Super hydrophobic particles, internal and external super hydrophobic grouting material and preparation method thereof

By preparing superhydrophobic particles and internal and external superhydrophobic grouting materials, the problem of easy aging of traditional coatings was solved by utilizing large quantities of silicon-aluminum waste, which improved the durability and resource utilization efficiency of concrete structures and achieved green treatment of waste.

CN118479788BActive Publication Date: 2024-11-05QINGDAO UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410445240.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-11-05
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

Traditional superhydrophobic coatings are prone to aging, have limited reliability and durability, and fail to effectively utilize large quantities of silica-alumina waste, leading to decreased durability of concrete structures and environmental pollution.

Method used

Superhydrophobic particles are prepared using bulk silicon-aluminum waste. Through the combination of alkaline catalyst, hydrogen-containing silicone oil, fluorosilane and silica sol, a micron-sized waxy papillary structure is formed to prepare an internally and externally superhydrophobic grouting material, achieving superhydrophobicity and impermeability.

Benefits of technology

It improves the service life of concrete structures, realizes the resource utilization of silicon-aluminum waste, and has excellent properties such as waterproofing, dustproofing, and wear resistance, meeting the requirements of green chemistry and sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118479788B_ABST
    Figure CN118479788B_ABST
Patent Text Reader

Abstract

The present invention provides a kind of super-hydrophobic particles, internal and external super-hydrophobic grouting materials and preparation method thereof, relate to the field of concrete repair technology, by weight ratio, the raw material of the super-hydrophobic particles includes bulk silicon-aluminum waste 70-73%, alkali catalyst 4-7%, hydrogen-containing silicone oil 9-12%, fluorosilane 1-3%, silica sol 5-8% and water 7-10%, the bulk silicon-aluminum waste includes slag, slag, red mud, phosphorus slag, waste concrete, one or more of silica ash and fly ash; the raw material of the internal and external super-hydrophobic grouting materials includes mortar and the super-hydrophobic particles. The super-hydrophobic particles prepared by the present invention have excellent comprehensive properties such as waterproof, dustproof, wear-resistant, and the internal and external super-hydrophobic grouting materials prepared by the super-hydrophobic particles have the characteristics of waterproof, anti-fog, anti-snow, anti-pollution, anti-freeze-thaw, anti-corrosion, and can solve the problem of easy cracking and silicon-aluminum waste pollution environment during the service of concrete structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete repair, and specifically relates to super-hydrophobic particles, internal and external super-hydrophobic grouting materials and preparation methods thereof. Background Art

[0002] As an important material in the construction field, concrete is a typical hydrophilic porous material. The gel pores in cement stone, the microcracks in the concrete matrix, and the connected pores in the interface transition zone can all serve as transmission channels for harmful media. Chloride, sulfate and other harmful substances use water as a carrier and penetrate into the concrete matrix through these transmission channels. Under the coupling of multiple factors such as load, freeze-thaw, and ion exchange, they accelerate the rust expansion of steel bars and the cracking of concrete, resulting in a significant decrease in the durability and reliability of the structure. It can be seen that the key to improving the durability of concrete is to improve the ability of concrete to resist water intrusion.

[0003] Superhydrophobicity generally refers to a phenomenon in which the static contact angle of a solid surface to water is greater than 150°. The superhydrophobic surface depends on the combination of low surface energy materials and rough surface structure.

[0004] Super-hydrophobic surface protection technology is an important measure that can effectively slow down the environmental erosion of concrete, thereby improving the durability and service life of concrete structures. Traditional super-hydrophobic coatings generally form a dense protective layer on the surface of the substrate to delay the erosion of harmful media. This method relies on the film-forming property of the coating itself. Its disadvantages are: on the one hand, the protective layer is airtight and easy to age, resulting in bulging, shedding, damage and cracking of the protective layer. Once a gap appears in the protective layer, water and moisture will quickly penetrate and cause failure; on the other hand, traditional protective coatings will seriously affect the appearance of the building after aging and yellowing. Therefore, the reliability and durability of traditional super-hydrophobic surface protection are very limited.

[0005] Promoting the comprehensive utilization of solid waste is of great significance to improving resource utilization efficiency, improving environmental quality, promoting social and economic development, and achieving comprehensive green transformation. The green and efficient comprehensive utilization of solid waste is an effective way to build ecological civilization in my country under the new situation, and it is also a key research direction in fields such as materials science.

[0006] Bulk silicon-aluminum waste usually has a porous morphology and a high specific surface area, which gives them a larger surface area for chemical reactions to occur. The hydrophobic particles prepared from bulk silicon-aluminum waste often contain certain chemical components, such as iron oxide, aluminum oxide, etc. These components have high chemical reactivity and can react with other substances to promote changes in physical and chemical properties. The morphology and structural characteristics of hydrophobic particles give them advantages in physical and mechanical properties. For example, they can provide better filling effects and enhance the material's compressive and shear resistance.

[0007] In order to reduce production costs and make full use of large amounts of silicon-aluminum waste is a technical problem that needs to be solved urgently in my country.

[0008] Therefore, it is necessary to provide an improved technical solution to address the above-mentioned deficiencies in the prior art. Summary of the invention

[0009] The purpose of the present invention is to provide a super-hydrophobic particle, an internal and external super-hydrophobic grouting material and a preparation method thereof, and to prepare a super-hydrophobic grouting material using bulk silicon-aluminum waste, which has excellent water repellency, impermeability and freeze-thaw resistance, and effectively improves the service life of concrete structures. At the same time, the resource utilization of silicon-aluminum solid waste is realized to solve the problem of easy cracking of concrete structures during service and environmental pollution caused by silicon-aluminum waste.

[0010] In order to achieve the above object, the present invention provides the following technical solutions:

[0011] The invention discloses a super hydrophobic particle. The raw materials thereof include 70-73% of bulk silicon-aluminum waste, 4-7% of alkali catalyst, 9-12% of hydrogenated silicone oil, 1-3% of fluorosilane, 5-8% of silica sol and 7-10% of water by weight ratio.

[0012] Preferably, the bulk silicoaluminous waste includes one or more of steel slag, ore slag, red mud, phosphorus slag, waste concrete, silica ash and fly ash.

[0013] Preferably, the alkaline catalyst includes one or more of sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, calcium hydroxide and barium hydroxide.

[0014] Preferably, the structural formula of the hydrogen-containing silicone oil is as shown in the following formula (I):

[0015]

[0016] In the formula, a, b, c, and n are all positive integers, wherein a is between 1 and 20, b is between 1 and 20, c is between 1 and 10, and n is between 2 and 1000.

[0017] Preferably, the preparation method of the hydrogen-containing silicone oil is as follows:

[0018] Amol trifluoroisopropyldichlorosilane, bmol polydimethylsiloxane, cmol hexafluoropropylene are used as raw materials, n-heptane is used as solvent, Karstedt catalyst is added, reacted at 80-100° C. for 6-8 hours, and the hydrogen-containing silicone oil is obtained after removing the light components;

[0019] Preferably, a=2, b=2, c=1.

[0020] Preferably, the fluorosilane includes triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane and / or 1H,1H,2H,2H-perfluorooctyltrichlorosilane.

[0021] Preferably, the silica sol includes one or more of acidic silica sol, alkaline silica sol and neutral silica sol.

[0022] The present invention also provides an internal and external super-hydrophobic grouting material, the raw materials of which include mortar and super-hydrophobic particles. By weight, the raw materials of the mortar include 18-35% of cement, 54-70% of sand and 6.3-14% of water. The super-hydrophobic particles are selected from any of the above-mentioned super-hydrophobic particles, and the mass ratio of the mortar to the super-hydrophobic particles is 100:(10-50).

[0023] The present invention also provides a method for preparing an internal and external super-hydrophobic grouting material, comprising the following steps:

[0024] S1, according to the ratio, weigh a large amount of silicon aluminum waste and alkaline catalyst into a container, stir and mix evenly, then add water, and stir at room temperature for 5-7h; according to the ratio, add hydrogen silicone oil, silica sol and fluorosilane, mix, stir for 1-2h, then settle for 24h, extract the bottom sediment, grind and sieve after drying to obtain super hydrophobic particles;

[0025] S2. Weigh sand and cement according to the proportion and stir at room temperature for at least 2 minutes, then add water according to the proportion and continue stirring at room temperature for at least 2 minutes, finally add super-hydrophobic particles according to the proportion and continue stirring for at least 3 minutes to obtain internal and external super-hydrophobic grouting material.

[0026] Preferably, in step S1, the stirring rate is 200-500 rpm.

[0027] Beneficial effects:

[0028] (1) The present invention utilizes a large amount of silicon-aluminum waste to prepare super-hydrophobic particles, wherein the silicon-aluminum waste is used as the main raw material, accounting for more than 70% of the raw materials, turning waste into treasure, saving natural resources, and having good economic benefits and long-term social benefits. The prepared super-hydrophobic particles have excellent comprehensive properties such as waterproof, dustproof, and wear-resistant, and the process of preparing the super-hydrophobic particles has little pollution, and the by-products are only H2 and H2O, which meets the purpose of green chemistry and carbon neutrality. Not only is the utilization rate high, but the preparation process does not require high-temperature calcination, and has outstanding characteristics such as energy saving and consumption reduction, and the application prospect is very broad;

[0029] (2) The alkaline catalyst in the super-hydrophobic particles is not only a reaction catalyst and stabilizer for fluorosilane, hydrogen-containing silicone oil and silica sol, but also an etchant for bulk silicon-aluminum waste, which can stimulate the complexation between fluorosilane, hydrogen-containing silicone oil and silica sol and bulk silicon-aluminum waste, so that fluorosilane, hydrogen-containing silicone oil and silica sol are fixed on the surface of bulk silicon-aluminum waste in a chemically bonded manner;

[0030] (3) The present invention proposes an internal and external super-hydrophobic grouting material and a preparation method thereof, which uses bulk silicon-aluminum waste as the main raw material. The scheme is mature and the process is simple. It has the characteristics of being waterproof, anti-fog, anti-snow, anti-pollution, anti-freeze and thaw, and anti-corrosion. It can effectively improve the durability of existing concrete structures and is in line with the country's long-term sustainable development strategy. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:

[0032] Figure 1 A schematic diagram of the microstructure of the internal and external super-hydrophobic grouting material after curing provided by an embodiment of the present invention;

[0033] Figure 2 A water absorption trend diagram of the internal and external super-hydrophobic grouting material provided in Example 1 of the present invention;

[0034] Figure 3 This is a contact angle test image of the internal and external super-hydrophobic grouting material provided in Example 1 of the present invention;

[0035] Figure 4 The freeze-thaw cycle test results of the internal and external super-hydrophobic grouting material provided in Example 1 of the present invention;

[0036] Figure 5 This is a SEM image of the super-hydrophobic particles provided in Example 1 of the present invention;

[0037] Figure 6 This is the infrared spectrum analysis result of the super-hydrophobic particles provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0039] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0040] The present invention aims at the problems of easy aging, limited reliability and durability of traditional super-hydrophobic coatings, and provides a super-hydrophobic particle. The raw materials thereof include, by weight, 70-73% (e.g., 70.1%, 70.5%, 71.0%, 71.5%, 72.0%, 72.5%, 72.9%) of bulk silicon-aluminum waste, 4-7% (e.g., 4.1%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 6.9%) of alkaline catalyst, 9-12% (e.g., 9. 1%, 9.5%, 10.0%, 10.5%, 11.0%, 11.5%, 11.9%), fluorosilane 1-3% (e.g. 1.1%, 1.5%, 1.9%, 2.0%, 2.1%, 2.5%, 2.9%), silica sol 5-8% (e.g. 5.1%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 7.9%) and water 7-10% (e.g. 7.1%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 9.9%).

[0041] In a preferred embodiment of the present invention, the bulk siliceous and aluminous waste includes one or more of steel slag, ore slag, red mud, phosphorus slag, waste concrete, silica ash and fly ash.

[0042] In a preferred embodiment of the present invention, the alkali metal hydroxide includes one or more of sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, calcium hydroxide and barium hydroxide.

[0043] In a preferred embodiment of the present invention, the structural formula of the hydrogen-containing silicone oil is shown in the following formula (I):

[0044]

[0045] In the formula, a, b, c, and n are all positive integers, wherein a is between 1 and 20, b is between 1 and 20, c is between 1 and 10, and n is between 2 and 1000.

[0046] In a preferred embodiment of the present invention, the preparation method of hydrogen-containing silicone oil is as follows:

[0047] A mol trifluoroisopropyldichlorosilane, b mol polydimethylsiloxane, cmol hexafluoropropylene are used as raw materials, n-heptane is used as solvent, Karstedt catalyst is added, and the mixture is reacted at 80-100° C. for 6-8 hours. After removing the light components by distillation or the like, hydrogen-containing silicone oil is obtained, as shown in the following formula (II):

[0048]

[0049] The above method can be used to prepare colorless, transparent, tasteless and odorless hydrogenated silicone oil, which can be changed from water to maltose, with a viscosity of 10 to 100 mm 2 / s, can be made into different viscosities according to the requirements of use, has good heat resistance and low temperature resistance, small surface tension, good hydrophobicity, electrical insulation, solubility, lubricity, oxidation resistance stability and physiological inertness.

[0050] In a preferred embodiment of the present invention, a=2, b=2, c=1.

[0051] In a preferred embodiment of the present invention, the fluorosilane includes triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane and / or 1H,1H,2H,2H-perfluorooctyltrichlorosilane. These two fluorosilane films have high stability. On the one hand, the strong CF bonds and covalent bonds between the hydroxysilane groups and the surface can prevent oxidation at ambient temperature, so that the fluorosilane film will not begin to decompose until it is above 230°C; on the other hand, the proportion of superhydrophobic surface in contact with water droplets is about a few percent, thereby reducing the possibility of hydrolysis and desorption.

[0052] In a preferred embodiment of the present invention, the silica sol includes one or more of acidic silica sol, alkaline silica sol and neutral silica sol.

[0053] The super-hydrophobic particles provided by the present invention are based on the "lotus effect" of micron-scale waxy papilla structure and low surface energy characteristics, so that they show excellent durability in wettability tests, waterproof performance and freeze-thaw test experiments. The internal and external super-hydrophobic grouting material prepared using the super-hydrophobic particles can provide three-dimensional super-hydrophobicity, so that it has excellent wear resistance, and the mortar has good air permeability, which can eliminate the problem of poor air permeability of film-forming super-hydrophobic coatings, and has better durability than surface super-hydrophobic modification.

[0054] The alkaline catalyst provides a highly alkaline environment in water, promotes the hydrolysis of fluorosilane, hydrogenated silicone oil and silica sol, produces active hydroxyl groups that can chemically bond with inorganic interfaces, and improves the bonding activity of low surface energy molecules with bulk silicon-aluminum waste.

[0055] Specifically, the metal cations (potassium, rubidium, cesium, calcium, barium) in the alkaline catalyst generate electrostatic attraction with the oxygen lone pair electrons in the active hydroxyl groups generated by the hydrolysis, stabilize the activity of the hydroxyl groups in the hydrophobic agent, and destabilize the active hydroxyl groups in the fluorosilane, hydrogen-containing silicone oil and silica sol, stimulate their condensation activity, and promote their bonding and fixation on the surface of bulk silicon-aluminum waste in the form of covalent bonds, coordination bonds, etc.

[0056] The present invention also provides an internal and external super-hydrophobic grouting material, wherein the raw materials include mortar and super-hydrophobic particles, and the raw materials of the mortar include cement 18-35% (for example, 19%, 21%, 23%, 25%, 27%, 29%, 31%, 33%, 34%), sand 54-70% (for example, 55%, 57%, 59%, 60%, 61%, 63%, 65%, 67%, 69%) and water 6.3-14% (for example, 6.5%, 7.0%, 8.5%, 9.0%, 10.0%, 11.0%, 12.0%, 13.0%, 14.0%, 15.0%, 16.0%, 17.0%, 18.0%, 19.0%, 20.0%, 21.0%, 22.0%, 23.0%, 24.0%, 25.0%, 26.0%, 27.0%, 28.0%, 29.0%, 31.0%, 33.0%, 34.0%, 35.0%, 36.0%, 37.0%, 38.0%, 39.0%, 40.0%, 41.0%, 42.0%, 43.0%, 44.0%, 45.0%, 46.0%, 47.0%, 48.0%, 49.0%, 49.0%, 48.0%, 49.0%, 49.0%, 49.0%, 40.0%, 45.0%, 46.0%, 47.0%, 48.0%, 49.0%, 49.0%, 49.0%, 49.0%, 48.0%, 49.0%, 49.0%, 7.5%, 8.0%, 9.0%, 10.0%, 11.0%, 12.0%, 13.0%, 13.9%), the super hydrophobic particles are selected from any of the above super hydrophobic particles, and the mass ratio of mortar to super hydrophobic particles is 100:(10-50), for example 100:10, 100:11, 100:15, 100:20, 100:25, 100:30, 100:35, 100:40, 100:45, 100:49.

[0057] The present invention also provides a method for preparing an internal and external super-hydrophobic grouting material, comprising the following steps:

[0058] S1. According to the ratio, weigh a large amount of silicon-aluminum waste and an alkali catalyst into a container, stir and mix evenly, then add water, and stir at room temperature for 5-7h (e.g., 5.1h, 5.5h, 6.0h, 6.5h, 6.9h); according to the ratio, add hydrogenated silicone oil, silica sol and fluorosilane and mix, stir for 1-2h (e.g., 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h), then settle for 24h, extract the bottom sediment, grind and sieve after drying to obtain super hydrophobic particles;

[0059] S2. Weigh sand and cement according to the proportion and stir at room temperature for at least 2 minutes, then add water according to the proportion and continue stirring at room temperature for at least 2 minutes, finally add super-hydrophobic particles according to the proportion and continue stirring for at least 3 minutes to obtain internal and external super-hydrophobic grouting material.

[0060] In a preferred embodiment of the present invention, in step S1, the stirring rate is 200-500 rpm.

[0061] The stirring time in step S2 is the shortest stirring time required for the preparation of internal and external super-hydrophobic grouting material, and the stirring time can be appropriately extended.

[0062] The super-hydrophobic particles, internal and external super-hydrophobic grouting materials and preparation methods thereof of the present invention are described in detail below through specific embodiments.

[0063] In the following examples, the sources of the raw materials used are as follows:

[0064] Cement, P.O42.5, was purchased from Qingdao Kramer New Building Materials Co., Ltd.;

[0065] Sodium hydroxide, analytical grade, was purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0066] Triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane, analytical grade, purchased from Qingdao Kramer New Building Materials Co., Ltd.;

[0067] 1H,1H,2H,2H-Perfluorooctyltrichlorosilane, analytical grade, was purchased from Qingdao Kramer New Building Materials Co., Ltd.;

[0068] Trifluoroisopropyldichlorosilane, analytical grade, was purchased from Qingdao Kramer New Building Materials Co., Ltd.;

[0069] Polydimethylsiloxane was purchased from Qingdao Kramer New Building Materials Co., Ltd.;

[0070] Silica sol, analytical grade, was purchased from Qingdao Kramer New Building Materials Co., Ltd.;

[0071] Hexafluoropropylene, purity 90%, purchased from Qingdao Kramer New Building Materials Co., Ltd.;

[0072] n-Heptane, analytical grade, was purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0073] Karstedt catalyst, concentration 500 ppm, purchased from Qingdao Kramer New Building Materials Co., Ltd.;

[0074] Commercially available hydrogen-containing silicone oil, analytically pure, was purchased from Qingdao Kramer New Building Materials Co., Ltd., and its structural formula is shown in the following formula (III):

[0075]

[0076] The bulk silicon-aluminum waste components used in the following examples and comparative examples are shown in Table 1:

[0077] Table 1 Composition of bulk silicon-aluminum waste

[0078]

[0079] In the following examples and comparative examples, unless otherwise specified, the raw material ratio used to prepare the hydrogen-containing silicone oil is: a:b:c=2:2:1, for example, 2 mol of trifluoroisopropyldichlorosilane, 2 mol of polydimethylsiloxane and 1 mol of hexafluoropropylene.

[0080] Example 1

[0081] The present embodiment provides an internal and external super-hydrophobic grouting material, wherein the raw materials of the mortar are composed of mortar and super-hydrophobic particles, wherein, by weight, the raw materials of the mortar are: 29.4% cement, 58.8% sand, and 11.8% water, and the raw materials of the super-hydrophobic particles are: 72% bulk silicon-aluminum waste, 5% sodium hydroxide, 10% hydrogen-containing silicone oil, 0.5% triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane, 0.5% 1H,1H,2H,2H-perfluorooctyltrichlorosilane, 5% silica sol and 7% water, wherein the bulk silicon-aluminum waste contains 30% steel slag, 50% slag, and 20% red mud, and the weight ratio of the mortar to the super-hydrophobic particles is 100:10.

[0082] In this embodiment, the preparation method of the internal and external super-hydrophobic grouting material is as follows:

[0083] S1. Preparation of super hydrophobic particles:

[0084] According to the above raw material ratio, a large amount of silicon-aluminum waste and sodium hydroxide are weighed, stirred and mixed in a container, and then water is added and stirred at room temperature for 5 hours; then hydrogen-containing silicone oil, silica sol, triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane and 1H,1H,2H,2H-perfluorooctyltrichlorosilane are added according to the ratio, stirred for 1-2 hours and then precipitated for 24 hours, the bottom precipitate is extracted, dried, ground, and sieved with a 200-mesh sieve to obtain super-hydrophobic particles;

[0085] S2. Preparation of internal and external super hydrophobic grouting material:

[0086] According to the above raw material ratio, sand and cement are weighed and stirred at room temperature for at least 2 minutes, then water is added according to the ratio and continued to be stirred at room temperature for at least 2 minutes, and finally super hydrophobic particles are added to obtain internal and external super hydrophobic grouting material.

[0087] The prepared internal and external super-hydrophobic grouting material was poured into a 40mm×40mm×160mm mold, placed at room temperature for 24 hours, then demolded, moved to a curing room for 28 days, and then the performance test was carried out as follows:

[0088] Figure 2 This is the water absorption test curve of the internal and external super-hydrophobic grouting material prepared in this embodiment. The Control group in the figure is ordinary mortar, and the Superhydrophobicity group is the internal and external super-hydrophobic grouting material prepared in this embodiment. It can be seen that with the addition of super-hydrophobic particles, the 2d water absorption rate of the internal and external super-hydrophobic grouting material is reduced by 25% compared with ordinary mortar, showing excellent water repellency.

[0089] Figure 3It is the wettability test result of the internal and external super-hydrophobic grouting material of the present embodiment, wherein the right side is the wettability test image of the test block surface layer, and the left side is the internal wettability test image of the test block after peeling off the surface layer, and the result shows that the internal and external super-hydrophobic grouting material shows three-dimensional super-hydrophobicity, and the contact angle of the internal and external surfaces is more than 150 °, indicating that the internal and external super-hydrophobic grouting material of the present invention not only has super-hydrophobicity on the surface, but also has super-hydrophobicity inside the material, even if the surface is worn, it will not cause the super-hydrophobicity of the material to be significantly affected, thus having excellent wear resistance, and the expected service life is long. And common super-hydrophobic materials mostly only embody super-hydrophobicity on the surface, and hydrophobicity is prone to a significant decline after being worn by the external environment, and the service life is relatively short.

[0090] Figure 4 The freeze-thaw mass loss test results of the internal and external super-hydrophobic grouting material of this embodiment show that the mass loss of the internal and external super-hydrophobic grouting material after 250 freeze-thaw cycles is only 2.5%, which is much lower than that of ordinary mortar, indicating that the internal and external super-hydrophobic grouting material of the present invention has excellent freeze-thaw resistance.

[0091] Figure 5 This is the result of the microscopic morphology observation of the surface of the super-hydrophobic particles prepared in this embodiment. As shown in the figure, the surface of the super-hydrophobic particles is obviously rough, which meets the characteristics of super-hydrophobic materials.

[0092] Figure 6 The infrared test results of the super-hydrophobic particles prepared in this embodiment are shown in the figure. The Control group in the figure is a bulk silicon-aluminum waste that has not been modified in step S1, and the Superhydrophobicity group is the super-hydrophobic particles prepared in step S1 of this embodiment. As shown in the figure, the super-hydrophobic particles prepared in this embodiment have an infrared radiation intensity of 1650 cm -1 Si-O-Si symmetric stretching appears near the surface. This is because silica sol, hydrogenated silicone oil, triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane and 1H,1H,2H,2H-perfluorooctyltrichlorosilane all contain Si-O-Si skeletons. -1 There is an obvious -CH3 stretching vibration peak near 2165cm -1 There is a stretching vibration peak of -Si-H nearby, 655cm -1 and 590cm -1 -CF3 and -CF2 stretching vibration peaks appeared nearby, while the bulk silicon-aluminum waste that had not been modified in step S1 did not have the above stretching vibration peaks. The results showed that the surface of bulk silicon-aluminum waste was successfully connected with fluorosilane and hydrogen-containing silicone oil, indicating that there were substances with low surface energy on the surface of the super-hydrophobic particles in the present invention.

[0093] Example 2

[0094] Based on Example 1, this embodiment changes the specific ingredients of the internal and external super-hydrophobic grouting material. In parts by weight, the raw materials of the mortar include: 29.4% cement, 58.8% sand, and 11.8% water. The raw materials of the super-hydrophobic particles include 71% bulk silica-alumina waste, 4% sodium hydroxide, 11% hydrogen-containing silicone oil, 0.5% triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane, 0.5% 1H,1H,2H,2H-perfluorooctyltrichlorosilane, 6% silica sol, and 7% water. The composition of the bulk silica-alumina waste is the same as that of Example 1, and the weight ratio of the mortar to the super-hydrophobic particles is 100:30.

[0095] The preparation method of the internal and external super-hydrophobic grouting material provided in this embodiment is the same as that in Example 1, and will not be repeated here.

[0096] The performance test of the internal and external super-hydrophobic grouting material prepared in this embodiment was carried out according to the performance test standard in Example 1, and the test results are as follows:

[0097] The 2d water absorption rate of the internal and external super-hydrophobic grouting material is reduced by 78% compared with ordinary mortar, showing three-dimensional super-hydrophobicity. The internal and external contact angles are above 150°, and the mass loss is only 5.32% after 250 freeze-thaw cycles.

[0098] Example 3

[0099] Based on Example 1, this embodiment changes the specific ingredients of the internal and external super-hydrophobic grouting material. In parts by weight, the raw materials of the mortar include: 29.4% cement, 58.8% sand, and 11.8% water. The raw materials of the super-hydrophobic particles include 72% bulk silica-alumina waste, 5% sodium hydroxide, 10% hydrogen-containing silicone oil, 0.5% triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane, 0.5% 1H,1H,2H,2H-perfluorooctyltrichlorosilane, 5% silica sol, and 7% water. The composition of the bulk silica-alumina waste is the same as that of Example 1, and the weight ratio of the mortar to the super-hydrophobic particles is 100:50.

[0100] The preparation method of the internal and external super-hydrophobic grouting material provided in this embodiment is the same as that in Example 1, and will not be repeated here.

[0101] The performance test of the internal and external super-hydrophobic grouting material prepared in this embodiment was carried out according to the performance test standard in Example 1, and the test results are as follows:

[0102] The 2d water absorption rate of the internal and external super-hydrophobic grouting material decreased by 33% compared with that of ordinary mortar, showing three-dimensional super-hydrophobicity. The internal and external contact angles were above 150°, and the mass loss was 6.31% after 250 freeze-thaw cycles.

[0103] Example 4

[0104] Based on Example 1, this embodiment changes the specific ingredients of the internal and external super-hydrophobic grouting material. In parts by weight, the raw materials of the mortar include: 29.4% cement, 58.8% sand, and 11.8% water. The raw materials of the super-hydrophobic particles include 71% bulk silicoaluminum waste, 4% sodium hydroxide, 11% hydrogen-containing silicone oil, 0.5% triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane, 0.5% 1H,1H,2H,2H-perfluorooctyltrichlorosilane, 6% silica sol, and 7% water, wherein the bulk silicoaluminum waste contains 10% phosphorus slag, 10% waste concrete, 40% silica ash, and 40% fly ash. The weight ratio of the mortar to the super-hydrophobic particles is 100:30.

[0105] The preparation method of the internal and external super-hydrophobic grouting material provided in this embodiment is the same as that in Example 1, and will not be repeated here.

[0106] The performance test of the internal and external super-hydrophobic grouting material prepared in this embodiment was carried out according to the performance test standard in Example 1, and the test results are as follows:

[0107] The 2d water absorption rate of the internal and external super-hydrophobic grouting material decreased by 77.5% compared with ordinary mortar, showing three-dimensional super-hydrophobicity. The internal and external contact angles were above 150°, and the mass loss was only 5.99% after 250 freeze-thaw cycles.

[0108] Comparative Example 1

[0109] In this comparative example, on the basis of Example 1, the specific ingredients of the internal and external super-hydrophobic grouting material were changed to prepare a grouting material. In parts by weight, the raw materials of the mortar included: 29.4% cement, 58.8% sand, and 11.8% water; the raw materials of the super-hydrophobic particles included 72% bulk silicoaluminate waste, 5% sodium hydroxide, 10% hydrogen-containing silicone oil, 0.5% triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane, 0.5% 1H,1H,2H,2H-perfluorooctyltrichlorosilane, 5% silica sol, and 7% water; and the weight ratio of the mortar to the super-hydrophobic particles was 100:1.

[0110] The preparation method of the grouting material provided in this comparative example is the same as that in Example 1, and will not be repeated here.

[0111] The grouting material prepared in this comparative example was tested for performance according to the performance test standard in Example 1, and the test results are as follows:

[0112] The 2d water absorption of the grouting material is 12% lower than that of ordinary mortar, the contact angle between the inside and the outside is about 110°, and the mass loss reaches 8.21% after 250 freeze-thaw cycles.

[0113] After analysis, it was found that since less super-hydrophobic particles were added in this comparative example, the hydrophobic effect of the grouting material was not obvious, and thus the durability effect was significantly reduced.

[0114] Comparative Example 2

[0115] In this comparative example, based on Example 1, the specific ingredients of the internal and external super-hydrophobic grouting material are changed to prepare a grouting material. In parts by weight, the raw materials of the mortar include: 29.4% cement, 58.8% sand, and 11.8% water; the raw materials of the super-hydrophobic particles include 73% bulk silicoaluminate waste, 9% sodium hydroxide, 0% hydrogenated silicone oil, 0% fluorosilane, 8% silica sol, and 10% water; and the weight ratio of the mortar to the super-hydrophobic particles is 100:30.

[0116] The preparation method of the grouting material provided in this comparative example refers to Example 1 and will not be repeated here.

[0117] The grouting material prepared in this comparative example was tested for performance according to the performance test standard in Example 1, and the test results are as follows:

[0118] The 2d water absorption of the grouting material increased by 3% compared with that of ordinary mortar, the contact angle between the inside and the outside was about 16°, and the mass loss after 250 freeze-thaw cycles increased slightly compared with that of ordinary mortar, reaching 14.23%.

[0119] After analysis, since the super-hydrophobic particles prepared in this control example are not linked with hydrogenated silicone oil and fluorosilane with low surface energy substances, only rough structures without the addition of low surface energy substances will only make the hydrophilic material more hydrophilic.

[0120] Comparative Example 3

[0121] In this comparative example, based on Example 1, the specific ingredients of the internal and external super-hydrophobic grouting material were changed to prepare a grouting material. The raw materials of the mortar included, by weight, 29.4% cement, 58.8% sand, and 11.8% water. The raw materials of the super-hydrophobic particles included 70% bulk silicoaluminate waste, 1% sodium hydroxide, 10% hydrogen-containing silicone oil, 0.5% triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane, 0.5% 1H,1H,2H,2H-perfluorooctyltrichlorosilane, 0% silica sol, and 18% water. The weight ratio of the mortar to the super-hydrophobic particles was 100:30.

[0122] The preparation method of the grouting material provided in this comparative example is the same as that in Example 1, and will not be repeated here.

[0123] The grouting material prepared in this comparative example was tested for performance according to the performance test standard in Example 1, and the test results are as follows:

[0124] The 2d water absorption rate of the grouting material is 55% lower than that of ordinary mortar, the contact angle between the inside and the outside is about 130°, and the mass loss after 250 freeze-thaw cycles is slightly lower than that of ordinary mortar, reaching 7.54%.

[0125] After analysis, it was found that since the super hydrophobic particles prepared in this control example were not linked to silica sol nanoparticles, the low surface energy substances of fluorosilane and hydrogen-containing silicone oil could only modify bulk silicon-aluminum waste into hydrophobic particles.

[0126] Comparative Example 4

[0127] In this comparative example, based on Example 1, the specific ingredients of the grouting material were changed to prepare a grouting material. The raw materials of the mortar included, by weight, 29.4% cement, 58.8% sand, and 11.8% water. The raw materials of the superhydrophobic particles included 73% bulk silicoaluminate waste, 9% sodium hydroxide, 10% commercially available hydrogenated silicone oil, 0.5% triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane, 0.5% 1H,1H,2H,2H-perfluorooctyltrichlorosilane, 8% silica sol, and 10% water. The weight ratio of the mortar to the superhydrophobic particles was 100:30.

[0128] The preparation method of the grouting material provided in this comparative example is the same as that in Example 1, and will not be repeated here.

[0129] The grouting material prepared in this comparative example was tested for performance according to the performance test standard in Example 1, and the test results are as follows:

[0130] In this control example, the 2d water absorption rate of the internal and external super-hydrophobic grouting material is greater than that of the internal and external super-hydrophobic grouting material in Example 2, and is reduced by 52% relative to ordinary mortar. The internal and external contact angles become about 130°, and the mass loss after 250 freeze-thaw cycles is slightly increased relative to that of the internal and external super-hydrophobic grouting material in Example 2, reaching 8.94%.

[0131] From the analysis of the above embodiments and comparative example 4, it can be seen that since the hydrogen-containing silicone oil prepared by the present invention contains a -CF2 group, it has extremely low surface energy, contains a flexible Si-O-Si skeleton, can provide excellent elasticity under external impact, strong CF bonds and covalent bonds, can prevent oxidation at ambient temperature, and is more robust than commercially available hydrogen-containing silicone oil.

[0132] By comparing Examples 1 to 4, it can be seen that by adding superhydrophobic particles, the 2d water absorption rate of the prepared internal and external superhydrophobic grouting material is significantly reduced compared with ordinary mortar, and it has better waterproof performance. When used as a grouting material, it can significantly improve the structural durability and reliability of concrete and extend the service life of concrete.

[0133] In addition, by comparing Examples 1 to 4, it can be seen that the ratio of superhydrophobic particles to mortar has a significant effect on the 2d water absorption of the test block. When the weight ratio of mortar to superhydrophobic particles is 100:30, the water absorption of the test block decreases most significantly, reaching 78%. When the ratio of superhydrophobic particles to mortar is increased to 100:50, the water absorption increases instead. This is because when there are more superhydrophobic particles, cement hydration will be hindered, and more pore structures will be generated inside the test block, thereby causing the water absorption to increase.

[0134] In summary:

[0135] The super-hydrophobic particles provided by the present invention are based on the "lotus effect" of micron-scale waxy papilla structure and low surface energy characteristics, so that they show excellent durability in wettability tests, waterproof performance and freeze-thaw test experiments. The internal and external super-hydrophobic grouting material prepared using the super-hydrophobic particles can provide three-dimensional super-hydrophobicity, so that it has excellent wear resistance and good air permeability, and has better durability than surface super-hydrophobic modification.

[0136] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A super hydrophobic particle, It is characterized in that By weight, the raw materials include 70-73% of bulk silicon-aluminum waste, 4-7% of base catalyst, 9-12% of hydrogenated silicone oil, 1-3% of fluorosilane, 5-8% of silica sol and 7-10% of water; The structural formula of the hydrogen-containing silicone oil is shown in the following formula (I): In the formula, a, b, c, and n are all positive integers, wherein a is between 1 and 20, b is between 1 and 20, c is between 1 and 10, and n is between 2 and 1000.

2. A super hydrophobic particle as claimed in claim 1, It is characterized in that The bulk siliceous and aluminous wastes include one or more of steel slag, ore slag, red mud, phosphorus slag, waste concrete, silica ash and fly ash.

3. A super hydrophobic particle as claimed in claim 1, It is characterized in that The alkaline catalyst includes one or more of sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, calcium hydroxide and barium hydroxide.

4. A super hydrophobic particle as claimed in claim 1, It is characterized in that The preparation method of the hydrogen-containing silicone oil is as follows: Amol trifluoroisopropyldichlorosilane, bmol polydimethylsiloxane, cmol hexafluoropropylene are used as raw materials, n-heptane is used as solvent, Karstedt catalyst is added, reacted at 80-100° C. for 6-8 hours, and the hydrogen-containing silicone oil is obtained after removing the light components; a=2, b=2, c=1.

5. A super hydrophobic particle as claimed in claim 1, It is characterized in that The fluorosilane includes triethoxy-1H,1H,2H,2H-tridecafluoro-N-octylsilane and / or 1H,1H,2H,2H-perfluorooctyltrichlorosilane.

6. A super hydrophobic particle as claimed in claim 1, It is characterized in that The silica sol includes one or more of acidic silica sol, alkaline silica sol and neutral silica sol.

7. A super hydrophobic grouting material inside and outside, It is characterized in that The raw materials include mortar and super-hydrophobic particles. By weight, the raw materials of the mortar include 18-35% cement, 54-70% sand and 6.3-14% water. The super-hydrophobic particles are selected from the super-hydrophobic particles described in any one of claims 1 to 6. The mass ratio of the mortar to the super-hydrophobic particles is 100:(10-50).

8. A method for preparing an internal and external super-hydrophobic grouting material as claimed in claim 7, It is characterized in that The steps include: S1, according to the ratio, weigh a large amount of silicon aluminum waste and alkaline catalyst into a container, stir and mix evenly, then add water, and stir at room temperature for 5-7h; according to the ratio, add hydrogen silicone oil, silica sol and fluorosilane, mix, stir for 1-2h, then settle for 24h, extract the bottom sediment, grind and sieve after drying to obtain super hydrophobic particles; S2. Weigh sand and cement according to the proportion and stir at room temperature for at least 2 minutes, then add water according to the proportion and continue stirring at room temperature for at least 2 minutes, finally add super-hydrophobic particles according to the proportion and continue stirring for at least 3 minutes to obtain internal and external super-hydrophobic grouting material.

9. A method for preparing an internal and external super-hydrophobic grouting material as claimed in claim 8, It is characterized in that In step S1, the stirring rate is 200-500 rpm.