Composite sodium ion positive electrode material, preparation method and sodium ion battery
By introducing carbon doping into sodium ferric sulfate material and using a preparation method combining wet and dry methods, the problem of insufficient sodium storage capacity and cycle stability of sodium ferric sulfate material is solved, and high sodium storage capacity and good quality are achieved electrochemical properties.
Patent Information
- Application Number
- CN202410909382.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing sodium ferric sulfate materials have poor performance in terms of specific capacity, cycle stability and rate performance, and there are problems of impurity phase generation and low conductivity.
Carbon-doped sodium ferrosulfate particles are prepared by wet and dry methods on the inside and outside of the sodium ferrosulfate particles to form a composite sodium ion positive electrode material. The dispersion and structural stability of the carbon material are improved, thereby improving Sodium storage specific capacity and circulation performance.
It significantly improves the specific capacity and cyclic stability of composite sodium ion positive electrode materials, enhances electrochemical performance, and is suitable for low-speed electric vehicles and energy storage fields.
Smart Images

Figure CN118472226B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a composite sodium ion positive electrode material, a preparation method and a sodium ion battery. Background Art
[0002] Sodium iron sulfate positive electrode material has the remarkable characteristics of low cost, high voltage, long cycle, and high safety performance. It is very suitable for application scenarios such as electric vehicles and energy storage. However, it is limited by conventional synthesis processes. The sodium iron sulfate material itself has the characteristics of easy generation of impurity phases, low electrical conductivity, and poor sodium storage performance, which manifests as lower sodium storage specific capacity, poor cycle stability and rate performance. Summary of the invention
[0003] In view of the problems existing in the above-mentioned prior art, the present application provides a composite sodium ion positive electrode material, a preparation method and a sodium ion battery, and the technical solution is as follows:
[0004] On the one hand, the present application provides a composite sodium ion positive electrode material, including carbon-doped sodium iron sulfate particles, wherein the molecular formula of the sodium iron sulfate particles is Na x Fe y (SO4) x / 2+y , the x / y ratio inside the carbon-doped sodium iron sulfate particle is smaller than the x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particle.
[0005] Furthermore, the ratio of x / y gradually increases from the inside to the outer layer of the carbon-doped sodium iron sulfate particles.
[0006] Furthermore, in the direction from the inside to the outside of the carbon-doped sodium iron sulfate particles, the increasing gradient of the ratio of x / y is less than or equal to the target increasing gradient, and the target increasing gradient is 0.10 / 10% to 0.18 / 10% of the particle diameter.
[0007] Furthermore, the composite sodium ion positive electrode material satisfies at least one of the following characteristics:
[0008] The ratio of x / y in the carbon-doped sodium iron sulfate particles is 1.2:1 to 1.8:1;
[0009] The x / y ratio inside the carbon-doped sodium iron sulfate particles is 1:1 to 1.5:1;
[0010] The x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particles is 1.5:1 to 2.0:1.
[0011] Furthermore, the carbon material in the carbon-doped sodium iron sulfate particles satisfies at least one of the following characteristics:
[0012] The carbon material comprises at least one of graphite, graphene, carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes and Ketjen black;
[0013] The mass proportion of the carbon material in the carbon-doped sodium iron sulfate particles is 0.1% to 10%;
[0014] The carbon material accounts for 0.1% to 10% by mass of the outer layer of the carbon-doped sodium iron sulfate particles.
[0015] Furthermore, the composite sodium ion positive electrode material forms carbon-doped sodium iron sulfate particles through a sodium source, an iron source and a carbon source, wherein the sodium source includes a first sodium source and a second sodium source, the iron source includes a first iron source and a second iron source, and the sodium source and the iron source are used to react to generate sodium iron sulfate; the carbon source includes a first carbon source and a second carbon source, and the carbon source is used to form the carbon material in the composite sodium ion positive electrode material;
[0016] The composite sodium ion positive electrode material includes a composite inner layer and a composite outer layer, wherein the composite outer layer is coated on the composite inner layer; the composite inner layer is prepared by wet method using a first sodium source, a first iron source and a first carbon source, and the composite outer layer is prepared by dry method using a second sodium source, a second iron source and a second carbon source.
[0017] On the other hand, the present application also provides a method for preparing a composite sodium ion positive electrode material, wherein carbon-doped sodium iron sulfate particles are formed by a sodium source, an iron source and a carbon source; the molecular formula of the sodium iron sulfate particles is Na x Fe y (SO4) x / 2+y , the x / y ratio inside the carbon-doped sodium iron sulfate particle is smaller than the x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particle.
[0018] Furthermore, the method comprises:
[0019] Dispersing a first sodium source, a first iron source, a first carbon source, and an antioxidant in deionized water to form a mixed slurry;
[0020] Drying the mixed slurry to obtain a first precursor;
[0021] Mixing a second sodium source, a second iron source and a second carbon source to obtain a second precursor; the ratio of x / y in the first precursor is less than the ratio of x / y in the second precursor;
[0022] The first precursor and the second precursor are mixed and ball-milled to obtain a composite precursor; the particle size of the first precursor is larger than the particle size of the second precursor, and during the mixing and ball-milling process, the second precursor covers the first precursor;
[0023] The composite precursor is sintered and crushed to obtain the composite sodium ion positive electrode material.
[0024] Further, the step of drying the mixed slurry to obtain a first precursor comprises:
[0025] Initially drying the mixed slurry to obtain a first initial precursor;
[0026] The first initial precursor is dehydrated to obtain the first precursor; during the dehydration process, the crystal water content in the first initial precursor is reduced.
[0027] Furthermore, the first initial precursor is Na x Fe y (SO4) x / 2+y 4H2O@C, where the ratio of x / y is 1:1 to 1.5:1;
[0028] The initial drying includes at least one of spray drying, vacuum drying, vibration drying and freeze drying.
[0029] Furthermore, the first precursor is Na x Fe y (SO4) x / 2+y @C, wherein the ratio of x / y is 1:1 to 1.5:1; during the dehydration process, the dehydration temperature is 200°C to 300°C, and the dehydration time is 4h to 12h.
[0030] Further, the mixing of the second sodium source, the second iron source and the second carbon source to obtain the second precursor comprises:
[0031] Pre-crushing the second sodium source and the second iron source to obtain a crushed dry material;
[0032] The crushed dry material is mixed with the second carbon source to obtain the second precursor.
[0033] Furthermore, in the process of mixing and ball-milling the first precursor and the second precursor to obtain a composite precursor, the method satisfies at least one of the following characteristics:
[0034] The mass ratio of the first precursor to the second precursor is 0.5:1 to 5:1;
[0035] The median particle size of the first precursor is 20 μm to 50 μm; the median particle size of the second precursor is 2 μm to 5 μm.
[0036] Furthermore, the antioxidant satisfies at least one of the following characteristics:
[0037] The antioxidant comprises at least one of ascorbic acid, oxalic acid and citric acid;
[0038] The weight proportion of the antioxidant in the total weight of the first sodium source, the first iron source, the first carbon source and the antioxidant is 0.1% to 2%.
[0039] Furthermore, in the process of sintering and crushing the composite precursor, the sintering temperature is 350° C. to 400° C., and the sintering time is 10 h to 20 h.
[0040] On the other hand, the present application also provides a sodium ion battery, comprising the composite sodium ion positive electrode material as described in any of the above items, or comprising a composite sodium ion positive electrode material prepared by the preparation method of the composite sodium ion positive electrode material as described in any of the above items.
[0041] Implementing this application has the following beneficial effects:
[0042] 1. In the composite sodium ion positive electrode material of the present application, the molecular formula of the sodium iron sulfate particles is Na x Fe y (SO4) x / 2+y The x / y ratio inside the carbon-doped sodium ferric sulfate particles is smaller than the x / y ratio of the outer layer of the carbon-doped sodium ferric sulfate particles, which can improve the mixing uniformity of the internal carbon material and the sodium ferric sulfate particles, reduce the impurities in the carbon-doped sodium ferric sulfate particles, and is beneficial to improving the specific capacity of the composite sodium ion positive electrode material; at the same time, the x / y ratio of the outer layer is relatively large, which can improve the structural stability of the outer layer of the carbon-doped sodium ferric sulfate particles, and is beneficial to improving the cycle stability of the composite sodium ion positive electrode material, thereby synergistically improving the specific capacity and cycle performance of the composite sodium ion positive electrode material.
[0043] 2. In the composite sodium ion positive electrode material of the present application, the interior of the carbon-doped sodium ferric sulfate particles is prepared by a wet method, which can greatly improve the mixing uniformity between various raw materials, reduce the generation of impurities during the preparation process, and greatly improve the specific capacity of the composite sodium ion positive electrode material; at the same time, the outer layer of the carbon-doped sodium ferric sulfate particles is prepared by a dry method, which can improve the structural stability of the outer layer of the carbon-doped sodium ferric sulfate particles, and can also synergistically improve the conductivity of the outer layer of the carbon-doped sodium ferric sulfate particles, thereby further improving the overall electrochemical performance of the composite sodium ion positive electrode material; and the preparation method has simple steps, readily available raw materials, and environmentally friendly processes. Through the organic combination of wet and dry processes, the prepared composite sodium ion positive electrode material has excellent electrochemical properties, can be widely used in low-speed electric vehicles, energy storage and other fields, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the embodiments, wherein the same components are represented by the same reference numerals. Obviously, the drawings described below are only some embodiments of the present application, and for those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0045] Figure 1 A cross-sectional SEM image of a composite sodium ion positive electrode material provided in Example 1 of the present application;
[0046] Figure 2 A cross-sectional SEM image of a composite sodium ion positive electrode material provided in Example 2 of the present application;
[0047] Figure 3 An XRD graph of a composite sodium ion positive electrode material provided in Example 1 of the present application;
[0048] Figure 4 This is a charge and discharge curve diagram of a composite sodium ion positive electrode material provided in Example 1 of the present application applied in a sodium ion battery. DETAILED DESCRIPTION
[0049] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments, and therefore cannot be understood as limiting the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0050] It should be noted that in the description of the present application, for the following defined terms, unless a different definition is given in the claims or elsewhere in this specification, these definitions should be applied. All numerical values, whether or not explicitly indicated, are defined herein as being modified by the term "about". The term "about" generally refers to a numerical range that a person of ordinary skill in the art would consider to be equivalent to the stated value to produce substantially the same properties, functions, results, etc. A numerical range indicated by a low value and a high value is defined to include all numerical values included in the numerical range and all subranges included in the numerical range.
[0051] It should be noted that the terms "first", "second", etc. in the specification, claims and drawings of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the objects used in this way can be interchanged where appropriate, so that the embodiments of the present application can be implemented in a sequence other than the following diagrams or the following descriptions. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, the process, method, system, product comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, or products.
[0052] The existing sodium iron sulfate materials have poor sodium storage capacity, cycle stability and rate performance. In order to solve at least one of the above problems, the present invention provides a composite sodium ion positive electrode material and a preparation method thereof. The composite sodium ion positive electrode material includes carbon-doped sodium iron sulfate particles, wherein the carbon material is dispersed between the sodium iron sulfate particles, and the molecular formula of the sodium iron sulfate particles is Na x Fe y (SO4) x / 2+y , where the x / y ratio inside the carbon-doped sodium iron sulfate particle is smaller than the x / y ratio outside the carbon-doped sodium iron sulfate particle, and the x / y ratio inside is relatively small. x Fe y (SO4) x / 2+y As for the material, its sodium storage capacity increases with the decrease of the ratio of x / y, thereby providing a good sodium storage capacity for the carbon-doped sodium iron sulfate particles; while the decrease of the ratio of x / y is not conducive to the Na x Fe y (SO4) x / 2+y The structural stability of the material, the ratio of the outer layer x / y is relatively large, and the outer layer of the carbon-doped sodium iron sulfate particles is coated on the inner part of the carbon-doped sodium iron sulfate particles, which can reduce the Fe 2+ / Fe 3+ Redox and more Na + The carbon-doped sodium iron sulfate particles are deintercalated and the structural stability is synergistically improved through the coating structure, so that the carbon-doped sodium iron sulfate particles as a whole have high sodium storage capacity, high rate performance, good structural stability and cycle performance.
[0053] Specifically, in some exemplary embodiments, the ratio of x / y gradually increases from the inside to the outer layer of the carbon-doped sodium iron sulfate particles, and a certain gradient distribution can be formed, thereby further achieving a synergistic improvement in the sodium storage capacity and the cycle performance, and greatly improving the electrochemical performance of the carbon-doped sodium iron sulfate particles and the sodium ion battery having the carbon-doped sodium iron sulfate particles.
[0054] In some exemplary embodiments, the outer layer of the carbon-doped sodium ferric sulfate particle includes at least one outer layer; exemplarily, the outer layer of the carbon-doped sodium ferric sulfate particle includes one outer layer, and the x / y ratio in the outer layer is greater than the x / y ratio inside the carbon-doped sodium ferric sulfate particle; exemplarily, the outer layer of the carbon-doped sodium ferric sulfate particle includes two outer layers, the two outer layers are respectively a first outer layer and a second outer layer, the first outer layer is coated on the inside of the carbon-doped sodium ferric sulfate particle, and the second outer layer is coated on the first outer layer, the x / y ratio in the first outer layer is greater than the x / y ratio inside the carbon-doped sodium ferric sulfate, and the x / y ratio in the second outer layer is greater than the x / y ratio in the first outer layer, so that the carbon-doped sodium ferric sulfate particle as a whole forms a structure in which the x / y ratio gradually increases from the inside to the outer layer, thereby synergistically improving the sodium storage capacity, conductivity, structural stability and cycle stability of the carbon-doped sodium ferric sulfate particle.
[0055] Specifically, along the direction from the inside to the outer layer of the carbon-doped sodium iron sulfate particles, the increasing gradient of the x / y ratio is less than or equal to the target increasing gradient, and the target increasing gradient is 0.10 / 10% to 0.18 / 10% of the particle diameter; it can be understood that the target increasing gradient can be any point value between 0.10 / 10% to 0.18 / 10% of the particle diameter; illustratively, the target increasing gradient can be 0.10 / 10% of the particle diameter, 0.11 / 10% of the particle diameter, 0.12 / 10% of the particle diameter, 0.15 / 10% of the particle diameter, 0.16 / 10% of the particle diameter, 0.17 / 10% of the particle diameter , 0.18 / 10% particle diameter, etc.; in this way, the compatibility and contact tightness between the interior of the carbon-doped sodium ferric sulfate particle and the outer layer of the carbon-doped sodium ferric sulfate particle can be improved, the stratification and isolation of the carbon-doped sodium ferric sulfate particle's own structure can be avoided, and a good sodium ion transmission path can be provided, which is beneficial to synergistically improve the overall self-structural stability and conductivity of the carbon-doped sodium ferric sulfate particle; illustratively, in a specific embodiment, the target incremental gradient is 0.17 / 10% particle diameter, that is, along the direction from the inside to the outer layer of the carbon-doped sodium ferric sulfate particle, the incremental gradient of the x / y ratio is less than or equal to 0.17 / 10% particle diameter.
[0056] Specifically, the x / y ratio inside the carbon-doped sodium ferric sulfate particles is 1:1 to 1.5:1; it can be understood that the x / y ratio inside the carbon-doped sodium ferric sulfate particles can be any point value between 1:1 and 1.5:1; illustratively, the x / y ratio inside the carbon-doped sodium ferric sulfate particles can be 1:1, 1.1:1, 1.15:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, etc.; in this way, the x / y ratio inside the carbon-doped sodium ferric sulfate particles is relatively small, which can effectively improve the specific capacity of the composite sodium ion positive electrode material, and improve the rate performance of the composite sodium ion positive electrode material and the sodium ion battery having the composite sodium ion positive electrode material.
[0057] Specifically, the x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particle is 1.5:1 to 2.0:1; it can be understood that the x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particle can be any point value in the range of 1.5:1 to 2.0:1; illustratively, the x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particle can be 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2.0:1, etc.; in this way, the x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particle is relatively large, which can effectively reduce Fe 2+ / Fe 3+ Redox and Na + The deintercalation and embedding of the composite sodium ion positive electrode material is beneficial to improving the structural stability of the composite sodium ion positive electrode material and improving the cycle performance of the composite sodium ion positive electrode material and the sodium ion battery having the composite sodium ion positive electrode material.
[0058] Specifically, in some exemplary embodiments, the ratio of x / y in the carbon-doped sodium iron sulfate particles is 1.2:1 to 1.8:1; it can be understood that the ratio of x / y in the carbon-doped sodium iron sulfate particles can be any point value in the range of 1.2:1 to 1.8:1; illustratively, the ratio of x / y in the carbon-doped sodium iron sulfate particles can be 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, etc.; in this way, the composite sodium ion positive electrode material as a whole can have a higher sodium storage specific capacity, higher conductivity and excellent structural stability, thereby improving the rate performance and cycle performance of the composite sodium ion positive electrode material and a sodium ion battery having the composite sodium ion positive electrode material.
[0059] In some preferred embodiments, the ratio of x / y in the carbon-doped sodium iron sulfate particles is 1.4:1 to 1.6:1.
[0060] Specifically, the carbon material in the carbon-doped sodium iron sulfate particles includes at least one of graphite, graphene, carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes and Ketjen black, has good electrical conductivity, can effectively enhance the electrical conductivity between ions, reduce the risk of battery polarization caused by the application of the carbon-doped sodium iron sulfate particles in sodium ion batteries, and can also inhibit grain growth, shorten the transmission path of sodium ions in the carbon-doped sodium iron sulfate particles, improve the sodium ion transmission efficiency, and greatly improve the conductivity of the composite sodium ion positive electrode material.
[0061] Specifically, the mass proportion of the carbon material in the carbon-doped sodium ferric sulfate particles is 0.1% to 10%; it can be understood that the mass proportion of the carbon material in the carbon-doped sodium ferric sulfate particles can be any point value between 0.1% and 10%; illustratively, the mass proportion of the carbon material in the carbon-doped sodium ferric sulfate particles can be 0.1%, 0.7%, 1.0%, 1.5%, 2.0%, 3.0%, 5.0%, 8.0%, 10%, etc.; in this way, the electrical conductivity inside the carbon-doped sodium ferric sulfate particles can be improved, which is beneficial to improve the overall electrical conductivity and electrochemical properties of the carbon-doped sodium ferric sulfate particles.
[0062] Specifically, the mass proportion of the carbon material in the outer layer of the carbon-doped sodium ferric sulfate particles is 0.1% to 10%; it can be understood that the mass proportion of the carbon material in the outer layer of the carbon-doped sodium ferric sulfate particles can be any point value between 0.1% and 10%; illustratively, the mass proportion of the carbon material in the outer layer of the carbon-doped sodium ferric sulfate particles can be 0.1%, 0.7%, 1.0%, 1.5%, 2.0%, 3.0%, 5.0%, 8.0%, 10%, etc.; in this way, the conductivity of the outer layer of the carbon-doped sodium ferric sulfate particles can be improved, and the dispersion uniformity of the carbon material in the outer layer of the carbon-doped sodium ferric sulfate is better. The carbon-doped sodium ferric sulfate outer layer with carbon material covers the interior of the carbon-doped sodium ferric sulfate, which can further improve the overall conductivity, conductive uniformity and electrochemical properties of the carbon-doped sodium ferric sulfate particles.
[0063] Specifically, the composite sodium ion positive electrode material forms carbon-doped sodium ferric sulfate particles through a sodium source, an iron source and a carbon source, wherein the sodium source and the iron source are used to react to generate sodium ferric sulfate, and the carbon source is used to form the carbon material in the composite sodium ion positive electrode material.
[0064] In some exemplary embodiments, the sodium source includes a first sodium source and a second sodium source, the iron source includes a first iron source and a second iron source, the carbon source includes a first carbon source and a second carbon source, the composite sodium ion positive electrode material includes a composite inner layer and a composite outer layer coated on the composite inner layer, and the ratio of x / y in the composite inner layer is less than the ratio of x / y in the composite outer layer; wherein the composite inner layer is prepared by wet process of the first sodium source, the first iron source and the first carbon source, and the composite outer layer is prepared by dry process of the second sodium source, the second iron source and the second carbon source, and the dry process can be organically combined to achieve dry process. The effective mixing of raw materials that is difficult to achieve by the wet ball milling process can greatly reduce the generation of impurities inside the carbon-doped sodium ferric sulfate particles, and can achieve the dispersion of carbon materials that is difficult to achieve by the wet precursor calcination process, greatly improving the dispersion of various materials in the outer layer of the carbon-doped sodium ferric sulfate particles. At the same time, the outer layer of the carbon-doped sodium ferric sulfate particles has carbon materials formed by dry coating, which can further improve the conductivity of the outer layer of the carbon-doped sodium ferric sulfate particles, thereby synergistically improving the overall specific capacity, conductivity, rate performance, stability, cycle performance and other properties of the composite sodium ion positive electrode material.
[0065] In some exemplary embodiments, the sodium source is sodium sulfate, and the first iron source includes ferrous sulfate heptahydrate, so as to facilitate wet preparation, have good preparation convenience, can stably and effectively generate sodium ferric sulfate, reduce the generation of impurities, and improve the specific capacity of the carbon-doped sodium ferric sulfate; the second iron source includes at least one of ferrous sulfate heptahydrate, ferrous sulfate monohydrate and ferrous sulfate, and can stably and effectively perform dry preparation to obtain sodium ferric sulfate; the carbon source includes at least one of graphite, graphene, carbon black, single-walled carbon nanotubes, multi-walled carbon nanotubes and Ketjen black, and has good conductivity. Dry coating with the second iron source and the second sodium source can greatly improve the structural stability and conductivity of the outer layer of the carbon-doped sodium ferric sulfate particles, thereby improving the overall cycle performance and electrochemical performance of the composite sodium ion positive electrode material.
[0066] In addition, in some exemplary embodiments, the composite sodium ion positive electrode material includes at least one composite inner layer and at least one composite outer layer; exemplarily, the composite sodium ion positive electrode material includes a composite inner layer and a composite outer layer; exemplarily, the composite sodium ion positive electrode material includes at least two composite inner layers and a composite outer layer, each composite inner layer is prepared by a wet process, and the ratio of x / y in at least two composite inner layers gradually increases from the composite inner layer to the composite outer layer; exemplarily, the composite sodium ion positive electrode material includes at least two composite inner layers and at least two composite outer layers, and the composite inner layers and the composite outer layers are alternately arranged in a direction toward the outer layer; exemplarily, in the case where the composite sodium ion positive electrode material includes a composite inner layer and at least two composite outer layers, the ratio of x / y in at least two composite outer layers gradually increases from the composite inner layer to the composite outer layer, so as to further improve the performance of the composite sodium ion positive electrode material.
[0067] On the other hand, the present application also provides a method for preparing a composite sodium ion positive electrode material, wherein carbon-doped sodium iron sulfate particles are formed by a sodium source, an iron source and a carbon source; the molecular formula of the sodium iron sulfate particles is Na x Fe y (SO4) x / 2+y The x / y ratio inside the carbon-doped sodium ferric sulfate particle is smaller than the x / y ratio of the outer layer of the carbon-doped sodium ferric sulfate particle, so as to improve the sodium storage capacity inside the carbon-doped sodium ferric sulfate and the structural stability of the outer layer of the carbon-doped sodium ferric sulfate, thereby improving the overall sodium storage capacity and structural stability of the composite sodium ion positive electrode material, and improving the conductivity, rate performance and cycle performance of the composite sodium ion positive electrode material and the sodium ion battery having the composite sodium ion positive electrode material.
[0068] Specifically, in some exemplary embodiments, the method includes:
[0069] S1, dispersing a first sodium source, a first iron source, a first carbon source and an antioxidant in deionized water to form a mixed slurry;
[0070] S2, drying the mixed slurry to obtain a first precursor;
[0071] S3, mixing a second sodium source, a second iron source and a second carbon source to obtain a second precursor; the ratio of x / y in the first precursor is less than the ratio of x / y in the second precursor;
[0072] S4, mixing and ball-milling the first precursor and the second precursor to obtain a composite precursor; the particle size of the first precursor is larger than that of the second precursor, and during the mixing and ball-milling process, the second precursor covers the first precursor;
[0073] S5, sintering and crushing the composite precursor to obtain the composite sodium ion positive electrode material.
[0074] Among them, step S1 adopts a wet process, and through subsequent drying, a first precursor is prepared. The wet process makes the mixing of various raw materials more uniform, that is, the mixing of the first sodium source, the first iron source, the first carbon source and the antioxidant is relatively uniform, especially the first sodium source, the first iron source and the antioxidant are evenly mixed, with less impurities, which can provide a higher specific capacity for the final composite sodium ion positive electrode material; and steps S3 to S4 adopt dry ball milling, which can increase the dispersibility of the carbon source in the first precursor and the second precursor, which is beneficial to improving the uniformity of the dispersion of the carbon material in the composite sodium ion positive electrode material, and dry ball milling is beneficial to improving the structural stability of the composite sodium ion positive electrode material, thereby synergistically improving the conductivity and cycle performance of the composite sodium ion positive electrode material.
[0075] Specifically, in step S1, the first sodium source and the first iron source dispersed in deionized water are added according to an x / y ratio of 1:1 to 1.5:1, that is, the x / y ratio in the mixed slurry is 1:1 to 1.5:1; it can be understood that the x / y ratio in the mixed slurry can be any point value in the range of 1:1 to 1.5:1, which is not enumerated here; in this way, the x / y ratio in the first precursor prepared subsequently can also reach 1:1 to 1.5:1, and the x / y ratio is relatively small, so that in the finally formed composite sodium ion positive electrode material, the carbon-doped sodium iron sulfate particles can have a relatively small x / y ratio, thereby improving the sodium storage capacity of the carbon-doped sodium iron sulfate particles and improving the charge and discharge performance of the composite sodium ion positive electrode material.
[0076] Specifically, in some exemplary embodiments, the mass proportion of the first carbon source in the total mass of the first sodium source, the first iron source, the first carbon source and the antioxidant is 0.1% to 10%; it can be understood that the mass proportion of the first carbon source in the total mass of the first sodium source, the first iron source, the first carbon source and the antioxidant can be any point value in the range of 0.1% to 10%, which is not enumerated here; in this way, the transmission efficiency of sodium ions in the first precursor can be improved to a certain extent, and the conductivity of the first precursor and the finally obtained composite sodium ion positive electrode material can be improved.
[0077] Specifically, in step S1, the antioxidant includes at least one of ascorbic acid, oxalic acid and citric acid, and has excellent antioxidant properties; this step adopts a wet preparation process, and the antioxidant can effectively prevent the divalent iron ions (Fe 2+ ) is oxidized to trivalent iron ions (Fe 3+ ), to avoid the decrease of electrical properties such as capacity and capacity retention rate of the prepared sodium iron sulfate.
[0078] Specifically, in some exemplary embodiments, in step S1, the weight proportion of the antioxidant in the total weight of the first sodium source, the first iron source, the first carbon source and the antioxidant is 0.1% to 2%; it can be understood that the weight proportion of the antioxidant in the total weight of the first sodium source, the first iron source, the first carbon source and the antioxidant can be any point value in the range of 0.1% to 2%; exemplarily, the weight proportion can be 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1.0%, 1.5%, 2%, etc.; in this way, the Fe in the first iron source can be effectively prevented from being 2+ Oxidized, the electrical properties of the carbon-doped sodium iron sulfate particles, such as sodium storage capacity and capacity retention rate, are improved.
[0079] Specifically, in step S1, the total mass of the first sodium source, the first iron source, the first carbon source and the antioxidant in the mixed slurry accounts for 25% to 50% by mass. Correspondingly, the mass of the solvent in the mixed slurry in step S1 accounts for 50% to 75% by mass. It can be understood that the total mass of the first sodium source, the first iron source, the first carbon source and the antioxidant in the mixed slurry can account for any point value between 25% and 50% by mass. Exemplarily, the total mass of the first sodium source, the first iron source, the first carbon source and the antioxidant in the mixed slurry can account for 25%, 28%, 30%, 33%, 35%, 40%, 45%, 50% and the like; in this way, each raw material can be effectively dispersed in deionized water, and the dispersion effect is relatively good, which is especially beneficial to the uniformity of the dispersion of the first sodium source, the first iron source and the antioxidant, and is beneficial to the reaction of the first sodium source and the first iron source to generate sodium ferric sulfate, which greatly reduces the risk of impurity phase generation, and is beneficial to synergistically improve the sodium storage capacity of the final composite sodium ion positive electrode material; in some preferred embodiments, the total mass of the first sodium source, the first iron source, the first carbon source and the antioxidant accounts for 30% to 40% of the mass of the mixed slurry.
[0080] Specifically, in some exemplary embodiments, dispersing the first sodium source, the first iron source, the first carbon source, and the antioxidant in deionized water to form a mixed slurry includes:
[0081] The first sodium source, the first iron source, the first carbon source and the antioxidant are dispersed in deionized water by sand milling to form a mixed slurry.
[0082] In this step, the dispersion and uniformity of various raw materials in the mixed slurry are increased by sand grinding, especially the dispersion of the first carbon source in the mixed slurry can be improved, so that the mixed slurry is stable and not stratified, which is beneficial to improve the uniformity of the first precursor, improve the transmission effectiveness and efficiency of sodium ions in the first precursor, and help improve the rate performance and conductivity of the final composite sodium ion positive electrode material.
[0083] Among them, the sand milling time is 0.1h~2h; it can be understood that the sand milling time can be any point value between 0.1h~2h; illustratively, the sand milling time can be 0.1h, 0.3h, 0.5h, 0.75h, 1h, 1.25h, 1.5h, 1.75h, 2h, etc.; in this way, the first sodium source, the first iron source, the first carbon source and the antioxidant can be effectively dispersed, the uniformity of the mixed slurry is improved, and then the uniformity inside the carbon-doped sodium ferric sulfate is improved, which is beneficial to improve the sodium storage capacity, conductivity and rate performance of the composite sodium ion positive electrode material.
[0084] Specifically, in step S2, drying the mixed slurry to obtain a first precursor includes:
[0085] Initially drying the mixed slurry to obtain a first initial precursor;
[0086] The first initial precursor is dehydrated to obtain the first precursor; during the dehydration process, the crystal water content in the first initial precursor is reduced.
[0087] Specifically, the initial drying includes at least one of spray drying, vacuum drying, vibration drying and freeze drying to remove most of the water in the mixed slurry, and the first initial precursor obtained is sodium iron sulfate tetrahydrate, with a molecular formula of Na x Fe y (SO4) x / 2+y ·4H2O@C, wherein @C refers to carbon doping, and the carbon material is dispersed between the sodium ferric sulfate tetrahydrate particles, and the ratio of x / y is 1:1 to 1.5:1, that is, in this step, the ratio of x / y in the first initial precursor is consistent with the ratio of x / y of the raw material input in step S1, which is beneficial to maintain the subsequent first precursor and the x / y ratio inside the carbon-doped sodium ferric sulfate particles within a relatively small range, thereby improving the sodium storage capacity of the composite sodium ion positive electrode material; illustratively, the initial drying is spray drying, the inlet air temperature is 170°C to 220°C, and the outlet air temperature is 90°C to 150°C, which can effectively remove most of the water in the mixed slurry.
[0088] Specifically, the first initial precursor can be dehydrated by a rotary kiln, a dryer or other dehydration process equipment to further remove the crystal water in the first initial precursor. The first precursor obtained is Na x Fe y (SO4) x / 2+y@C, wherein @C refers to carbon doping, the carbon material is dispersed between the sodium iron sulfate particles, and the ratio of x / y is 1:1 to 1.5:1, that is, in this step, the ratio of x / y in the first precursor is consistent with the ratio of x / y of the raw material input in step S1, which is beneficial to maintain the x / y ratio inside the carbon-doped sodium iron sulfate particles within a relatively small range, thereby improving the sodium storage capacity of the composite sodium ion positive electrode material.
[0089] Specifically, in some exemplary embodiments, during the dehydration process, the dehydration temperature is 200°C to 300°C, and the dehydration time is 4h to 12h; it can be understood that the dehydration temperature can be any point value between 200°C and 300°C, and the dehydration time can be any point value between 4h and 12h; illustratively, the dehydration temperature can be 200°C, 210°C, 240°C, 250°C, 260°C, 270°C, 295°C, 300°C, etc., and the dehydration time can be 4h, 5h, 6h, 7h, 8h, 9h, 10h, 12h, etc.; in this way, the crystal water in the first initial precursor can be effectively removed to avoid the presence of crystal water causing the weight of the carbon source in the subsequent steps (for example The addition amount of the second carbon source is inaccurate, and the oxidation of ferrous sulfate to generate impurities during the subsequent sintering process is avoided, which is beneficial to improving the capacity of the first precursor, the second precursor, the composite precursor and the finally prepared composite sodium ion positive electrode material. In addition, the dehydration process can introduce micropores inside the carbon-doped sodium ferric sulfate particles, which are conducive to the subsequent infiltration and absorption of the electrolyte, thereby helping to improve the performance of the battery cell with the composite sodium ion positive electrode material; in addition, it can also avoid the phenomenon of iron dissolution caused by the reaction of crystal water with the electrolyte during use, which can greatly improve the safety performance of the composite sodium ion positive electrode material and the sodium ion battery with the composite sodium ion positive electrode material.
[0090] Then, in step S3, the second sodium source and the second iron source are mixed according to an x / y ratio of 1.5:1 to 2:1, that is, the x / y ratio in the mixed dry material formed by the second sodium source, the second iron source and the second carbon source is 1.5:1 to 2:1; it can be understood that the x / y ratio can be any point value in the range of 1.5:1 to 2:1, which is not enumerated here; in this way, the x / y ratio in the second precursor can also reach 1.5:1 to 2:1, and the x / y ratio in the second precursor is relatively large and greater than the x / y ratio in the first precursor, so that in the finally formed composite sodium ion positive electrode material, the outer layer of the carbon-doped sodium iron sulfate particles can have a relatively large x / y ratio, thereby improving the structural stability of the outer layer of the carbon-doped sodium iron sulfate particles and improving the cycle performance of the composite sodium ion positive electrode material.
[0091] Specifically, in some exemplary embodiments, the mass proportion of the second carbon source in the total mass of the second sodium source, the second iron source and the second carbon source is 0.1% to 10%, that is, the mass proportion of the second carbon source in the second precursor is 0.1% to 10%; it can be understood that the mass proportion of the second carbon source in the second precursor can be any point value between 0.1% and 10%, which is not enumerated here; in this way, in conjunction with the dry ball milling process, the transmission path and transmission efficiency of sodium ions in the second precursor can be greatly increased, and the conductivity of the outer layer of the carbon-doped sodium iron sulfate particles and the overall composite sodium ion positive electrode material can be improved.
[0092] Specifically, in step S3, the mixing of the second sodium source, the second iron source and the second carbon source to obtain the second precursor comprises:
[0093] Pre-crushing the second sodium source and the second iron source to obtain a crushed dry material;
[0094] The crushed dry material is mixed with the second carbon source to obtain the second precursor.
[0095] Among them, the pre-crushing includes at least one of planetary ball milling, vibration ball milling, mechanical crushing and air flow crushing, which can effectively crush the second sodium source and the second iron source, reduce the particle size of the second sodium source and the second iron source, and help reduce the particle size of the second precursor, so that the particle size of the second precursor is smaller than that of the first precursor, so that the second precursor can effectively cover the first precursor in the subsequent mixed ball milling process, thereby improving the morphology accuracy and structural stability of the prepared composite sodium ion positive electrode material.
[0096] Specifically, in some exemplary embodiments, in step S4, the median particle size D50 of the first precursor used for mixed ball milling with the second precursor is 20μm~50μm, and the median particle size refers to the diameter of the particles when the cumulative particle size distribution reaches 50%; it can be understood that the median particle size D50 of the first precursor can be any point value between 20μm and 50μm; exemplarily, the median particle size D50 of the first precursor can be 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, etc.
[0097] Specifically, in some exemplary embodiments, the median particle size D50 of the second precursor used for mixed ball milling with the first precursor is 2μm to 5μm; it can be understood that the median particle size D50 of the second precursor can be any point value between 2μm and 5μm; exemplarily, the median particle size D50 of the second precursor can be 2μm, 2.5μm, 2.8μm, 3μm, 3.5μm, 4μm, 5μm, etc.
[0098] In this way, the median particle size of the first precursor is relatively large, while the median particle size of the second precursor is relatively small. The particle size of the first precursor is generally larger than that of the second precursor. During the ball milling process, the second precursor with a smaller particle size can be effectively coated on the first precursor with a relatively larger particle size, forming a composite structure with a smaller internal x / y ratio and a larger outer x / y ratio, that is, a composite precursor with good coating effectiveness and coating stability. In the carbon-coated sodium ferric sulfate particles finally prepared, the conductivity, rate performance, structural stability and cycle performance of the carbon-coated sodium ferric sulfate particles can also be effectively and synergistically improved.
[0099] Specifically, in some exemplary embodiments, D10 of the first precursor is 5 μm to 15 μm, D90 is 70 μm to 90 μm, and D99 is less than or equal to 200 μm, wherein D10 refers to the diameter of the particles when the cumulative particle size distribution reaches 10%, D90 refers to the diameter of the particles when the cumulative particle size distribution reaches 90%, and D99 refers to the diameter of the particles when the cumulative particle size distribution reaches 99%; it can be understood that D10 of the first precursor can be any point value between 5 μm and 15 μm, D90 can be any point value between 70 μm and 90 μm, and D99 can be any point value less than or equal to 200 μm, which are not enumerated here.
[0100] In some other exemplary embodiments, D90 of the second precursor is less than or equal to 10 μm. It is understandable that D90 of the second precursor can be any point value less than or equal to 10 μm, which will not be enumerated here.
[0101] In this way, the particle size of the first precursor is larger than the particle size of the second precursor within a larger proportion range, which enables the second precursor to be stably and effectively coated on the first precursor during the ball milling process, thereby improving the morphology accuracy of the final composite sodium ion positive electrode material, improving the effectiveness and accuracy of the performance improvement of the composite sodium ion positive electrode material, and greatly improving the conductivity, rate performance and cycle performance of the composite sodium ion positive electrode material and the sodium ion battery having the composite sodium ion positive electrode material.
[0102] Specifically, in some exemplary embodiments, in the process of mixing and ball-milling the first precursor and the second precursor to obtain a composite precursor, the mass ratio of the first precursor to the second precursor is 0.5:1 to 5:1; it can be understood that the mass ratio of the first precursor to the second precursor can be any point value in the range of 0.5:1 to 5:1; illustratively, the mass ratio of the first precursor to the second precursor can be 0.5:1, 0.8:1, 1:1, 1.5:1, 2:1, 2.5:1, 3.5:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 21:1, 22:1, 23:1, 24:1, 25:1, 26:1, 27:1, 28:1, 29:1, 30:1, 31:1, 32:1 :1, 4.5:1, 5:1, etc.; in this way, the second precursor can effectively cover the first precursor and form a structurally stable composite precursor, thereby improving the preparation accuracy and efficiency of the subsequent sintering to form the final carbon-doped sodium iron sulfate particles, improving the morphology and structural accuracy of the carbon-doped sodium iron sulfate particles, that is, the composite sodium ion positive electrode material, and greatly improving the overall conductivity, rate performance and cycle performance of the composite sodium ion positive electrode material; in some preferred embodiments, the mass ratio of the first precursor to the second precursor can be 1:1 to 2:1.
[0103] Specifically, step S4 is to dry-mix the first precursor and the second precursor and then ball-mill them, wherein the ball milling may include at least one of planetary ball milling and vibration ball milling, which can effectively improve the mixing uniformity between the first precursor and the second precursor, improve the effectiveness and uniformity of the second precursor coating the first precursor, and is also beneficial to increase the contact area between the first precursor and the second precursor and the contact area between various raw materials, which is beneficial to improve the subsequent sintering preparation of carbon-doped sodium iron sulfate particles. Preparation efficiency and preparation yield; it should be noted that in the process of obtaining the first precursor by drying, part of the ferrous sulfate in the first iron source will precipitate due to dehydration to form a mixed phase, then in step S4, the precipitated part of the ferrous sulfate can be effectively crushed by ball milling, so that the precipitated ferrous sulfate can react with the sodium source in the subsequent sintering process of step S5 to generate sodium iron sulfate, reduce the generation of mixed phases, and further improve the specific capacity and performance of the prepared composite sodium ion positive electrode material.
[0104] Specifically, in some exemplary embodiments, during the ball milling process, the mass ratio of the total mass of the first precursor and the second precursor to the ball milling medium is 10:1 to 50:1, and the ball milling time is 0.1h to 24h; it can be understood that the mass ratio of the total mass of the first precursor and the second precursor to the ball milling medium can be any value between 10:1 and 50:1, and the ball milling time can be any value between 0.1h and 24h; illustratively, the mass ratio of the total mass of the first precursor and the second precursor to the ball milling medium can be 10:1, 20 :1, 30:1, 40:1, 50:1, etc., and the ball milling time can be 0.5h, 1h, 2h, 5h, 8h, 9h, 10h, 15h, etc.; in this way, the first precursor and the second precursor can be effectively dispersed and mixed, and the ferrous sulfate precipitated during the dehydration process can be effectively crushed to increase the contact area between the precipitated ferrous sulfate and sodium sulfate in the subsequent sintering process, promote the precipitated ferrous sulfate to react more with sodium sulfate to generate sodium ferric sulfate, reduce the formation of impurities, and help improve the performance of the composite sodium ion positive electrode material.
[0105] Specifically, in step S5, during the process of sintering and crushing the composite precursor, the sintering temperature is 350°C to 400°C, and the sintering time is 10h to 20h; it can be understood that the sintering temperature can be any point value between 350°C and 400°C, and the sintering time can be any point value between 10h and 20h; illustratively, the sintering temperature can be 350°C, 360°C, 370°C, 375°C, 380°C, 390°C, 400°C, etc., and the sintering time can be 20h. It can be 10h, 11h, 13h, 15h, 16h, 18h, 19h, 20h, etc.; the sintering process produces a pure solid-phase reaction, which can make the iron source and the sodium source in the composite precursor fully react to generate sodium ferric sulfate. The sintering effect is good, which can effectively reduce the generation of impurities, and further improve the specific capacity and rate performance of the composite sodium ion positive electrode material. In addition, crushing after sintering can also improve the convenience of using the composite sodium ion positive electrode material in sodium ion batteries.
[0106] On the other hand, the present application also provides a sodium ion battery, comprising the composite sodium ion positive electrode material as described above, or comprising a composite sodium ion positive electrode material prepared by the preparation method of the composite sodium ion positive electrode material as described above.
[0107] In some exemplary embodiments, the composite sodium ion positive electrode material is present in the positive electrode sheet of the sodium ion battery; in other exemplary embodiments, the composite sodium ion positive electrode material can be present in the solid electrolyte membrane of the sodium ion battery; in other exemplary embodiments, both the positive electrode sheet and the solid electrolyte membrane of the sodium ion battery can include the composite sodium ion positive electrode material to further improve the performance of the sodium ion battery, meet the performance requirements of different sodium ion batteries, and have a wide range of applications.
[0108] The following describes the embodiments of the present application in combination with the above technical solutions.
[0109] Example 1
[0110] The composite sodium ion positive electrode material of this embodiment is prepared by the following steps:
[0111] 1. Disperse sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes (CNTs) and ascorbic acid in deionized water, stir for 15 minutes to form a mixed slurry, and sand grind the mixed slurry for 1 hour to fully disperse the CNTs to form a stable non-stratified mixed slurry; wherein the Na / Fe molar ratio of sodium sulfate and ferrous sulfate heptahydrate is 1.2:1, the mass of each of the carbon nanotubes and ascorbic acid is 1% of the total mass of sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes and ascorbic acid, and the total mass of sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes and ascorbic acid accounts for 35% of the total mass of the mixed slurry;
[0112] 2. The mixed slurry is spray dried with an inlet air temperature of 200°C and an outlet air temperature of 100°C to obtain a first initial precursor; the first initial precursor is a gray-black powder; the molecular formula of the first initial precursor is Na x Fe y (SO4) x / 2+y 4H2O@C, where the ratio of x / y is 1.2:1;
[0113] 3. Mixing sodium sulfate, anhydrous ferrous sulfate and CNT to obtain a second precursor; wherein the molar ratio of Na / Fe of sodium sulfate and anhydrous ferrous sulfate is 1.8:1, the mass of CNT is 2% of the total mass of sodium sulfate, anhydrous ferrous sulfate and CNT, and the ratio of x / y in the second precursor is 1.8:1;
[0114] 4. Add the first initial precursor and the second precursor to a ball mill and mill for 2 hours to obtain a composite precursor; wherein the mass ratio of the first precursor to the second precursor is calculated based on the water content of the first initial precursor with the x / y ratio of the final composite sodium ion positive electrode material being 1.5:1 as the target;
[0115] 5. Sinter and crush the composite precursor at a sintering temperature of 350°C for 10 hours to obtain a composite sodium ion positive electrode material; the molecular formula of the composite sodium ion positive electrode material is Na x Fe y (SO4) x / 2+y @C, where the ratio of x / y is 1.5:1.
[0116] Example 2
[0117] The composite sodium ion positive electrode material of this embodiment is prepared by the following steps:
[0118] 1. Disperse sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes (CNTs) and ascorbic acid in deionized water, stir for 15 minutes to form a mixed slurry, and sand grind the mixed slurry for 1 hour to fully disperse the CNTs to form a stable non-stratified mixed slurry; wherein the Na / Fe molar ratio of sodium sulfate and ferrous sulfate heptahydrate is 1.2:1, the mass of each of the carbon nanotubes and ascorbic acid is 1% of the total mass of sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes and ascorbic acid, and the total mass of sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes and ascorbic acid accounts for 35% of the total mass of the mixed slurry;
[0119] 2. The mixed slurry is spray-dried at an air inlet temperature of 200° C. and an air outlet temperature of 100° C. to obtain a first initial precursor; the first initial precursor is a gray-black powder;
[0120] 3. Dehydrate the first initial precursor by a rotary kiln at a dehydration temperature of 300°C for 6 hours to obtain a first precursor; the molecular formula of the first precursor is Na x Fe y (SO4) x / 2+y @C, where the ratio of x / y is 1.2:1;
[0121] 4. Mixing sodium sulfate, anhydrous ferrous sulfate and CNT to obtain a second precursor; wherein the molar ratio of Na / Fe of sodium sulfate and anhydrous ferrous sulfate is 1.8:1, the mass of CNT is 2% of the total mass of sodium sulfate, anhydrous ferrous sulfate and CNT, and the ratio of x / y in the second precursor is 1.8:1;
[0122] 5. Add the first precursor and the second precursor into a ball mill and mill for 2 hours to obtain a composite precursor; wherein the mass ratio of the first precursor to the second precursor is 1:1;
[0123] 6. Sinter and crush the composite precursor at a sintering temperature of 350°C for 10 hours to obtain a composite sodium ion positive electrode material; the molecular formula of the composite sodium ion positive electrode material is Na x Fe y(SO4) x / 2+y @C, where the ratio of x / y is 1.5:1.
[0124] Example 3
[0125] The composite sodium ion positive electrode material of this embodiment is prepared by the following steps:
[0126] 1. Disperse sodium sulfate, ferrous sulfate heptahydrate, graphene and ascorbic acid in deionized water, stir for 10 minutes to form a mixed slurry, and sand grind the mixed slurry for 0.5 hours to fully disperse the graphene to form a stable non-stratified mixed slurry; wherein the molar ratio of Na / Fe of sodium sulfate and ferrous sulfate heptahydrate is 1.0:1, the mass of each of carbon nanotubes and ascorbic acid is 1% of the total mass of sodium sulfate, ferrous sulfate heptahydrate, graphene and ascorbic acid, and the total mass of sodium sulfate, ferrous sulfate heptahydrate, graphene and ascorbic acid accounts for 35% of the total mass of the mixed slurry;
[0127] 2. The mixed slurry is spray-dried at an air inlet temperature of 190° C. and an air outlet temperature of 100° C. to obtain a first initial precursor; the first initial precursor is a gray-black powder;
[0128] 3. Dehydrate the first initial precursor by a rotary kiln at a dehydration temperature of 300°C for 6 hours to obtain a first precursor; the molecular formula of the first precursor is Na x Fe y (SO4) x / 2+y @C, where the ratio of x / y is 1:1;
[0129] 4. Mix sodium sulfate, ferrous sulfate monohydrate and CNT to obtain a second precursor; wherein the molar ratio of Na / Fe of sodium sulfate and ferrous sulfate monohydrate is 1.6:1, the mass of CNT is 2% of the total mass of sodium sulfate, ferrous sulfate monohydrate and CNT, and the ratio of x / y in the second precursor is 1.6:1;
[0130] 5. Add the first precursor and the second precursor into a ball mill and mill for 2 hours to obtain a composite precursor; wherein the mass ratio of the first precursor to the second precursor is 1:1;
[0131] 6. Sinter and crush the composite precursor at a sintering temperature of 350°C for 10 hours to obtain a composite sodium ion positive electrode material; the molecular formula of the composite sodium ion positive electrode material is Na x Fe y (SO4) x / 2+y @C, where the ratio of x / y is 1.3:1.
[0132] Example 4
[0133] The composite sodium ion positive electrode material of this embodiment is prepared by the following steps:
[0134] 1. Disperse sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes (CNTs) and ascorbic acid in deionized water, stir for 10 minutes to form a mixed slurry, and sand grind the mixed slurry for 0.5 hours to fully disperse the CNTs to form a stable non-stratified mixed slurry; wherein the Na / Fe molar ratio of sodium sulfate and ferrous sulfate heptahydrate is 1.3:1, the mass of each of the carbon nanotubes and ascorbic acid is 1% of the total mass of sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes and ascorbic acid, and the total mass of sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes and ascorbic acid accounts for 35% of the total mass of the mixed slurry;
[0135] 2. The mixed slurry is spray-dried at an air inlet temperature of 190° C. and an air outlet temperature of 100° C. to obtain a first initial precursor; the first initial precursor is a gray-black powder;
[0136] 3. Dehydrate the first initial precursor by a rotary kiln at a dehydration temperature of 300°C for 6 hours to obtain a first precursor; the molecular formula of the first precursor is Na x Fe y (SO4) x / 2+y @C, where the ratio of x / y is 1.3:1;
[0137] 4. Mixing sodium sulfate, ferrous sulfate heptahydrate and CNT to obtain a second precursor; wherein the molar ratio of Na / Fe of sodium sulfate and ferrous sulfate heptahydrate is 1.9:1, the mass of CNT is 2% of the total mass of sodium sulfate, ferrous sulfate heptahydrate and CNT, and the ratio of x / y in the second precursor is 1.9:1;
[0138] 5. Add the first precursor and the second precursor into a ball mill and mill for 2 hours to obtain a composite precursor; wherein the mass ratio of the first precursor to the second precursor is 2:1;
[0139] 6. Sinter and crush the composite precursor at a sintering temperature of 350°C for 10 hours to obtain a composite sodium ion positive electrode material; the molecular formula of the composite sodium ion positive electrode material is Na x Fe y (SO4) x / 2+y @C, where the ratio of x / y is 1.5:1.
[0140] Example 5
[0141] The difference between this embodiment and embodiment 1 is that in the prepared first initial precursor, the ratio of x / y is 1.1:1; the rest is the same as embodiment 1.
[0142] Example 6
[0143] The difference between this embodiment and embodiment 1 is that in the prepared second precursor, the ratio of x / y is 2.0:1; the rest is the same as embodiment 1.
[0144] Example 7
[0145] The difference between this embodiment and embodiment 1 is that, during the process of adding the first initial precursor and the second precursor into the ball mill for ball milling, the ball milling time is 0.5 h; the rest is the same as embodiment 1.
[0146] Example 8
[0147] The difference between this embodiment and Embodiment 1 is that, in the process of adding the first initial precursor and the second precursor into the ball mill for ball milling, the mass ratio of the first precursor to the second precursor is calculated based on the water content of the first initial precursor with the x / y ratio of the final composite sodium ion positive electrode material being 1.35:1 as the target; the rest is the same as Embodiment 1.
[0148] Comparative Example 1
[0149] The difference between this comparative example and Example 2 is that the mass ratio of the first precursor to the second precursor is 10:1, and the ratio of x / y in the final composite sodium ion positive electrode material is 1.25:1; the rest is the same as Example 1.
[0150] Comparative Example 2
[0151] The difference between this comparative example and Example 2 is that the mass ratio of the first precursor to the second precursor is 0.5:1, and the ratio of x / y in the final composite sodium ion positive electrode material is 1.6:1; the rest is the same as Example 1.
[0152] Comparative Example 3
[0153] This comparative example adopts a wet method for preparation, without dehydration or coating of the second precursor, and the specific preparation steps are as follows:
[0154] 1. Disperse sodium sulfate, ferrous sulfate heptahydrate, carbon nanotubes (CNTs) and ascorbic acid in deionized water, stir for 15 minutes to form a mixed slurry, and sand grind the mixed slurry for 2 hours to fully disperse the CNTs to form a stable non-stratified mixed slurry; wherein the Na / Fe molar ratio of sodium sulfate and ferrous sulfate heptahydrate is 1.7:1, the mass of the carbon nanotubes is 3% of the total mass of the sodium sulfate, ferrous sulfate heptahydrate, the carbon nanotubes and the ascorbic acid, and the mass of the ascorbic acid is 1% of the total mass of the sodium sulfate, ferrous sulfate heptahydrate, the carbon nanotubes and the ascorbic acid;
[0155] 2. The mixed slurry is spray-dried at an air inlet temperature of 200° C. and an air outlet temperature of 100° C. to obtain a first initial precursor; the first initial precursor is a gray-black powder;
[0156] 3. Sinter and crush the first initial precursor at a sintering temperature of 350° C. for 10 h to obtain a sodium ion positive electrode material; the molecular formula of the sodium ion positive electrode material is Na x Fe y (SO4) x / 2+y @C, where the ratio of x / y is 1.7:1.
[0157] Taking Example 2 and Example 3 as examples, the composite sodium ion positive electrode material is scanned at cross-section points to determine the sodium content (i.e., the molar percentage of the sodium element) and the iron content (i.e., the molar percentage of the iron element) at each sampling point, such as Figure 1 and Figure 2 As shown, the distance between the sampling points A / D and the outer surface of the carbon-doped sodium ferric sulfate particles is no more than 15% of the overall diameter of the particles, and the distance between the sampling points B / C and the center point of the carbon-doped sodium ferric sulfate particles is no more than 15% of the overall diameter of the particles.
[0158] Depend on Figure 1 and Figure 2 It can be seen that in the composite sodium ion positive electrode material prepared in the embodiment of the present application, the particle structure has two obvious forms. Inside the carbon-doped sodium ferric sulfate particles, especially in the center, the dark gray particle area is carbon nanotubes. Since the dispersion effect of sand milling on carbon nanotubes is limited, most of the carbon nanotubes still exist in the form of agglomerates, and there are micropores inside the carbon-doped sodium ferric sulfate particles. The micropores are formed by dehydration, which is conducive to the subsequent infiltration and absorption of the electrolyte, and is beneficial to improving the first-cycle discharge capacity and other performance of the battery cell; and in the outer layer of the carbon-doped sodium ferric sulfate particles, the connection between the particles is relatively tight, and no obvious CNT agglomeration morphology is seen, indicating that dry ball milling has a good effect on the crushing, dispersion and coating of various materials.
[0159] Table 1 Element scanning results of the composite sodium ion positive electrode material in Example 2
[0160]
[0161] Table 2 Element scanning results of the composite sodium ion positive electrode material in Example 3
[0162]
[0163] Further, the element scanning results of the four points A / B / C / D in Example 2 are shown in Table 1, and the element scanning results of the four points A / B / C / D in Example 3 are shown in Table 2. Then, combining the element scanning results in Table 1 and Table 2, and Figure 3 The XRD curve diagram verifies that the element distribution in the carbon-doped sodium iron sulfate particles is basically consistent with the expected element distribution, that is, the Na / Fe molar ratio in the center of the composite sodium ion positive electrode material is relatively low to provide higher capacity, while the Na / Fe molar ratio in the outer layer of the composite sodium ion positive electrode material is relatively high, which provides better cycle stability for the composite sodium ion positive electrode material as a whole.
[0164] Table 3 Electrical performance test results of the composite sodium ion positive electrode materials of the embodiment and the sodium ion positive electrode materials of the comparative example
[0165]
[0166] according to Figure 4 As shown, the composite sodium ion positive electrode material prepared in Example 2 has good charge and discharge performance; further, Table 3 is the electrical performance test results obtained by conducting electrical performance tests on the materials in the above embodiments and comparative examples, among which the first-cycle discharge capacity and 2C cycle 200-cycle capacity retention rate of the composite sodium ion positive electrode materials in Examples 1-8 are both high; while in the comparative examples, excessive addition of the first precursor in comparative example 1 results in decreased structural stability and a relatively low capacity retention rate of only 90.2%; too little addition of the first precursor in comparative example 2 and relatively more addition of the second precursor result in a decrease in the first-cycle discharge capacity. It can be seen that the mass ratio of the first precursor to the second precursor is within the range of 0.5:1 to 5:1 provided in the present application, in order to take into account a good first-cycle discharge capacity. Capacity and capacity retention rate; Comparative Example 3 is a wet process as a whole, which cannot meet the structural stability requirements, resulting in a decrease in capacity retention rate, and also has a certain adverse effect on the first-cycle discharge capacity; It can be seen that only the composite sodium ion positive electrode material of the embodiment of the present application can take into account the synergistic improvement of the first-cycle discharge capacity and capacity retention rate. While the first-cycle discharge capacity is higher than 93%, the capacity retention rate of 2C cycle 200 cycles can also reach more than 96%; especially in Examples 2-4, after dehydration of the first initial precursor, the introduction of impurities caused by the presence of crystallization water is avoided, and micropores can be introduced into the structure, which is beneficial to the entry and absorption of subsequent electrolytes. While the first-cycle discharge capacity is greater than 98%, the capacity retention rate of 2C cycle 200 cycles can also reach more than 98%.
[0167] It should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0168] What is described above are only some embodiments of the present application and are not intended to limit the present application. Those skilled in the art should understand that the present application may undergo various changes and improvements, and any modifications, equivalent substitutions and improvements made in accordance with the present application shall fall within the scope of protection required by the present application.
Claims
1. A composite sodium ion positive electrode material, It is characterized in that The invention comprises carbon-doped sodium iron sulfate particles, wherein the molecular formula of the sodium iron sulfate particles is Na x Fe y (SO4) x / 2+y , the x / y ratio inside the carbon-doped sodium iron sulfate particle is smaller than the x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particle; The ratio of x / y in the carbon-doped sodium iron sulfate particles is 1.2:1 to 1.8:1; The x / y ratio inside the carbon-doped sodium iron sulfate particles is 1:1 to 1.5:1; The x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particles is 1.5:1 to 2.0:
1.
2. The composite sodium ion positive electrode material according to claim 1, It is characterized in that The ratio of x / y gradually increases from the inside to the outer layer of the carbon-doped sodium iron sulfate particles.
3. The composite sodium ion positive electrode material according to claim 2, It is characterized in that In the direction from the inside to the outside of the carbon-doped sodium iron sulfate particles, the increasing gradient of the x / y ratio is less than or equal to the target increasing gradient, and the target increasing gradient is 0.10 / 10% to 0.18 / 10% of the particle diameter.
4. The composite sodium ion positive electrode material according to any one of claims 1 to 3, It is characterized in that The carbon material in the carbon-doped sodium iron sulfate particles satisfies at least one of the following characteristics: The carbon material includes at least one of graphite, graphene, carbon black, single-walled carbon nanotubes and multi-walled carbon nanotubes; The mass proportion of the carbon material in the carbon-doped sodium iron sulfate particles is 0.1% to 10%; The carbon material accounts for 0.1% to 10% by mass of the outer layer of the carbon-doped sodium iron sulfate particles.
5. The composite sodium ion positive electrode material according to any one of claims 1 to 3, It is characterized in that The composite sodium ion positive electrode material forms carbon-doped sodium iron sulfate particles through a sodium source, an iron source and a carbon source, wherein the sodium source includes a first sodium source and a second sodium source, the iron source includes a first iron source and a second iron source, and the sodium source and the iron source are used to react to generate sodium iron sulfate; the carbon source includes a first carbon source and a second carbon source, and the carbon source is used to form the carbon material in the composite sodium ion positive electrode material; The composite sodium ion positive electrode material includes a composite inner layer and a composite outer layer, wherein the composite outer layer is coated on the composite inner layer; the composite inner layer is prepared by wet method using a first sodium source, a first iron source and a first carbon source, and the composite outer layer is prepared by dry method using a second sodium source, a second iron source and a second carbon source.
6. A method for preparing a composite sodium ion positive electrode material, It is characterized in that Carbon-doped sodium iron sulfate particles are formed by a sodium source, an iron source and a carbon source; the molecular formula of the sodium iron sulfate particles is Na x Fe y (SO4) x / 2+y , the x / y ratio inside the carbon-doped sodium iron sulfate particle is smaller than the x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particle; The ratio of x / y in the carbon-doped sodium iron sulfate particles is 1.2:1 to 1.8:1; The x / y ratio inside the carbon-doped sodium iron sulfate particles is 1:1 to 1.5:1; The x / y ratio of the outer layer of the carbon-doped sodium iron sulfate particles is 1.5:1 to 2.0:
1.
7. The method for preparing the composite sodium ion positive electrode material according to claim 6, It is characterized in that The method comprises: Dispersing a first sodium source, a first iron source, a first carbon source, and an antioxidant in deionized water to form a mixed slurry; Drying the mixed slurry to obtain a first precursor; Mixing a second sodium source, a second iron source and a second carbon source to obtain a second precursor; the ratio of x / y in the first precursor is less than the ratio of x / y in the second precursor; The first precursor and the second precursor are mixed and ball-milled to obtain a composite precursor; the particle size of the first precursor is larger than the particle size of the second precursor, and during the mixing and ball-milling process, the second precursor covers the first precursor; The composite precursor is sintered and crushed to obtain the composite sodium ion positive electrode material.
8. The method for preparing the composite sodium ion positive electrode material according to claim 7, It is characterized in that The step of drying the mixed slurry to obtain a first precursor comprises: Initially drying the mixed slurry to obtain a first initial precursor; The first initial precursor is dehydrated to obtain the first precursor; during the dehydration process, the crystal water content in the first initial precursor is reduced.
9. The method for preparing the composite sodium ion positive electrode material according to claim 8, It is characterized in that The first initial precursor is Na x Fe y (SO4) x / 2+y ·4H 2 O@C, where the ratio of x / y is 1:1 to 1.5:1; The initial drying includes at least one of spray drying, vacuum drying, vibration drying and freeze drying.
10. The method for preparing the composite sodium ion positive electrode material according to claim 8, It is characterized in that The first precursor is Na x Fe y (SO4) x / 2+y , wherein the ratio of x / y is 1:1 to 1.5:1; during the dehydration process, the dehydration temperature is 200° C. to 300° C., and the dehydration time is 4 h to 12 h.
11. A method for preparing a composite sodium ion positive electrode material according to any one of claims 7 to 10, It is characterized in that The step of mixing the second sodium source, the second iron source and the second carbon source to obtain the second precursor comprises: Pre-crushing the second sodium source and the second iron source to obtain a crushed dry material; The crushed dry material is mixed with the second carbon source to obtain the second precursor.
12. A method for preparing a composite sodium ion positive electrode material according to any one of claims 7 to 10, It is characterized in that In the process of mixing and ball-milling the first precursor and the second precursor to obtain a composite precursor, the method satisfies at least one of the following characteristics: The mass ratio of the first precursor to the second precursor is 0.5:1 to 5:1; The median particle size of the first precursor is 20 μm to 50 μm; the median particle size of the second precursor is 2 μm to 5 μm.
13. A method for preparing a composite sodium ion positive electrode material according to any one of claims 7 to 10, It is characterized in that The antioxidant meets at least one of the following characteristics: The antioxidant comprises at least one of ascorbic acid, oxalic acid and citric acid; The weight proportion of the antioxidant in the total weight of the first sodium source, the first iron source, the first carbon source and the antioxidant is 0.1% to 2%.
14. A method for preparing a composite sodium ion positive electrode material according to any one of claims 7 to 10, It is characterized in that In the process of sintering and crushing the composite precursor, the sintering temperature is 350° C. to 400° C., and the sintering time is 10 h to 20 h.
15. A sodium ion battery, It is characterized in that The invention comprises the composite sodium ion positive electrode material as described in any one of claims 1 to 5, or comprises the composite sodium ion positive electrode material prepared by the preparation method of the composite sodium ion positive electrode material as described in any one of claims 6 to 14.