Aluminum-lithium alloy waste recycling method
By using a combination heating of multi-layer waste layer and non-lithium-containing aluminum melt and argon degassing refining method in the recycling of aluminum-lithium alloy waste, the problems of complex processes, high costs and high impurity content in the prior art are solved, and the problem of complex processes, high costs and high impurity content in the existing technology is achieved. High-efficiency and low-cost aluminum-lithium alloy waste recycling.
Patent Information
- Application Number
- CN202410925867.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The existing aluminum-lithium alloy waste recycling technology is complex, has high cost, and has high impurity content. Lithium is easily oxidized and debris are easily agglomerated, affecting the recycling effect.
Aluminum-lithium alloy waste debris and large pieces of waste are arranged in the furnace in a radial direction to form a multi-layer waste layer, and a non-lithium-containing aluminum melt is laid on the top of the last layer, and refining by heating melting and argon gas degassing. Obtain a complex ingot.
The process flow is simplified, the recycling cost is reduced, the lithium oxidation and debris agglomeration are effectively avoided, the recycling efficiency is improved, and the slag content is reduced.
Smart Images

Figure CN118480705B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of aluminum-lithium alloy waste recycling, and in particular to a method for recycling aluminum-lithium alloy waste. Background Art
[0002] Aluminum-lithium alloy has become the preferred material for lightweight aircraft structures in the aerospace field due to its low density, high elastic modulus and high strength. However, since lithium is very active and can react with most media in the surrounding environment, the storage of aluminum-lithium alloy waste, especially small-volume waste such as debris, poses a great safety hazard and is difficult to recycle. If lithium-containing debris is added to other alloy grades, it will affect the performance of other alloys, becoming an industry problem that needs to be solved urgently in the application of aluminum-lithium alloy.
[0003] In response to the above problems, research on corresponding recycling solutions has been carried out both at home and abroad. For example, aluminum-lithium alloy debris is directly sent into the melt to melt and then cool to form a complex ingot through inert gas, vacuum melting, molten salt medium protection and other methods. However, simple inert gas and molten salt protection solutions are prone to cause problems such as the agglomeration of debris into shells and the introduction of new impurities brought by molten salt. The cost is high, the impurity content is high, and special tools are required to achieve real-time addition of debris, and the process control is complex. Summary of the invention
[0004] The present invention provides a method for recycling aluminum-lithium alloy waste, so as to solve the technical problems of complex process flow, high recycling cost and high impurity content in the aluminum-lithium alloy recycling process in the prior art.
[0005] To achieve the above object, the technical solution provided by the present invention is as follows:
[0006] The first aspect of the present invention provides a method for recycling aluminum-lithium alloy waste, comprising the following steps: arranging aluminum-lithium alloy waste fragments and large pieces of waste alternately along the radial direction in a furnace to form a waste layer, and laying multiple layers of the waste layer in the furnace; after drying the waste layer, introducing argon gas into the furnace; and laying a non-lithium aluminum melt on the top of the last layer of the waste layer to form a melt layer; heating and melting the waste layer and the melt layer in the furnace, and then using argon gas for degassing and refining to obtain a complex ingot.
[0007] Furthermore, the thickness of each waste layer is 200 mm to 500 mm.
[0008] Furthermore, the waste fragments of two adjacent waste layers are arranged alternately, and the large pieces of waste of two adjacent waste layers are arranged alternately.
[0009] Furthermore, the thickness of the melt layer is 50 mm to 200 mm.
[0010] Furthermore, the non-lithium-containing aluminum melt includes an aluminum alloy melt, in which the silicon content is less than or equal to 0.15%, and the iron content is less than or equal to 0.2%.
[0011] Furthermore, the heating and melting temperature of the waste layer and the melt layer in the furnace is less than or equal to 780°C.
[0012] Furthermore, the flow rate of the argon gas used in the degassing and refining is 40L / min to 70L / min, and the pressure of the argon gas is 5bar to 10bar.
[0013] Furthermore, the drying temperature of the waste layer is 100°C to 200°C.
[0014] Furthermore, the degassing and refined melt is introduced into a discharge box, and argon gas is introduced into the discharge box for protection.
[0015] The recycling method of aluminum-lithium alloy waste provided by the present invention adopts non-lithium aluminum melt and waste to heat and melt, and introduces argon gas for protection, which solves the problem of easy oxidation of lithium; adopts the method of alternately arranging waste debris and large pieces of waste to form a waste layer, which effectively solves the problem of easy agglomeration of debris during the smelting process; the method of pre-loading waste debris and covering the waste layer with non-lithium aluminum melt can effectively reduce the burning loss and slag content of lithium and silver in the waste. In the present invention, the waste is pre-loaded once, and it is not necessary to use other special tools to add it in real time during the operation, nor is it necessary to prefabricate block materials first, and the process is simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 Schematic diagram of the structure of the aluminum-lithium alloy scrap melting furnace in an embodiment of the present invention.
[0018] Reference numerals:
[0019] 1. Furnace; 2. Melt layer; 3. Waste layer; 4. Waste debris; 5. Large pieces of waste. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0021] It should be noted that when an element is referred to as being "fixed on" or "set on" another element, it can be directly on the other element or indirectly set on the other element; when an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0022] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0023] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, "multiple" and "several" mean two or more, unless otherwise clearly and specifically defined.
[0024] It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the conditions under which this application can be implemented. Therefore, they have no substantive technical significance. Any structural modification, change in proportional relationship or adjustment of size should still fall within the scope of the technical content disclosed in this application without affecting the effects and purposes that can be achieved by this application.
[0025] The present application provides a method for recycling aluminum-lithium alloy waste, comprising the following steps:
[0026] The scraps of aluminum-lithium alloy and the large pieces of waste are arranged alternately along the radial direction in a furnace to form a scrap layer, and multiple scrap layers are laid in the furnace; after the scrap layers are dried, argon gas is introduced into the furnace; and non-lithium aluminum melt is laid on the top of the last scrap layer to form a melt layer; the scrap layer and the melt layer are heated and melted in the furnace, and then argon gas is used for degassing and refining to obtain a complex ingot.
[0027] The recycling method of aluminum-lithium alloy waste provided by the present application adopts non-lithium aluminum melt and waste to heat and melt, and introduces argon gas for protection, which solves the problem of easy oxidation of lithium; the waste layer is formed by arranging waste debris and large pieces of waste alternately, which effectively solves the problem of easy agglomeration of debris during the smelting process; the method of pre-loading waste debris and covering the waste layer with non-lithium aluminum melt can effectively reduce the burning loss and slag content of lithium and silver in the waste. In the present invention, the waste is pre-loaded once, and there is no need to use other special tools to add it in real time during the operation, nor is there any need to pre-fabricate block materials, and the process is simple.
[0028] Reference Figure 1 In the embodiment of the present application, multiple waste layers are pre-loaded in the furnace, and the waste layers are formed by alternating waste debris and large waste blocks; preferably, the waste debris of two adjacent waste layers are arranged alternately, and the large waste blocks of two adjacent waste layers are arranged alternately, so as to better avoid the agglomeration of waste debris. Specifically, the thickness of each waste layer is 200mm to 500mm.
[0029] In the embodiment of the present application, a melt layer is laid on top of the multi-layer waste layer, and the melt layer is a non-lithium aluminum melt; specifically, the non-lithium aluminum melt includes an aluminum alloy melt, and the silicon content in the aluminum alloy melt is less than or equal to 0.15%, and the iron content is less than or equal to 0.2%. The thickness of the melt layer is 50mm to 200mm. The aluminum alloy melt can be utilized in combination with existing resources in the production process of the enterprise, for example, the aluminum alloy melt smelted on the aluminum alloy casting line is used without increasing the cost.
[0030] The argon gas used in the embodiments of the present application is preferably argon gas in a smelting furnace or a launder on a smelting and casting line in the same workshop, which is recycled to maximize the use of existing equipment and resources and save costs.
[0031] The recycling method of aluminum-lithium alloy waste in the embodiment of the present application is as follows:
[0032] Charging: Al-lithium alloy scraps and large scraps are arranged alternately along the radial direction in the furnace to form scrap layers, each layer is 200mm to 500mm high. After one layer is filled, continue to lay it upward in an alternate arrangement until 50% to 70% of the furnace height is filled.
[0033] Drying the charge: Heat the charge to 100℃~200℃, keep it for 1h~3h, and dry the waste layer.
[0034] Ventilation: Introduce argon into the furnace. It is preferred to use the argon in the smelting furnace or launder on the melting and casting line in the same workshop for recycling.
[0035] Covering: Add non-lithium aluminum melt to the waste layer to form a melt layer with a height of 50 mm to 200 mm. It is preferred to use aluminum alloy melt smelted on an aluminum alloy casting line, transfer it into a crucible, and then transfer it to the waste layer. The preferred non-lithium aluminum melt has a silicon content of no more than 0.15% and an iron content of no more than 0.2%.
[0036] Heating: Heat the waste layer and the melt layer until the charges are melted, and the melting temperature is not higher than 780℃.
[0037] Refining: After the alloy is melted, when the temperature reaches 730℃~760℃, degassing refining begins. Argon is used for refining. The argon flow rate is 40L / min~70L / min, the argon pressure is 5bar~10bar, and the rotor speed is 500rpm~800rpm.
[0038] Discharging: Argon is introduced into the discharge box, and the refined melt is introduced into the discharge box to form a complex ingot.
[0039] Cooling: After the complex ingot is cooled to a temperature less than 400°C, stop introducing argon and allow it to cool naturally to room temperature.
[0040] The embodiment of the present application solves the problem of recycling aluminum-lithium alloy waste and has the following advantages:
[0041] The waste is pre-loaded once, and there is no need to use other special tools to add it in real time during the operation, nor is there any need to prefabricate the block material, so the process is simple; the method of alternately loading aluminum-lithium alloy debris and block materials can effectively solve the problem of debris agglomeration during the smelting process; the method of pre-loading waste debris at the bottom and pre-covering the non-lithium-containing aluminum alloy melt can effectively reduce the burnout and slag content of lithium and silver in the waste; the inert gas and conventional aluminum alloy melt used in the recycling process can be combined with the existing resources in the production enterprise process for utilization without increasing costs.
[0042] The reagents used in the following examples are all commercially available.
[0043] Example 1
[0044] The recycling method of aluminum-lithium alloy waste in this embodiment is as follows:
[0045] Charging: Al-lithium alloy scraps and large scraps are arranged alternately along the radial direction in the furnace to form scrap layers, each layer is 300mm high. After one layer is filled, continue to lay it upwards in an alternate arrangement until 60% of the furnace height is filled.
[0046] Drying: Heat the charge to 150℃, keep it for 2h, and dry the waste layer.
[0047] Ventilation: Connect the argon outlet of the smelting furnace on the melting and casting line in the same workshop to the aluminum-lithium alloy scrap melting furnace through a pipeline, and introduce argon into the furnace.
[0048] Covering: The 2219 aluminum alloy melt smelted on the aluminum alloy casting line is transferred to a crucible, and the melt in the crucible is transferred to an aluminum-lithium alloy scrap furnace. Non-lithium aluminum melt is added above the scrap layer to form a melt layer. The height of the melt layer is 100 mm. The content of non-lithium aluminum melt is not more than 0.15%, and the iron content is not more than 0.2%.
[0049] Heating: Heat the waste layer and the melt layer until the charges are melted, and the melting temperature is not higher than 780℃.
[0050] Refining: After the alloy is melted, when the temperature reaches 740°C, degassing refining begins. Argon is used for refining. The argon flow rate is 60L / min, the argon pressure is 7bar, and the rotor speed is 600rpm.
[0051] Discharging: Argon is introduced into the discharge box, and the refined melt is introduced into the discharge box to form a complex ingot.
[0052] Cooling: After the complex ingot is cooled to a temperature less than 380°C, stop introducing argon and allow it to cool naturally to room temperature.
[0053] Example 2
[0054] The recycling method of aluminum-lithium alloy waste in this embodiment is as follows:
[0055] Charging: Al-lithium alloy scraps and large scraps are arranged alternately along the radial direction in the furnace to form scrap layers, each layer is 400mm high. After one layer is filled, continue to lay it upwards in an alternate arrangement until 70% of the furnace height is filled.
[0056] Drying: Heat the charge to 150℃, keep it for 2h, and dry the waste layer.
[0057] Ventilation: Connect the argon outlet of the smelting furnace on the melting and casting line in the same workshop to the aluminum-lithium alloy scrap melting furnace through a pipeline, and introduce argon into the furnace.
[0058] Covering: The 5083 aluminum alloy melt smelted on the aluminum alloy casting line is transferred to a crucible, and the melt in the crucible is transferred to an aluminum-lithium alloy scrap furnace. Non-lithium aluminum melt is added above the scrap layer to form a melt layer. The melt layer height is 100 mm. The silicon content of the non-lithium aluminum melt is not more than 0.15%, and the iron content is not more than 0.2%.
[0059] Heating: Heat the waste layer and the melt layer until the charges are melted, and the melting temperature is not higher than 780℃.
[0060] Refining: After the alloy is melted, when the temperature reaches 740°C, degassing refining begins. Argon is used for refining. The argon flow rate is 60L / min, the argon pressure is 7bar, and the rotor speed is 600rpm.
[0061] Discharging: Argon is introduced into the discharge box, and the refined melt is introduced into the discharge box to form a complex ingot.
[0062] Cooling: After the complex ingot is cooled to a temperature less than 380°C, stop introducing argon and allow it to cool naturally to room temperature.
[0063] Comparative Example 1
[0064] A method for recycling aluminum-lithium alloy waste (without covering with aluminum melt), comprising the following steps:
[0065] Step 1: Arrange the scraps of aluminum-lithium alloy and large pieces of scrap alternately in the radial direction in the furnace to form scrap layers, each layer is 300 mm high. After one layer is filled, continue to lay it upward in an alternate arrangement until 60% of the furnace height is filled.
[0066] Step 2: Dry the charge and heat it to 150℃ and keep it for 2h.
[0067] Step 3: Connect the argon outlet of the smelting furnace on the melting and casting line in the same workshop to the aluminum-lithium alloy scrap melting furnace through a pipeline.
[0068] Step 4: Heat the charge until it is melted, with the melting temperature not exceeding 770°C.
[0069] Step 5: After the alloy is melted, when the temperature reaches 740°C, degassing and refining begins. Argon is used for refining. The argon flow rate is 60L / min, the argon pressure is 7bar, and the rotor speed is 600rpm.
[0070] Step 6: Argon gas is introduced into the discharge box, and the refined melt is introduced into the discharge box to form a complex ingot.
[0071] Step 7: After the complex ingot is cooled to 380°C, stop introducing argon gas and allow it to cool naturally to room temperature.
[0072] Comparative Example 2
[0073] A method for recycling aluminum-lithium alloy waste (without alternate loading of debris and block materials) comprises the following steps:
[0074] Step 1: Fill the furnace to 60% of its height with aluminum-lithium alloy scrap chips.
[0075] Step 2: Dry the charge and heat it to 150℃ and keep it for 2h.
[0076] Step 3: Connect the argon outlet of the smelting furnace on the melting and casting line in the same workshop to the pipeline to the aluminum-lithium alloy scrap melting furnace.
[0077] Step 4: Transfer the 2219 aluminum alloy melt smelted on the aluminum alloy casting line to a crucible, and transfer the melt in the crucible to an aluminum-lithium alloy scrap melting furnace, with a melt height of 100 mm.
[0078] Step 5: Heat the charge until it is melted, with the melting temperature not exceeding 770°C.
[0079] Step 6: After the alloy is melted, when the temperature reaches 740°C, degassing and refining begins. Argon is used for refining. The argon flow rate is 60L / min, the argon pressure is 7bar, and the rotor speed is 600rpm.
[0080] Step 7: Argon gas is introduced into the discharge box, and the refined melt is introduced into the discharge box to form a complex ingot.
[0081] Step 8: After the complex ingot is cooled to 380°C, stop introducing argon and allow it to cool naturally to room temperature.
[0082] Samples were taken from the complex ingots formed after recovery in Examples 1 and 2 and Comparative Examples 1 and 2, and tested using a Bruker full spectrometer. The test standard was GB / T 7999 Aluminum and Aluminum Alloy Photoelectric Direct Reading Emission Spectroscopy Analysis Method. The test results are shown in Table 1, and the contents in Table 1 are weight percentages. In Examples 1 and 2 and Comparative Examples 1 and 2, after degassing and refining, samples were taken from the melt to measure the slag content. The slag content was measured using an ABB slag meter, and the test method was a filtration method.
[0083] Table 1 Test results of Li, Ag content and slag content in complex ingots of Examples 1, 2 and Comparative Examples 1, 2
[0084]
[0085] According to the test results in Table 1, it can be seen that the Li content and Ag content in the complex ingots of Examples 1 and 2 are greater than those of Comparative Examples 1 and 2. Compared with the comparative examples, the recycling method of aluminum-lithium alloy waste of the present application can effectively reduce the burning loss of lithium and silver, and has a high recovery rate of lithium and silver, while also effectively controlling the slag content.
[0086] The complex ingots obtained by the aluminum-lithium alloy waste recovery method of the present application can be used as raw materials for the production of aluminum-lithium alloy ingots, and can be cast into ingots of required specifications after re-smelting, dilution or supplementation of the alloy to the required components.
[0087] As measured in Example 1, the composition of the complex ingot is 4.6% Cu, 0.77% Li, 0.4% Mg, 0.29% Ag, 0.11% Zr, and the rest is aluminum. The complex ingot is used as a raw material for smelting, and then pure aluminum is added to dilute the Cu element, and metal elements such as Li are added to form a composition that meets the standard requirements of 2195 aluminum-lithium alloy: 3.7-4.3% Cu, 0.8-1.2% Li, 0.25-0.8% Mg, 0.25-0.6% Ag and 0.08-0.16% Zr, and the rest is aluminum.
[0088] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for recycling aluminum-lithium alloy waste, characterized in that: The following steps are involved: Arranging the scraps of aluminum-lithium alloy and the bulk waste alternately in radial direction in a furnace to form a scrap layer, and laying multiple scrap layers in the furnace; the scraps of two adjacent scrap layers are alternately arranged, and the bulk waste of two adjacent scrap layers are alternately arranged; After drying the waste layer, introducing argon gas into the furnace; and laying non-lithium-containing aluminum melt on the top of the last waste layer to form a melt layer; The waste layer and the melt layer are heated and melted in the furnace, and then degassed and refined with argon to obtain a complex ingot.
2. The method for recycling aluminum-lithium alloy waste according to claim 1, characterized in that: The thickness of each waste layer is 200 mm to 500 mm.
3. The method for recycling aluminum-lithium alloy waste according to claim 1, characterized in that: The thickness of the melt layer is 50 mm to 200 mm.
4. The method for recycling aluminum-lithium alloy waste according to claim 1, characterized in that: The non-lithium-containing aluminum melt includes an aluminum alloy melt, in which the silicon content is less than or equal to 0.15% and the iron content is less than or equal to 0.2%.
5. The method for recycling aluminum-lithium alloy waste according to claim 1, characterized in that: The heating and melting temperature of the waste layer and the melt layer in the melting furnace is less than or equal to 780°C.
6. The method for recycling aluminum-lithium alloy waste according to any one of claims 1 to 5, characterized in that: The flow rate of the argon gas used in the degassing refining is 40L / min to 70L / min, and the pressure of the argon gas is 5bar to 10bar.
7. The method for recycling aluminum-lithium alloy waste according to any one of claims 1 to 5, characterized in that: The drying temperature of the waste layer is 100°C to 200°C.
8. The method for recycling aluminum-lithium alloy waste according to any one of claims 1 to 5, characterized in that: The degassing and refined melt is introduced into a discharge box, and argon gas is introduced into the discharge box for protection.
Citation Information
Patent Citations
Method for recycling aluminum-lithium alloy waste scraps
CN111893335A