A method for preparing wafer-level tellurium-selenium alloy thin film and its application
The preparation of tellurium selenium alloy films through low-pressure physical vapor deposition method solves the problems of complex process and low crystallinity in traditional methods, and achieves the preparation of high-quality and low-cost tellurium selenium alloy films, which improves the performance of infrared photodetectors.
Patent Information
- Application Number
- CN202410910669.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The preparation method of traditional tellurium selenium alloy thin films is complex, has low crystallinity and high production costs, making it difficult to achieve industrial application.
Low-pressure physical vapor deposition method is used to prepare wafer-level tellurium selenium alloy films. By controlling the molar ratio of tellurium and selenium and the growth substrate, a high crystallinity and controllable morphology tellurium selenium alloy film is achieved.
A high-quality and uniform tellurium selenium alloy film preparation is achieved, which reduces production costs, avoids complex annealing steps, and improves the device's response speed and photoelectric detection performance.
Smart Images

Figure CN118480761B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of preparation of chalcogenide alloy thin films and photoelectric detectors, and in particular to a preparation method of a wafer-level tellurium-selenium alloy thin film and application thereof. Background Art
[0002] Short-wave infrared photodetectors are crucial in the fields of remote sensing, optical communication, imaging technology, night surveillance, and medical diagnosis. Traditional short-wave infrared photodetectors mainly use semiconductors such as germanium, indium gallium arsenide, indium antimonide, indium gallium arsenide phosphide, and mercury cadmium telluride. Short-wave infrared photodetectors based on these semiconductor materials face challenges such as complex preparation technology and high production costs. Therefore, the development of a new material system with simple preparation process and excellent device performance has important scientific significance and practical application value.
[0003] Tellurium is a narrow bandgap P-type semiconductor with an indirect bandgap of about 0.31 eV. In the rhombohedral tellurium phase, one atom is linked to two adjacent atoms by strong covalent bonds to form a one-dimensional spiral chain, and the spiral chains are bound by van der Waals interactions. Tellurium semiconductor materials have few dangling bonds on the surface and high stability, and have broad application prospects in the field of infrared light detection. However, optoelectronic devices prepared based on tellurium semiconductor materials have a slow response speed and extremely high dark current. Rhombohedral selenium is a single element semiconductor with a wide bandgap (≈1.95 eV), and its crystal structure is similar to that of rhombohedral tellurium. Alloying narrow-bandgap tellurium with wide-bandgap selenium to form tellurium-selenium alloy is considered to be an effective method to adjust the bandgap and its optoelectronic properties. Tellurium-selenium alloy can adjust its bandgap size (0.31-1.95 eV) by controlling different molar ratios of tellurium and selenium, which is expected to suppress the dark current of the device, improve the response speed, broaden the detection spectrum range, and achieve low-cost large-scale manufacturing and device integration. Traditional methods for preparing tellurium-selenide alloys mainly include chemical vapor transport and liquid phase epitaxy. The prepared alloy films have a single morphology and poor crystallinity, and subsequent complex annealing treatments are required to improve the crystallinity of the film. The evaporation preparation method of tellurium-selenide alloy films is to first heat tellurium powder and selenium powder in a closed environment to grow into tellurium-selenide alloy block solids, and then heat evaporate them onto the substrate using a vacuum evaporator. This method has cumbersome steps and expensive vacuum evaporators. In short, the above methods have high production costs, and the growth mechanism is still unclear. The controllable preparation of high-quality and uniform tellurium-selenide alloy films still faces huge challenges. Summary of the invention
[0004] In view of the problems of complex process, low crystallinity and difficulty in industrial application in the existing tellurium-selenium alloy film preparation technology, the present invention provides a method for preparing a wafer-level tellurium-selenium alloy film and application thereof. The preparation of tellurium-selenium alloy films with different morphologies and different molar ratios is achieved through a low-pressure physical vapor deposition method. The obtained tellurium-selenium alloy film has high crystallinity and good stability. The tellurium-selenium alloy film prepared by this method has an adjustable band gap and controllable morphology, good repeatability and controllability, and has broad application prospects in infrared photoelectric detection and imaging devices.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a wafer-level tellurium-selenium alloy thin film is prepared by a low-pressure physical vapor deposition method, and specifically comprises the following steps:
[0007] S1. The tellurium powder and selenium powder are mixed and ground evenly and placed in an alumina boat;
[0008] S2. The alumina boat containing the tellurium-selenium mixed powder is placed at the center of the tube furnace heating, and the growth substrate is placed downstream of the tube furnace in the order of gas flow from upstream to downstream;
[0009] S3. Use argon to purge the reaction chamber in the tube furnace for 30-60 minutes;
[0010] S4. Turn on the vacuum pump to place the reaction chamber in the tube furnace in a negative pressure state, raise the temperature to 450°C-650°C in an argon atmosphere, and maintain for 5-120 minutes;
[0011] S5. After the heating is completed, the temperature is cooled naturally to room temperature, and the argon gas and the vacuum pump are turned off to obtain a wafer-level tellurium selenide alloy thin film.
[0012] Furthermore, in S1, the molar ratio of tellurium powder and selenium powder is 4~9:1~6. For example, when the tellurium-selenium ratio is 9:1, 8:2, 7:3, 6:4, 5:5, 4:6, etc., the film deposition is very uniform and not easy to fall off. However, as the proportion of selenium increases further, such as when the tellurium-selenium ratio is 3:7, 2:8, 1:9 or a larger proportion of selenium, the film deposition becomes less uniform, is more likely to fall off, and may even fail to grow into a film. Therefore, controlling the molar ratio of tellurium and selenium within an appropriate range can not only ensure the high crystallinity and high stability of the alloy film obtained after the two are mixed, but also achieve precise control of tellurium-selenium alloy films with different morphologies by adjusting the molar ratio of tellurium powder and selenium powder.
[0013] Furthermore, in S2, the growth substrate is one of silicon wafer, silicon dioxide, fluorophlogopite, sapphire, FTO conductive glass, ITO conductive glass, soda-lime glass or polyimide (PI). The substrate also plays a very important role in the growth of the tellurium selenide alloy film. A suitable substrate helps to improve the uniformity and crystallinity of the tellurium selenide alloy film.
[0014] Further, in S2, the downstream of the tubular furnace is 26-34 cm downstream from the heating center of the tubular furnace.
[0015] Furthermore, in S3, the argon gas flow rate is 200-500 sccm. When cleaning the reaction chamber, a larger argon gas flow rate is used to ensure the cleaning effect and efficiency.
[0016] Furthermore, in S4, the negative pressure is -0.1 to -0.08 MPa. By constructing a negative pressure environment, the low-pressure physical vapor deposition method can be used to prepare the tellurium selenide alloy film. The two are very well matched, and the obtained tellurium selenide alloy film has high crystallinity and good stability.
[0017] Furthermore, in S4, the argon flow rate is 15-100 sccm. An appropriate argon flow rate can ensure that the reaction is carried out under an inert atmosphere without disturbing the reaction or causing waste. The heating rate is 10-16 °C / min, preferably 14 °C / min.
[0018] The tellurium-selenium alloy film obtained by the above preparation method is used to construct infrared detection devices, and has excellent photoelectric detection performance, fast response speed and high responsiveness.
[0019] Tellurium selenide alloy thin films can be grown by chemical vapor transport, liquid phase epitaxy and other methods, but the alloy effect is not ideal, and complex steps such as annealing are required to improve the crystallinity of the thin film. The present invention adopts low-pressure physical vapor deposition method, which can realize the preparation of high-crystalline tellurium selenide thin films in one step, but this method cannot solve the problems of all alloy thin films and is very picky about the type of alloy. After a large number of tests and analysis verifications, the present invention found that this method has a high degree of matching with tellurium selenide alloy thin films, so that tellurium selenide alloy thin films with uniform growth, high crystallinity and stability can be obtained.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) Compared with traditional alloy film preparation methods, the low-pressure physical vapor deposition method can achieve the controllable preparation of high-quality and uniform tellurium-selenium alloy films.
[0022] (2) The present invention can achieve precise control of tellurium-selenium alloy films with different morphologies by adjusting the molar ratio of tellurium powder and selenium powder, which is expected to broaden the spectral detection range, while reducing the device dark current and improving the device response speed.
[0023] (3) The tellurium-selenium alloy thin film prepared by the low-pressure physical vapor deposition method in one step has high crystallinity, and subsequent complex steps such as annealing are no longer required to improve the crystallinity of the thin film, and the high cost problem of the evaporation method is also avoided.
[0024] (4) The present invention can realize the controllable preparation of tellurium-selenium alloy thin films on different growth substrates, promoting their wide application in different fields.
[0025] (5) The tellurium-selenide alloy film obtained in the present invention is used to construct infrared detection devices, which exhibit excellent photoelectric detection performance in the near-infrared band (850 nm) with fast response speed and high responsiveness. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The tellurium-selenium alloy (Te 0.9 Se 0.1 ) Optical microscope characterization and scanning electron microscope characterization of the film (wherein the left and right correspond to optical microscope characterization and scanning electron microscope characterization respectively);
[0027] Figure 2 The tellurium-selenium alloy (Te 0.9 Se 0.1 ) Raman spectrum and X-ray diffraction characterization of the film (where the left and right correspond to Raman spectrum and X-ray diffraction characterization respectively);
[0028] Figure 3 The tellurium-selenium alloy (Te 0.8 Se 0.2 ) Optical microscope characterization and scanning electron microscope characterization of the film (wherein the left and right correspond to optical microscope characterization and scanning electron microscope characterization respectively);
[0029] Figure 4 The tellurium-selenium alloy (Te 0.8 Se 0.2 ) Raman spectrum and X-ray diffraction characterization of the film (where the left and right correspond to Raman spectrum and X-ray diffraction characterization respectively);
[0030] Figure 5 The tellurium-selenium alloy (Te 0.7 Se 0.3) Optical microscope characterization, scanning electron microscope characterization and energy dispersive X-ray characterization of the film (wherein the left, middle and right correspond to optical microscope characterization, scanning electron microscope characterization and energy dispersive X-ray characterization respectively);
[0031] Figure 6 The tellurium-selenium alloy (Te 0.7 Se 0.3 ) Raman spectrum, X-ray diffraction, and X-ray photoelectron spectroscopy characterization of the film (wherein the upper left, upper right, lower left, and lower right correspond to Raman spectrum, X-ray diffraction, Te 3d spectrum, and Se 3d spectrum characterization respectively);
[0032] Figure 7 The tellurium-selenium alloy (Te 0.6 Se 0.4 ) Optical microscope characterization and scanning electron microscope characterization of the film (wherein the left and right correspond to optical microscope characterization and scanning electron microscope characterization respectively);
[0033] Figure 8 The tellurium-selenium alloy (Te 0.6 Se 0.4 ) Raman spectrum and X-ray diffraction characterization of the film (where the left and right correspond to Raman spectrum and X-ray diffraction characterization respectively);
[0034] Fig. 9 The tellurium-selenium alloy (Te 0.5 Se 0.5 ) Digital photos and optical microscope characterization of the film (wherein the left and right correspond to digital photos and optical microscope characterization respectively);
[0035] Fig.10 The tellurium-selenium alloy (Te 0.5 Se 0.5 ) Scanning electron microscopy and energy dispersive X-ray characterization of the film (where the left and right correspond to scanning electron microscopy and energy dispersive X-ray, respectively);
[0036] Fig.11 The tellurium-selenium alloy (Te 0.5 Se 0.5 ) Raman spectrum and X-ray diffraction characterization of thin films (left and right correspond to Raman spectrum and X-ray diffraction characterization respectively)
[0037] Fig.12The tellurium-selenium alloy (Te 0.4 Se 0.6 ) Optical microscope characterization and scanning electron microscope characterization of the film (wherein the left and right correspond to optical microscope characterization and scanning electron microscope characterization respectively);
[0038] Fig.13 The tellurium-selenium alloy (Te 0.4 Se 0.6 ) Raman spectrum, X-ray diffraction, and X-ray photoelectron spectroscopy characterization of the film (wherein the upper left, upper right, lower left, and lower right correspond to Raman spectrum, X-ray diffraction, Te 3d spectrum, and Se 3d spectrum characterization respectively);
[0039] Fig.14 The tellurium-selenium alloy (Te 0.3 Se 0.7 ) Optical microscope characterization and scanning electron microscope characterization of the film (wherein the left and right correspond to optical microscope characterization and scanning electron microscope characterization respectively);
[0040] Fig.15 The tellurium-selenium alloy (Te 0.3 Se 0.7 ) Raman spectrum and X-ray diffraction characterization of the film (where the left and right correspond to Raman spectrum and X-ray diffraction characterization respectively);
[0041] Fig.16 The tellurium-selenium alloy (Te 0.2 Se 0.8 ) Optical microscope characterization and scanning electron microscope characterization of the film (wherein the left and right correspond to optical microscope characterization and scanning electron microscope characterization respectively);
[0042] Fig.17 The tellurium-selenium alloy (Te 0.2 Se 0.8 ) Raman spectrum and X-ray diffraction characterization of the film (where the left and right correspond to Raman spectrum and X-ray diffraction characterization respectively);
[0043] Fig.18 The tellurium-selenium alloy (Te 0.1 Se 0.9 ) Optical microscope characterization and scanning electron microscope characterization of the film (wherein the left and right correspond to optical microscope characterization and scanning electron microscope characterization respectively);
[0044] Fig.19 The tellurium-selenium alloy (Te 0.1 Se 0.9 ) Raman spectrum and X-ray diffraction characterization of the film (where the left and right correspond to Raman spectrum and X-ray diffraction characterization respectively);
[0045] Fig. 20 The tellurium-sulfur alloy (Te 0.6 S 0.4 ) Optical microscope characterization and Raman spectroscopy characterization of the film (wherein the left and right correspond to optical microscope characterization and Raman spectroscopy characterization respectively);
[0046] Fig.21 The tellurium-selenium alloy (Te 0.5 Se 0.5 ) Performance characterization of infrared photodetector of thin film (left, middle and right correspond to IT curve, response time, responsivity and photocurrent respectively). DETAILED DESCRIPTION
[0047] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments, but the present invention is not limited thereto. Example 1
[0048] 300 mg of tellurium / selenium mixed powder (molar ratio of tellurium to selenium is 9:1) was placed in an alumina boat; the alumina boat containing the tellurium / selenium mixed powder was then placed in the heating center of an open vacuum tube furnace, and the Si substrate was placed 30 cm downstream of the heating center of the tube furnace; 500 sccm of argon gas was introduced into the tube for cleaning for 30 minutes to remove the air in the tube; the vacuum pump was turned on to keep the reaction chamber in the tube furnace in a low pressure state, the argon flow rate was set to 40 sccm, the temperature of the tube furnace was increased to 550 ℃ at a heating rate of 14 ℃ / min, and maintained for 20 minutes; after the growth was completed, the tube furnace was naturally cooled to room temperature, the argon gas and the vacuum pump were turned off, and a tellurium-selenium alloy (TeSe) was obtained. 0.9 Se 0.1 )film.
[0049] The obtained tellurium-selenide alloy (Te 0.9 Se 0.1 ) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Figure 1 , Figure 2 As shown in Figure 2, optical microscopy and scanning electron microscopy showed that tellurium selenide alloy (Te 0.9 Se 0.1) film grows uniformly. Compared with pure tellurium film, tellurium selenide alloy (Te 0.9 Se 0.1 ) film showed a blue shift in the three Raman characteristic peaks. X-ray diffraction characterization data showed that the diffraction peaks moved to higher angles, among which the diffraction peak of the (101) crystal plane shifted from 27.68° to 27.93°, and the interplanar spacing decreased. This was because selenium (covalent radius 1.18 Å) replaced tellurium (covalent radius 1.37 Å) atoms, which reduced the lattice distance. The above results showed that tellurium selenide alloy (Te 0.9 Se 0.1 ) film was successfully prepared. Example 2
[0050] The tellurium-selenium alloy (Te 0.8 Se 0.2 )film.
[0051] The obtained tellurium-selenide alloy (Te 0.8 Se 0.2 ) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Figure 3 , Figure 4 As shown in Figure 2, optical microscopy and scanning electron microscopy showed that tellurium selenide alloy (Te 0.8 Se 0.2 ) film grows uniformly. Compared with pure tellurium film, tellurium selenide alloy (Te 0.8 Se 0.2 ) film showed a blue shift in the three Raman characteristic peaks. X-ray diffraction characterization data showed that the diffraction peaks moved to higher angles, among which the diffraction peak of the (101) crystal plane shifted from 27.68° to 28.23°, and the interplanar spacing decreased. The above results indicate that the tellurium selenide alloy (Te 0.8 Se 0.2 ) film was successfully prepared. Example 3
[0052] The tellurium-selenium alloy (Te) can be obtained by changing the molar ratio of tellurium to selenium in Example 1 to 7:3 and keeping other preparation conditions unchanged. 0.7 Se 0.3 )film.
[0053] The obtained tellurium-selenide alloy (Te 0.7 Se 0.3 ) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Figure 5 , Figure 6 As shown in Figure 2, optical microscopy and scanning electron microscopy showed that tellurium selenide alloy (Te 0.7 Se 0.3) thin film grows uniformly, and energy dispersive X-ray characterization qualitatively and quantitatively proves that the tellurium selenide alloy (Te 0.7 Se 0.3 ) film has a tellurium-selenium atomic ratio of about 7:3. Compared with pure tellurium film, tellurium-selenium alloy (Te 0.7 Se 0.3 ) The three Raman characteristic peaks of the film are blue-shifted. X-ray diffraction characterization data show that the diffraction peaks move to higher angles, among which the diffraction peak of the (101) crystal plane shifts from 27.68° to 28.53°, and the interplanar spacing decreases. X-ray photoelectron spectroscopy characterization data is further used to directly obtain the chemical composition and surface information of the tellurium selenide film. In the Te 3d spectrum, there are two peaks Te 3d 5 / 2 and Te 3d 3 / 2 are located at 573.83 eV and 584.19 eV respectively. Compared with pure tellurium film, Te 3d 5 / 2 and Te 3d 3 / 2 The peak positions all move toward the direction of high binding energy, which is because the bond energy of tellurium-selenium bond is smaller than that of selenium-selenium bond. In the Se 3d energy spectrum, there are two peaks Se 3d 5 / 2 and Se 3d 3 / 2 are located at 54.98 eV and 55.81 eV respectively. Compared with pure selenium film, Se 3d 5 / 2 and Se 3d 3 / 2 The peak positions all move toward the direction of low binding energy, which is because the bond energy of Se-Se bond is larger than that of Tellurium-Se bond. 0.7 Se 0.3 ) film was successfully prepared. Example 4
[0054] The tellurium-selenium alloy (Te 0.6 Se 0.4 )film.
[0055] The obtained tellurium-selenide alloy (Te 0.6 Se 0.4 ) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Figure 7 , Figure 8 As shown in Figure 2, optical microscopy and scanning electron microscopy showed that tellurium selenide alloy (Te 0.6 Se 0.4 ) film grows uniformly. Compared with pure tellurium film, tellurium selenide alloy (Te 0.6 Se 0.4) film showed a blue shift in the three Raman characteristic peaks. X-ray diffraction characterization data showed that the diffraction peaks moved to higher angles, among which the diffraction peak of the (101) crystal plane shifted from 27.68° to 28.72°, and the interplanar spacing decreased. The above results indicate that the tellurium selenide alloy (Te 0.6 Se 0.4 ) film was successfully prepared. Example 5
[0056] The tellurium-selenium alloy (Te) can be obtained by changing the molar ratio of tellurium to selenium in Example 1 to 5:5 and keeping other preparation conditions unchanged. 0.5 Se 0.5 )film.
[0057] The obtained tellurium-selenide alloy (Te 0.5 Se 0.5 ) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Fig. 9 , Fig.10 , Fig.11 shown. Fig. 9 Wafer-level Te 0.5 Se 0.5 Digital photo of the film. According to optical microscopy and scanning electron microscopy, the tellurium selenide alloy (Te 0.5 Se 0.5 ) thin film grows uniformly. Energy dispersive X-ray characterization has qualitatively and quantitatively proved that the tellurium selenide alloy (Te 0.5 Se 0.5 ) film has a tellurium-selenium atomic ratio of about 5:5. Compared with pure tellurium film, tellurium-selenium alloy (Te 0.5 Se 0.5 ) film showed a blue shift in the three Raman characteristic peaks. X-ray diffraction characterization data showed that the diffraction peaks moved to higher angles, among which the diffraction peak of the (101) crystal plane shifted from 27.68° to 28.9°, and the interplanar spacing decreased. The above results show that the tellurium selenide alloy (Te 0.5 Se 0.5 ) film was successfully prepared.
[0058] Constructing tellurium-selenide alloy (Te 0.5 Se 0.5 ) Thin film infrared photoelectric detector and photoelectric performance test, the results are as follows Fig.21 As shown. Under a bias voltage of 0.5 V, the tellurium selenide alloy (Te 0.5 Se 0.5 The film has a good photoresponse to 850 nm near-infrared light, with a rise time and a fall time of 67 ms and 122 ms, respectively. The responsivity decreases with the increase of optical power density. 2The maximum response can reach 310 mA / W. θ ) derived the functional relationship between the photocurrent and the incident light power density and determined the exponent θ to be ~0.64, which has good optoelectronic properties. Example 6
[0059] The tellurium-selenium alloy (Te 0.4 Se 0.6 )film.
[0060] The obtained tellurium-selenide alloy (Te 0.4 Se 0.6 ) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Fig.12 , Fig.13 As shown in Figure 2, optical microscopy and scanning electron microscopy showed that tellurium selenide alloy (Te 0.4 Se 0.6 ) film grows uniformly. Compared with pure tellurium film, tellurium selenide alloy (Te 0.4 Se 0.6 ) film showed a blue shift in the three Raman characteristic peaks. X-ray diffraction characterization data showed that the diffraction peaks moved to higher angles, among which the diffraction peak of the (101) crystal plane shifted from 27.68° to 29.04°, and the interplanar spacing decreased. X-ray photoelectron spectroscopy characterization data was further used to directly obtain the tellurium selenide alloy (Te 0.4 Se 0.6 ) The chemical composition and surface information of the film. In the Te 3d spectrum, there are two peaks Te 3d 5 / 2 and Te 3d 3 / 2 They are located at 573.88 eV and 584.25 eV respectively. Compared with pure tellurium film, both peaks move toward higher binding energy, which is because the bond energy of tellurium-selenium bond is smaller than that of selenium-selenium bond. In the Se 3d energy spectrum, there are two peaks Se 3d 5 / 2 and Se 3d 3 / 2 are located at 55.21 eV and 56.05 eV respectively. Compared with the pure selenium film, both of them move toward the direction of low binding energy. This is because the bond energy of Se-Se bond is larger than that of Tellurium-Se bond. The above results show that Tellurium-Selenium alloy (Te 0.4 Se 0.6 ) film was successfully prepared. Example 7
[0061] The tellurium-selenium alloy (Te 0.3 Se 0.7 )film.
[0062] The obtained tellurium-selenide alloy (Te 0.3 Se 0.7 ) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Fig.14 , Fig.15 Compared with pure tellurium thin film, tellurium selenide alloy (Te 0.3 Se 0.7 ) film showed a blue shift in the three Raman characteristic peaks. X-ray diffraction characterization data showed that the diffraction peaks moved to higher angles, among which the diffraction peak of the (101) crystal plane shifted from 27.68° to 29.20°, and the interplanar spacing decreased, indicating that the tellurium selenide alloy (Te 0.3 Se 0.7 ) film. Fig.14 It can be seen that the grown tellurium-selenide alloy (Te 0.3 Se 0.7 )The film growth is not uniform. Example 8
[0063] The tellurium-selenium alloy (Te 0.2 Se 0.8 )film.
[0064] The obtained tellurium-selenide alloy (Te 0.2 Se 0.8 ) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Fig.16 , Fig.17 Compared with pure tellurium thin film, tellurium selenide alloy (Te 0.2 Se 0.8 ) film showed a blue shift in the three Raman characteristic peaks. X-ray diffraction characterization data showed that the diffraction peaks moved to higher angles, among which the diffraction peak of the (101) crystal plane shifted from 27.68° to 29.37°, and the interplanar spacing decreased, indicating that the tellurium selenide alloy (Te 0.2 Se 0.8 ) The film has a certain growth. Fig.16 It can be seen that the generated tellurium-selenide alloy (Te 0.2 Se 0.8 )The film exhibits a distinctly non-uniform morphology. Example 9
[0065] The tellurium-selenium alloy (Te 0.1 Se 0.9 )film.
[0066] The obtained tellurium-selenide alloy (Te 0.1 Se 0.9) Thin film samples were subjected to optical microscopy, scanning electron microscopy, Raman spectroscopy, and X-ray diffraction. The results are as follows Fig.18 , Fig.19 Compared with pure tellurium thin film, tellurium selenide alloy (Te 0.1 Se 0.9 ) film showed a blue shift in the three Raman characteristic peaks. X-ray diffraction characterization data showed that the diffraction peaks moved to higher angles, among which the diffraction peak of the (101) crystal plane shifted from 27.68° to 29.49°, and the interplanar spacing decreased, indicating that the tellurium selenide alloy (Te 0.1 Se 0.9 ) The film has a certain growth. Fig.18 It can be seen that the generated (Te 0.1 Se 0.9 ) The film is not only uneven, but it can't even be connected into a piece, thus failing to form a film shape.
[0067] By comparing the above characterization diagrams of different tellurium and selenium molar ratios, it can be seen that as the proportion of selenium increases, the film deposition gradually becomes less uniform, is easier to fall off, and may even fail to grow into a thin film form. Example 10
[0068] The tellurium / selenium mixed powder (the molar ratio of tellurium to selenium is 6:4) in Example 4 was changed to a tellurium / sulfur mixed powder (the molar ratio of tellurium to sulfur is 6:4), and other preparation conditions remained unchanged.
[0069] The obtained samples were characterized by optical microscopy and X-ray diffraction. Fig. 20 As shown in Figure 2, the tellurium sulfur film is not uniform as shown by optical microscopy. X-ray diffraction data show the crystal structure at 23.67°, 29.84° and 43.86°, and the diffraction peaks point to the (100), (101) and (102) crystal planes of the tellurium film, respectively. These diffraction peaks are consistent with the standard colorimetric card (JCPDS 06-0362). The above results indicate that a uniform and adjustable tellurium sulfur film cannot be successfully prepared under the same conditions.
Claims
1. A method for preparing a wafer-level tellurium-selenium alloy thin film, characterized in that: The low-pressure physical vapor deposition method is used for preparation, which specifically includes the following steps: S1. The tellurium powder and selenium powder are mixed and ground evenly in a molar ratio of 4 to 9: 1 to 6, and placed in an alumina boat; S2. The alumina boat containing the tellurium-selenium mixed powder is placed at the center of the tube furnace heating, and the growth substrate is placed downstream of the tube furnace in the order of gas flow from upstream to downstream; S3. Use argon to purge the reaction chamber in the tube furnace for 30-60 minutes; S4. Turn on the vacuum pump to make the reaction chamber in the tube furnace in a negative pressure state, the negative pressure is -0.1 ~ -0.08MPa, and heat to 450 ℃ -650 ℃ in an argon atmosphere, and maintain for 5-120 minutes; S5. After the heating is completed, the temperature is cooled naturally to room temperature, and the argon gas and the vacuum pump are turned off to obtain a wafer-level tellurium selenide alloy thin film.
2. The method for preparing a wafer-level tellurium-selenium alloy thin film according to claim 1, characterized in that: In S2, the growth substrate is one of silicon wafer, silicon dioxide, fluorophlogopite, sapphire, FTO conductive glass, ITO conductive glass, soda-lime glass or polyimide.
3. The method for preparing a wafer-level tellurium-selenium alloy thin film according to claim 1, characterized in that: In S2, the downstream of the tube furnace is 26-34 cm downstream from the heating center of the tube furnace.
4. The method for preparing a wafer-level tellurium-selenium alloy thin film according to claim 1, characterized in that: In S3, the argon gas flow rate is 200-500 sccm.
5. The method for preparing a wafer-level tellurium-selenium alloy thin film according to claim 1, characterized in that: In S4, the argon gas flow rate is 15-100 sccm; the heating rate is 10~16 ℃ / min.
6. Use of the wafer-level tellurium-selenide alloy thin film obtained by the preparation method according to any one of claims 1 to 5 in constructing infrared detection devices.
Citation Information
Patent Citations
Selenium tellurium alloy film, light guide type infrared light detector and preparation method
CN114990520A
Preparation method of large-area Te-MX2 vertical heterojunction with enhanced nonlinear optical property
CN115652261A
Improvements in and relating to optical filters
GB1014300A