Needle punching preparation method of ultra-thin pre-oxidized silk felt for flow battery electrodes

The needling preparation method of ultra-thin pre-oxygenated silk felt for flow battery electrodes solves the problem of high process cost of existing carbon fiber preforms. By enhancing fiber cross-linking and filling efficiency, the mechanical properties and production efficiency of the material are improved, achieving A lower cost and efficient process.

CN118461225BActive Publication Date: 2024-10-29烟台奥森制动材料有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410912422.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-29
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The existing carbon fiber preform process requires repeated processes such as high temperature, carbonization and deposition in the deposition process, resulting in large investment in electricity, material resources and manpower, and high production costs.

Method used

The preparation method of ultra-thin pre-oxygenated silk felt for flow battery electrodes is adopted, which includes cutting the pre-oxidized silk fiber into short fibers and spraying water and treatment agent to form a mesh, and forming a single-layer composite through continuous needling, followed by multiple Angular cross-needling layer by layer, using a polyethylene glycol-based treatment agent containing silicon-based iron and tin complexes to enhance fiber cross-linking and filling efficiency.

Benefits of technology

It improves the mechanical properties of carbon fiber and the density of polyacrylonitrile pre-oxidized yarn, reduces process costs and energy consumption, and improves the mechanical properties and production efficiency of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of pre-oxidized wire needle-punching, and discloses a method for preparing ultra-thin pre-oxidized wire felt for liquid flow battery electrodes by needle-punching. The specific process comprises: 1,1'-di(dimethylsilyl) iron undergoes a silylation reaction with allyl glycidyl ether, and then undergoes a silylation reaction with tributyl(1-ethoxyvinyl)tin, wherein the intermediate product undergoes an epoxy-amino reaction with double-terminated amino polyethylene glycol to obtain a polyethylene glycol-based treating agent containing a silicon-based iron and tin complex; the treating agent prepared by the invention enhances the cross-linking between fibers inside the carbon fiber, thereby improving the overall mechanical strength; the treating agent prepared by the invention can effectively improve the filling efficiency of polyacrylonitrile pre-oxidized fibers in the carbon fiber felt; the interaction between the active groups in the treating agent and the polyacrylonitrile chain improves the microstructure of the fiber surface, makes the fiber surface smoother, reduces defect points, and further improves the uniformity and performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pre-oxidized wire needling, in particular to a method for needling preparation of ultra-thin pre-oxidized wire felt for liquid flow battery electrodes. Background Art

[0002] Preoxidized silk fiber is one of the high-performance C / C composite materials. The product obtained by modern high-tech carbon / carbon deposition process has high carbon content, strong wear resistance, high temperature resistance, radiation resistance, corrosion resistance, light weight and other excellent properties. Preoxidized silk fiber needle punched preform is an emerging functional structural product. Its unique performance and advanced production process ensure that carbon fiber products can be widely used in aviation, aerospace, automobiles, civil engineering, sports medicine, electronic communications and other fields, and the prospects are promising.

[0003] A Chinese patent with authorization announcement number CN201873842U discloses a preoxidized silk needle-punched preform, which is formed by continuous needle-punching of several composite material single layers, each composite material single layer is made of two layers of preoxidized silk fiber layers and a layer of preoxidized silk mesh in the middle, and the preoxidized silk fiber layer is formed by preoxidized silk fibers that are radially evenly arranged on the upper and lower surfaces of the preoxidized silk mesh and are formed by continuous needle-punching.

[0004] The patent application with the publication number CN116373398A discloses a carbon fiber needle-punched preform and its preparation method. It includes the following steps: step 1, preparing carbon fiber plain cloth and carbon fiber mesh; step 2, after the turning layer unit layer is completed by laying a layer of carbon fiber plain cloth, it is fixed obliquely with 12K carbon fiber, and then covered with the mesh and needle-punched; step 3, after the finished layer unit layer is completed by laying a layer of carbon fiber plain cloth, it is fixed obliquely with 12K carbon fiber, and then hoop-wound with 12K carbon fiber, and finally covered with the mesh and needle-punched; step 4, the turning layer is obtained by stacking the turning layer unit layers in sequence through needle-punching, and the finished layer is obtained by stacking the finished layer unit layers in sequence through needle-punching, and the turning layer and the finished layer are needle-punched to obtain a carbon fiber needle-punched preform.

[0005] The Chinese patent with authorization announcement number CN114645462B discloses a high-performance carbon fiber needle-punched preform and a preparation method thereof, comprising: widening ordinary long carbon fiber bundles to form widened continuous long carbon fibers within a preset range of the fiber bundles; using the widened continuous long carbon fibers to prepare short-cut carbon fiber webs; using the widened continuous long carbon fibers and short-cut carbon fibers through needle-punching to prepare various types of unit layers; and composite needle-punching the same type of unit layers to prepare a high-performance carbon fiber needle-punched preform.

[0006] At present, the mainstream process for carbon fiber preforms is to carbonize the material in the deposition process. In the subsequent deposition process, it needs to go through repeated treatment processes such as high temperature, carbonization, and deposition. This requires a lot of electricity, material and manpower investment, and has a high production cost. Summary of the invention

[0007] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for needle punching an ultra-thin pre-oxidized wire felt for a flow battery electrode.

[0008] According to one aspect of the present invention, a method for preparing ultra-thin pre-oxidized wire felt for flow battery electrodes by needle punching is provided, comprising the following steps:

[0009] S1: Cut the pre-oxidized silk fibers into short fibers, spray water and treatment agent on the short fibers, the treatment agent is added in an amount of 0.5-2% by weight of the short fibers, and the water is added in an amount of 4-10% by weight of the short fibers, and dry at 30-40°C for 25-30 hours; after being opened by an opener, the short fibers are laid into a web;

[0010] S2: Arrange two layers of polyacrylonitrile preoxidized silk fibers radially on the upper and lower surfaces of the web respectively, and perform continuous needle punching to form a single-layer composite material;

[0011] S3: The single-layer composite material is cross-punctured layer by layer at multiple angles to obtain an ultra-thin pre-oxidized fiber felt for flow battery electrodes.

[0012] In some embodiments of the present invention, the short fiber length of S1 is 60-100 mm and the surface density is 100-200 g / m 2 .

[0013] In some embodiments of the present invention, the surface density of the S1 web is 100-200 g / m 2 The mesh thickness is 0.3-0.6mm.

[0014] In some embodiments of the present invention, the fiber content of the single-layer composite material S2 is 80-90%, the thickness is 0.6-0.8 mm, and the surface density is 250-350 g / cm 2 , volume density is 0.5-0.7g / cm 3 , mesh tire content 10-30%.

[0015] In some embodiments of the present invention, the acupuncture density of S2 is 35-40 needles / m 3 .

[0016] In some embodiments of the present invention, the interlayer density of S3 is controlled at 10-13 layers / cm, and the pre-puncture density is 40-45 needles / cm 3 The needle insertion depth is 15-20mm.

[0017] According to another aspect of the present invention, a method for preparing a treatment agent is provided, comprising the following steps:

[0018] H1: Mix 5-10 parts of 1,1'-bis(dimethylsilyl)iron and 30-40 parts of allyl glycidyl ether by weight;

[0019] H2: Add 1.5-3.5x10 -3 1 part of chloroplatinic acid, 0.03-0.4 part of tributyl (1-ethoxyvinyl) tin, and then stirred at 60-70 ° C for 60-120 minutes;

[0020] H3: Add 10-20 parts of double-terminated amino polyethylene glycol (CAS956496-54-1) and 1.5-3.5 parts of sodium tert-butoxide to the reactants, and continue to stir and react at 60-70°C for 60-120 minutes to obtain a treating agent.

[0021] The preparation mechanism of the above-mentioned treatment agent is as follows: 1,1'-bis(dimethylsilyl)iron undergoes a silylation reaction with allyl glycidyl ether, and then undergoes a silylation reaction with tributyl(1-ethoxyvinyl)tin, and the intermediate product then undergoes an epoxy-amino reaction with double-terminated amino polyethylene glycol to obtain a polyethylene glycol-based treatment agent containing a silicon-based iron and tin complex.

[0022] The present invention has the following beneficial effects:

[0023] 1. Improve the mechanical properties of carbon fiber:

[0024] Strengthen fiber cross-linking: By introducing a polyethylene glycol-based treatment agent containing silicon-based iron and tin complexes, a more complex three-dimensional network structure can be formed on the carbon fiber surface. This structure strengthens the cross-linking between fibers inside the carbon fiber, thereby improving the overall mechanical strength;

[0025] 2. Improve the density of polyacrylonitrile pre-oxidized yarn:

[0026] Increase filling efficiency: The use of this treatment agent can effectively improve the filling efficiency of polyacrylonitrile pre-oxidized fibers in carbon fiber felt. Higher filling efficiency means that more fibers can be used in the same volume, thereby increasing the density and mechanical properties of the carbon fiber felt; Optimize surface properties: The interaction between the active groups in the treatment agent and the polyacrylonitrile chains improves the microstructure of the fiber surface, making the fiber surface smoother, reducing defects, and further improving the uniformity and performance of the material. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0028] 1. A chemical vapor deposition experiment was performed on the needle-punched pre-oxidized fiber felts prepared in Examples 1 to 4 and Comparative Examples 1 to 3 to test the density changes before and after the chemical vapor deposition;

[0029] 2. Test the bending mechanical properties using the 3385H universal mechanical strength tester.

[0030] Example 1: A method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes by needle punching, wherein the steps are as follows:

[0031] S1: Cut the pre-oxidized silk fibers into short fibers, spray water and treatment agent on the short fibers, the treatment agent is added in an amount of 0.5% by weight of the short fibers, and the water is added in an amount of 4% by weight of the short fibers, and dry at 30°C for 25 hours; after being opened by an opener, the short fibers are laid into a web;

[0032] S2: Arrange two layers of polyacrylonitrile preoxidized silk fibers radially on the upper and lower surfaces of the web respectively, and perform continuous needle punching to form a single-layer composite material;

[0033] S3: The single-layer composite material is cross-punctured layer by layer at multiple angles to obtain an ultra-thin pre-oxidized fiber felt for flow battery electrodes.

[0034] The short fiber length of S1 is 60 mm and the surface density is 100 g / m 2 .

[0035] The surface density of the S1 web is 100 g / m 2 , the mesh thickness is 0.3mm.

[0036] The fiber content of the single-layer composite material of S2 is 80%, the thickness is 0.6mm, and the surface density is 250g / cm 2 , volume density is 0.5g / cm 3 , mesh tire content 10%.

[0037] The needle density of S2 is 35 needles / m 3 .

[0038] The interlayer density of S3 is controlled at 10 layers / cm, and the pre-puncture density is 40 needles / cm 3 The needle insertion depth is 15mm.

[0039] The preparation method of the treating agent is:

[0040] H1: Mix 5 g of 1,1'-bis(dimethylsilyl)iron and 30 g of allyl glycidyl ether;

[0041] H2: Add 1.5x10 -3 g chloroplatinic acid, 0.03 g tributyl(1-ethoxyvinyl)tin, and then stirred at 60°C for 60 minutes;

[0042] H3: 10 g of double-terminated amino polyethylene glycol (CAS 956496-54-1) and 1.5 g of sodium tert-butoxide were added to the reactants, and the mixture was stirred and reacted at 60° C. for 60 minutes to obtain a treating agent.

[0043] Example 2: A method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes by needle punching, wherein the steps are as follows:

[0044] S1: Cut the pre-oxidized silk fibers into short fibers, spray water and treatment agent on the short fibers, the treatment agent is added in an amount of 1% by weight of the short fibers, and the water is added in an amount of 6% by weight of the short fibers, and dry at 35°C for 26 hours; after being opened by an opener, the short fibers are laid into a web;

[0045] S2: Arrange two layers of polyacrylonitrile preoxidized silk fibers radially on the upper and lower surfaces of the web respectively, and perform continuous needle punching to form a single-layer composite material;

[0046] S3: The single-layer composite material is cross-punctured layer by layer at multiple angles to obtain an ultra-thin pre-oxidized fiber felt for flow battery electrodes.

[0047] The short fiber length of S1 is 70 mm and the surface density is 140 g / m 2 .

[0048] The surface density of the S1 web is 140 g / m 2 , the mesh thickness is 0.4mm.

[0049] The fiber content of the single-layer composite material of S2 is 85%, the thickness is 0.7mm, and the surface density is 280g / cm 2 , the volume density is 0.6g / cm 3 , mesh content 15%.

[0050] The needle density of S2 is 36 needles / m 3 .

[0051] The interlayer density of S3 is controlled at 11 layers / cm, and the pre-puncture density is 42 needles / cm 3 The needle insertion depth is 16mm.

[0052] The preparation method of the treating agent is:

[0053] H1: Mix 6 g of 1,1'-bis(dimethylsilyl)iron and 33 g of allyl glycidyl ether;

[0054] H2: Add 2x10 -3 g chloroplatinic acid, 0.1 g tributyl(1-ethoxyvinyl)tin, and then stirred at 65°C for 80 minutes;

[0055] H3: 13 g of double-terminated amino polyethylene glycol (CAS 956496-54-1) and 2 g of sodium tert-butoxide were added to the reactants, and the mixture was stirred and reacted at 65° C. for 80 minutes to obtain a treating agent.

[0056] Example 3: A method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes by needle punching, wherein the steps are as follows:

[0057] S1: Cut the pre-oxidized silk fibers into short fibers, spray water and treatment agent on the short fibers, the treatment agent is added in an amount of 1.5% by weight of the short fibers, and the water is added in an amount of 8% by weight of the short fibers, and dry at 35°C for 28 hours; after being opened by an opener, the short fibers are laid into a web;

[0058] S2: Arrange two layers of polyacrylonitrile preoxidized silk fibers radially on the upper and lower surfaces of the web respectively, and perform continuous needle punching to form a single-layer composite material;

[0059] S3: The single-layer composite material is cross-punctured layer by layer at multiple angles to obtain an ultra-thin pre-oxidized fiber felt for flow battery electrodes.

[0060] The short fiber length of S1 is 90 mm and the surface density is 180 g / m 2 .

[0061] The surface density of the S1 web is 180 g / m 2 , the mesh thickness is 0.5mm.

[0062] The fiber content of the single-layer composite material of S2 is 85%, the thickness is 0.7mm, and the surface density is 330g / cm 2 , the volume density is 0.6g / cm 3 , mesh content 25%.

[0063] The needle density of S2 is 39 needles / m 3 .

[0064] The interlayer density of S3 is controlled at 12 layers / cm, and the pre-puncture density is 44 needles / cm 3 The needle insertion depth is 18mm.

[0065] The preparation method of the treating agent is:

[0066] H1: Mix 8 g of 1,1'-bis(dimethylsilyl)iron and 38 g of allyl glycidyl ether;

[0067] H2: Add 2.5x10 -3 g chloroplatinic acid, 0.3 g tributyl(1-ethoxyvinyl)tin, and then stirred at 65°C for 100 minutes;

[0068] H3: 18 g of double-terminated amino polyethylene glycol (CAS 956496-54-1) and 3 g of sodium tert-butoxide were added to the reactants, and the mixture was stirred and reacted at 65° C. for 100 minutes to obtain a treating agent.

[0069] Example 4: A method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes by needle punching, wherein the steps are as follows:

[0070] S1: Cut the pre-oxidized silk fibers into short fibers, spray water and treatment agent on the short fibers, the treatment agent is added in an amount of 2% by weight of the short fibers, and the water is added in an amount of 10% by weight of the short fibers, and dry at 40°C for 30 hours; after being opened by an opener, the short fibers are laid into a web;

[0071] S2: Arrange two layers of polyacrylonitrile preoxidized silk fibers radially on the upper and lower surfaces of the web respectively, and perform continuous needle punching to form a single-layer composite material;

[0072] S3: The single-layer composite material is cross-punctured layer by layer at multiple angles to obtain an ultra-thin pre-oxidized fiber felt for flow battery electrodes.

[0073] The short fiber length of S1 is 100 mm and the surface density is 200 g / m 2 .

[0074] The surface density of the S1 web is 200 g / m 2 , the mesh thickness is 0.6mm.

[0075] The fiber content of the single-layer composite material of S2 is 90%, the thickness is 0.8mm, and the surface density is 350g / cm 2 , the volume density is 0.7g / cm 3 , mesh tire content 30%.

[0076] The needle density of S2 is 40 needles / m 3 .

[0077] The interlayer density of S3 is controlled at 13 layers / cm, and the pre-puncture density is 45 needles / cm 3 The needle insertion depth is 20mm.

[0078] The preparation method of the treating agent is:

[0079] H1: Mix 10 g of 1,1'-bis(dimethylsilyl)iron and 40 g of allyl glycidyl ether;

[0080] H2: Add 3.5x10 -3 g chloroplatinic acid, 0.4 g tributyl(1-ethoxyvinyl)tin, and then stirred at 70°C for 120 minutes;

[0081] H3: Add 20 g of double-terminated amino polyethylene glycol (CAS 956496-54-1) and 3.5 g of sodium tert-butoxide to the reactant, and continue to stir and react at 70° C. for 120 minutes to obtain a treating agent.

[0082] Comparative Example 1: For comparison, no treatment agent was added in this example, and the rest was the same as in Example 1.

[0083] Comparative Example 2: For comparison, in this example, tributyl (1-ethoxyvinyl) tin is not added, and the rest is the same as in Example 1.

[0084] Comparative Example 3: For comparison, in this example, 1,1'-bis(dimethylsilyl)iron is not added, and the rest is the same as in Example 1.

[0085] Table 1: Test results of various embodiments and comparative examples

[0086]

[0087] Through the data analysis of the above embodiments and comparative examples, the treating agent prepared by the present invention improves the overall mechanical strength of the ultra-thin pre-oxidized fiber felt and simultaneously increases the density of the polyacrylonitrile pre-oxidized fiber.

[0088] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes by needle punching, characterized in that: The operation steps are: S1: Cut the pre-oxidized silk fibers into short fibers, spray water and treatment agent on the short fibers, the treatment agent is added in an amount of 0.5-2% by weight of the short fibers, and the water is added in an amount of 4-10% by weight of the short fibers, and dry at 30-40°C for 25-30 hours; after being opened by an opener, the short fibers are laid into a web; The preparation method of the treatment agent of S1 is: H1: Mix 5-10 parts of 1,1'-bis(dimethylsilyl)iron and 30-40 parts of allyl glycidyl ether by weight; H2: Add 1.5-3.5x10 -3 1 part of chloroplatinic acid, 0.03-0.4 part of tributyl (1-ethoxyvinyl) tin, and then stirred at 60-70 ° C for 60-120 minutes; H3: Add 10-20 parts of double-terminated amino polyethylene glycol and 1.5-3.5 parts of sodium tert-butoxide to the reactants, and continue to stir and react at 60-70°C for 60-120 minutes to obtain a treating agent; S2: Arrange two layers of polyacrylonitrile preoxidized silk fibers radially on the upper and lower surfaces of the web respectively, and perform continuous needle punching to form a single-layer composite material; S3: The single-layer composite material is cross-punctured layer by layer at multiple angles to obtain an ultra-thin pre-oxidized fiber felt for flow battery electrodes.

2. The method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes according to claim 1, characterized in that: The short fiber length of S1 is 60-100mm and the surface density is 100-200g / m 2 .

3. The method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes according to claim 1, characterized in that: The mesh thickness of S1 is 0.3-0.6 mm.

4. The method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes according to claim 1, characterized in that: The fiber content of the single-layer composite material of S2 is 80-90%, the thickness is 0.6-0.8mm, and the surface density is 250-350g / cm 2 , volume density is 0.5-0.7g / cm 3 , mesh tire content 10-30%.

5. The method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes according to claim 1, characterized in that: The needle density of S2 is 35-40 needles / m 3 .

6. The method for preparing ultra-thin pre-oxidized silk felt for flow battery electrodes according to claim 1, characterized in that: The interlayer density of S3 is controlled at 10-13 layers / cm, and the pre-puncture density is 40-45 needles / cm 3 The needle insertion depth is 15-20mm.

Citation Information

Patent Citations

  • A high-performance carbon fiber needle-punched preform and preparation method thereof

    CN114645462B

  • Carbon fiber needling preform and preparation method thereof

    CN116373398A

  • PANOF (Polyacrylonitrile Oxidized Fiber) acupuncture preform

    CN201873842U

  • Continuous fiber reinforced PET (Polyethylene Terephthalate) composite material for automobile wheel cover and preparation method of continuous fiber reinforced PET composite material

    CN116219642A

  • Ultrahigh-temperature-resistant self-healing multifunctional gradient gradient carbon fiber reinforced ceramic matrix composite flat plate component

    CN116589296A