steel in the tundish is 10°C, and the molten steel flows into the crystallizer from the tundish through the immersed water nozzle. The crystallizer taper is 1.25, there are 5 pairs of narrow side foot rollers, the roller spacing is 30mm, the continuous casting speed is 0.95m / min, the water volume on the wide surface of the crystallizer is 3650L / min, the water volume on the narrow surface of the crystallizer is 575L / min, and the crystallizer electromagnetic stirring parameters are current 600 A. Frequency is 5Hz, the electromagnetic force at the center of the meniscus of the molten steel in the crystallizer is 25N, the secondary cooling electromagnetic stirring parameters are current 500A, frequency 4Hz, secondary cooling water volume is 0.45L / kg, of which the water volume of the full roll section and the zero section accounts for 8% and 52% respectively, the water volume of the narrow side and the wide side of the full roll section accounts for 30% and 70% respectively, the roll gap contraction of the full roll section and the zero section is 0.2mm, the roll gap contraction of the fan-shaped sections No. 1#~6# is -0.2mm, and the roll gap contraction of the fan-shaped sections No. 7#~12# is 0.4mm.
[0103] Finally, a low-magnification sample was taken from the continuous casting billet to measure the bulging amount on the narrow side and the central equiaxed crystal ratio. The bulging amount on the narrow side of the continuous casting billet was 2 mm, and the central equiaxed crystal ratio was 75%.
[0104] Measured in mass percentage, the chemical composition of the silicon steel continuous casting billet includes: C≤0.0020%, 3.2%≤Si≤3.5%, 0.20%≤Mn≤0.30%, 0.010%≤P≤0.020%, S≤0.0020%, 0.6%≤Al≤0.7%, Ti≤0.0010%, and the balance is Fe and other inevitable impurities.
[0105] In Example 1 to Example 3, the narrow side bulging amount of the high-grade silicon steel continuous casting billet is controlled to be ≤2mm, and the central equiaxed crystal ratio is controlled to be ≥70%.
[0106] The silicon steel continuous casting billet obtained by this method has been tested and its composition fully meets the use requirements. The chemical composition, calculated by mass percentage, includes: C≤0.0020%, 2.5%≤Si≤3.5%, 0.10%≤Mn≤0.30%, 0.010%≤P≤0.020%, S≤0.0020%, 0.5%≤Al≤0.8%, Ti≤0.0010%, and the balance is Fe and other inevitable impurities.
[0107] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as generally understood by those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless defined as herein.
[0108] The meaning of "and / or" described in this application means that the situations where each exists alone or both exist at the same time are included.
[0109] The term “connection” as used in this application may mean a direct connection between components or an indirect connection between components via other components.
[0110] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for producing a continuous casting billet for high-grade silicon steel, characterized in that: The specific steps include: Step S1: Pre-desulfurization of molten iron: mechanically stir the molten iron and spray a desulfurizer to desulfurize it. The temperature of the molten iron before desulfurization is ≥1450°C, S≤0.03%, and the temperature of the molten iron after desulfurization is ≥1350°C, S≤0.0010%, and the slag skimming rate is ≥98%; Step S2: smelting in a converter, pouring the desulfurized molten iron into the converter, adding 20-25% scrap steel, adding lime and blowing oxygen to slag for dephosphorization, heating, and decarburization. The T.Fe content of the slag at the end of the converter smelting is ≤20%, and the temperature is 1650-1680°C. The components in molten steel are as follows in terms of mass percentage: 0.03%≤C≤0.05%, 0.05%≤O≤0.07%, S≤0.0015%; Step S3: RH refining, deep decarburization of molten steel, adding aluminum and alloy after decarburization, adjusting the composition of molten steel to the preset target composition, and then performing net circulation treatment. After the net circulation treatment, the steel is tapped. The tapping temperature is defined as ; Step S4: Slab continuous casting, define the liquidus temperature of high grade silicon steel as According to the difference between the tapping temperature and the liquidus temperature of high-grade silicon steel, the current of the induction heating tundish is set, and the current control range is 0-1800A; the temperature range of the molten steel in the tundish is controlled to be 10-15℃; The casting speed, mold and secondary cooling water volume are set according to the cross-sectional dimensions of the high-grade silicon steel continuous casting billet. The current and frequency of the mold electromagnetic stirring and the secondary cooling electromagnetic stirring are also set based on the set casting speed, mold and secondary cooling water volume. The secondary cooling water volume range is 0.4-0.7L / kg. The mold taper, number of narrow side foot rollers and roller spacing are set according to the cross-sectional dimensions of the high-grade silicon steel continuous casting billet. The mold taper range is 1.15-1.25, the number of narrow side foot rollers ranges from 3 to 5 pairs, and the roller spacing is 30-50 mm. Finally, the equiaxed grain rate of silicon steel continuous casting billet is controlled to be ≥70%, and the bulge on the narrow side of silicon steel continuous casting billet is controlled to be ≤2mm.
2. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, wherein: In step S1, desulfurization is carried out using a desulfurizer, which includes injected lime powder and fluorite. In the desulfurizer, CaO:CaF=9:1, and the desulfurizer consumes 5-7kg per ton of iron.
3. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, wherein: In step S2, the scrap iron is cut into scraps using low-sulfur silicon steel.
4. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, wherein: In step S3, during RH vacuum refining, the vacuum degree is set to ≤ 0.67 bar; and the duration of the net circulation treatment is ≥ 12 min.
5. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, wherein: In step S4, according to the tapping temperature Liquidus temperature of high grade silicon steel The difference between the two sets is used to set the current of the induction heating tundish, specifically: when When the induction heating tundish is turned on, the current value is 0-600A; when When the induction heating tundish is turned on, the current value is 600-1200A; when When the induction heating ladle is turned on, the current value is 1200-1800A.
6. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, characterized in that: In step S4, when the cross-sectional size of the silicon steel continuous casting billet is (800-1000) mm×220 mm, the pulling speed is 1.10-1.20 m / min, the water volume on the wide surface of the crystallizer is 3400-3500 L / min, the water volume on the narrow surface of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.6-0.7 L / kg, the crystallizer electromagnetic stirring parameters are current 500-550 A, frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 400-450 A, frequency 4 Hz.
7. The method for producing a continuous casting billet for high-grade silicon steel according to claim 6, characterized in that: When the cross-sectional size of the silicon steel continuous casting billet is (800-1000) mm × 220 mm, the taper of the crystallizer is 1.15, there are 3 pairs of narrow side foot rollers, and the roller spacing is 50 mm.
8. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, wherein: In step S4, when the cross-sectional size of the silicon steel continuous casting billet is (1001-1200) mm×220 mm, the pulling speed is 1.00-1.10 m / min, the water volume on the wide side of the crystallizer is 3500-3600 L / min, the water volume on the narrow side of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.5-0.6 L / kg, the crystallizer electromagnetic stirring parameters are current 550-600 A, frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 450-500 A, frequency 4 Hz.
9. The method for producing a continuous casting billet for high-grade silicon steel according to claim 8, characterized in that: When the cross-sectional size of the silicon steel continuous casting billet is (1001-1200) mm × 220 mm, the taper of the crystallizer is 1.20, there are 4 pairs of narrow side foot rollers, and the roller spacing is 40 mm.
10. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, characterized in that: In step S4, when the cross-sectional size of the silicon steel continuous casting billet is (1201-1400) mm×220 mm, the pulling speed is 0.90-1.00 m / min, the water volume on the wide surface of the crystallizer is 3600-3700 L / min, the water volume on the narrow surface of the crystallizer is 550-600 L / min, the secondary cooling water volume is 0.4-0.5 L / kg, the crystallizer electromagnetic stirring parameters are current 600-650 A and frequency 5 Hz, and the secondary cooling electromagnetic stirring parameters are current 500-550 A and frequency 4 Hz.
11. The method for producing a continuous casting billet for high-grade silicon steel according to claim 10, characterized in that: When the cross-sectional size of the silicon steel continuous casting billet is (1201-1400) mm × 220 mm, the taper of the crystallizer is 1.25, the number of narrow side foot rollers is 5 pairs, and the roller spacing is 30 mm.
12. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, characterized in that: In step S4, the secondary cooling zone includes a full roller section, a zero section, and a fan section. The water volume of the full roller section accounts for 8-12% of the secondary cooling water volume, and the water volume of the zero section accounts for 52-64% of the secondary cooling water volume. The foot roll section is divided into the narrow side and the wide side of the silicon steel continuous casting billet. The narrow side accounts for 30-40% of the water volume relative to the foot roll section, and the wide side accounts for 60-70% of the water volume relative to the foot roll section.
13. The method for producing a continuous casting billet for high-grade silicon steel according to claim 12, characterized in that: The wide length of the foot roller section is 0.52m, with 2 pairs of rollers distributed; The zero section length is 3m, with 10 pairs of rollers distributed; There are 12 fan-shaped segments, numbered 1#-12#. The length of the fan-shaped segments 1#-12# is 2.4m, and each fan-shaped segment is equipped with 7 pairs of rollers. Control the gap between the crystallizer and the roller, and set the change of the roller gap contraction to positive, negative, and positive.
14. The method for producing a continuous casting billet for high-grade silicon steel according to claim 13, characterized in that: The shrinkage of the roller gap in the full roller section and the zero section is 0-0.2mm; The roller gap shrinkage of the sector segments numbered 1#-6# is -0.2-0.1mm; The shrinkage of the roller gap of the sector segments numbered 7#-12# is 0.2-0.4mm.
15. The method for producing a continuous casting billet for high-grade silicon steel according to claim 1, characterized in that: The length of the crystallizer is 1000 mm, and the electromagnetic force at the center of the meniscus of the molten steel in the crystallizer is 20-25 N; There are two pairs of secondary cooling electromagnetic stirring rollers, installed at the exit of zero section and the entrance of 1# sector section, 4.3m and 4.5m away from the meniscus of molten steel in the crystallizer respectively.
16. Silicon steel continuous casting billet produced by the production method according to claim 1 or 2 or 3 or 4 or 5 or 7 or 9 or 11 or 14 or 15, characterized in that: Calculated in percentage by mass, the chemical composition of the silicon steel continuous casting billet includes: C≤0.0020%, 2.5%≤Si≤3.5%, 0.10%≤Mn≤0.30%, 0.010%≤P≤0.020%, S≤0.0020%, 0.5%≤Al≤0.8%, Ti≤0.0010%, and the balance is Fe and other inevitable impurities.