A kind of high activity silver powder and preparation method thereof
By using a high-polar surfactant to form an internal pore structure in the preparation of silver powder, the problem of low sintering activity of silver powder is solved, the preparation process is simplified and the photoelectric conversion efficiency of solar cells is improved.
Patent Information
- Application Number
- CN202410957228.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-17
Smart Images

Figure CN118492396B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of conductive silver powder, and in particular relates to a high-activity silver powder and a preparation method thereof. Background Art
[0002] The photovoltaic industry is an important development direction for the transformation of the global energy structure, and countries around the world attach great importance to the development of the photovoltaic industry. Photovoltaic silver paste is a key material for making photovoltaic cell electrodes, the largest auxiliary material for photovoltaic cells, and the second largest component of cell costs, accounting for about 33% of the non-silicon cost of cells.
[0003] Solar cells are mainly composed of silicon wafers, passivation films and metal electrodes. The metal electrodes are formed by printing photovoltaic silver paste on both sides of the silicon wafer through screen printing, drying and sintering. Photovoltaic silver paste, as the electrode material of photovoltaic crystalline silicon cells, mainly plays the role of collecting and conducting photogenerated carriers. It is often used on the light-receiving side of P-type cells and both sides of N-type cells.
[0004] Photovoltaic silver powder is the most important material for producing photovoltaic silver paste. Silver powder accounts for about 90% of the silver paste composition, and silver powder accounts for more than 95% of the silver paste cost. The morphology, structure, particle size and distribution characteristics, tap density, specific surface area, sintering performance, corrosion resistance, etc. of silver powder will directly affect the performance of the paste, and the morphology, particle size and sintering performance are the most critical characteristics, which directly or indirectly determine the photoelectric conversion efficiency of crystalline silicon cells.
[0005] At present, the preparation methods of silver powder mainly include physical methods and chemical methods. The physical methods include gas phase evaporation condensation method, physical and chemical method, grinding method, etc. The above methods have the disadvantages of high cost and low efficiency. Chemical methods include liquid phase reduction method, sol-gel method, electrolysis method, spray thermal decomposition method, other pyrometallurgical processes, etc. Among them, liquid phase reduction method is the main preparation method. In the preparation process, most of the silver-containing solution is mixed with reducing agent solution and dispersant solution. The obtained silver powder products are mostly dense structures, and there are still problems such as high melting point and low sintering activity. In addition, hollow silver powder is prepared by liquid phase reduction method. In this process, a large number of nanobubbles need to be introduced, and silver nitrate is adsorbed on its surface with nanobubbles as carriers. It is also necessary to adjust the pH value of the reaction solution and other steps. The preparation process is relatively complicated. In addition, this method only examines the increase of the specific surface area of silver powder by forming a hollow structure, and does not study the melting point characteristics of silver powder. The higher melting point will still affect the sintering performance of silver powder, limiting its application range in photovoltaic cells, such as low temperature curing silver paste. Summary of the invention
[0006] The invention discloses a method for preparing high-activity silver powder, aiming to solve the problem that the existing silver powder has low sintering activity, resulting in low photoelectric conversion efficiency of solar cells.
[0007] In order to solve the above problems, the technical solution adopted by the present invention is:
[0008] In one aspect of the present invention, a method for preparing a high-activity silver powder is provided, the preparation method comprising the following steps:
[0009] S1, adding a silver-containing compound and a high-polarity surfactant to a solvent, stirring evenly to obtain a solution A;
[0010] S2, adding a reducing agent and a dispersant to the solvent, stirring evenly, to obtain a solution B;
[0011] S3, injecting the solution A and the solution B into a reaction container respectively, reacting at 20-40° C. for a period of time to obtain a reaction solution;
[0012] S4, centrifuging the reaction solution at least once, removing the upper layer of solution, and drying to obtain high-activity silver powder with pores inside.
[0013] Preferably, the content of the silver-containing compound is 80-160 parts by mass; the content of the reducing agent is 50-120 parts by mass; the content of the high-polarity surfactant is 40-100 parts by mass; the content of the dispersant is 20-40 parts by mass; and the content of the solvent is 1000-2500 parts by mass.
[0014] Preferably, in step S1, the silver-containing compound is at least one of silver nitrate and silver trifluoroacetate.
[0015] Preferably, in step S1, the high polarity surfactant is a copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide.
[0016] Preferably, in step S1, the molecular weight of the high polarity surfactant is 10000-30000, and the molecular weight distribution is 1.2-2.5.
[0017] Preferably, in step S1, the high polarity surfactant is prepared by the following method:
[0018] The histamine acrylamide monomer, 2-hydroxypropyl methacrylamide monomer, chain transfer agent, thermal initiator, methanol and deionized water are uniformly mixed, and free radical polymerization is carried out at 80-90° C. for 5-7 hours to obtain a copolymer solution of histamine acrylamide and 2-hydroxypropyl methacrylamide;
[0019] The copolymer solution is diluted, settled, filtered and dried to obtain a copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide.
[0020] Preferably, in step S2, the reducing agent is at least one of formaldehyde, sodium borohydride, hydrazine hydrate, ascorbic acid, sodium ascorbate, and glucose.
[0021] Preferably, in step S2, the dispersant is at least one of gelatin, gum arabic, polyvinyl pyrrolidone, sodium citrate and polyvinyl alcohol.
[0022] Preferably, in step S3, the solution A and the solution B are injected into the reaction container at a constant speed to react for 8-12 minutes; wherein the constant speed is 50-1000 mL / min.
[0023] Preferably, in step S4, the high-activity silver powder has an obvious pore structure inside.
[0024] Preferably, in step S4, the average particle size of the high-activity silver powder is 0.5-2.0 μm.
[0025] Preferably, in step S4, the tap density of the high-activity silver powder is 5.0 to 6.5 g / cm 3 .
[0026] Preferably, in step S4, the specific surface area of the high-activity silver powder is 0.5 to 1.2 m 2 / g.
[0027] Another aspect of the present invention provides a high-activity silver powder, which is prepared by the preparation method described above.
[0028] Compared with the prior art, the present invention uses a high-polarity surfactant in the process of preparing silver powder. The polyhistamine acrylamide chain segment in the high-polarity surfactant can be coated on the high surface energy surface (111) of the silver grains, so that the silver grains can only grow from the two surfaces (100) and (110) with lower surface energy. At the same time, the poly 2-hydroxypropyl methacrylamide hydrophilic chain segment in the surfactant forms a steric hindrance, thereby forcing the silver powder to form an internal pore structure. The present invention has simple preparation steps and good repeatability, and can effectively reduce the cost of silver powder preparation. The obtained high-activity silver powder has good particle size uniformity and can meet the application requirements of conductive paste. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a flowchart of a method for preparing high-activity silver powder according to an embodiment of the present invention;
[0030] Figure 2 The internal microscopic morphology of the method for preparing high-activity silver powder in Example 1 of the present invention;
[0031] Figure 3 The melting point results of Example 1 and Comparative Examples 1-3 of the present invention are shown below;
[0032] Figure 4 This is the internal microscopic morphology of the silver powder of Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0033] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by those of ordinary skill in the art without the need for creative work are within the scope of protection of the present disclosure.
[0034] Unless otherwise specified, the technical terms or scientific terms used in the present disclosure shall have the usual meanings understood by persons with ordinary skills in the field to which the present disclosure belongs. The terms "include" or "comprising" used in the present disclosure neither limit the shapes, numbers, steps, operations and / or groups thereof mentioned, nor exclude the presence or addition of one or more other different shapes, numbers, steps, operations and / or groups thereof.
[0035] like Figure 1 As shown, in one aspect of the present disclosure, a method for preparing high-activity silver powder S100 is provided, which specifically includes the following steps S110-S130:
[0036] S110, adding a silver-containing compound and a high-polarity surfactant to a solvent, stirring evenly, to obtain a solution A.
[0037] Specifically, a solvent may be added to the liquid preparation kettle I, and then the silver-containing compound may be added to the liquid preparation kettle I, and the silver-containing compound may be fully dissolved in the solvent by mechanical stirring, and then a high-polarity surfactant may be added to the liquid preparation kettle I, and the mixed solution may be stirred evenly to obtain a silver-containing solution, i.e., solution A. It is understood that, in other embodiments, the high-polarity surfactant may be added first and then the silver-containing compound, or the high-polarity surfactant and the silver-containing compound may be added simultaneously, and the present embodiment does not limit the order and method of adding the silver-containing compound and the high-polarity surfactant.
[0038] In some preferred embodiments, the solvent can be at least one of deionized water, ethanol, isopropanol, isoamyl alcohol, and ethylene glycol. In addition, the content of the solvent can be preferably 1000-2500 parts by mass, for example, 1000 parts by mass, 1300 parts by mass, 1500 parts by mass, 2000 parts by mass, 2200 parts by mass, 2500 parts by mass, etc.
[0039] In other preferred embodiments, the silver-containing compound is at least one of silver nitrate and silver trifluoroacetate. In addition, the content of the silver-containing compound may preferably be 80-160 parts by mass, for example, 80 parts by mass, 90 parts by mass, 100 parts by mass, 120 parts by mass, 140 parts by mass, 160 parts by mass, etc.
[0040] In other preferred embodiments, the content of the high-polarity surfactant may preferably be 40-100 parts by mass, for example, 40 parts by mass, 50 parts by mass, 70 parts by mass, 89 parts by mass, 90 parts by mass, 100 parts by mass, etc.
[0041] In other preferred embodiments, the high-polarity surfactant is a copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide, which not only plays a coating role, coating the silver crystal core, which is equivalent to a coating agent for the silver crystal core, but also plays a steric hindrance role. Based on the steric hindrance effect, the growth of the coated surface of the silver crystal core is inhibited, so that it grows from the uncoated surface, thereby adjusting the internal pore structure of the silver powder, thereby improving the sintering activity of the silver powder.
[0042] It is worth noting that the high polarity surfactant used in this embodiment is not the commonly referred to small molecule surfactant or dispersant, but an organic polymer with a larger molecular weight and higher polarity, such as the copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide mentioned above.
[0043] As a further preferred embodiment, the molecular weight of the copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide is preferably 10000-30000, and the molecular weight distribution is preferably 1.2-2.5, which can adjust the uniformity of the silver powder particle size and make the melting point of the silver powder consistent.
[0044] As a further preferred embodiment, the highly polar surfactant is formed by the following method:
[0045] 5-15 parts by weight of histamine acrylamide monomer, 5-15 parts by weight of 2-hydroxypropyl methacrylamide monomer, 0.002-0.007 parts by weight of chain transfer agent, 0.01-0.05 parts by weight of thermal initiator, methanol and 70-90 parts by weight of deionized water are added into a round-bottom flask and mixed evenly, and free radical polymerization is carried out at 80-90° C. for 5-7 hours to obtain a copolymer solution of histamine acrylamide and 2-hydroxypropyl methacrylamide; the copolymer solution is diluted with 80-110 parts by weight of methanol, precipitated in acetone for 3 times, filtered and then vacuum dried at room temperature for 40-50 hours to obtain a copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide.
[0046] Among them, in the preparation process of high-polarity surfactant, the chain transfer agent can be octadecyl mercaptan, and the thermal initiator can be benzoyl peroxide, etc. Of course, for those skilled in the art, other chain transfer agents and thermal initiators can also be used, and there is no specific limitation on this.
[0047] S120. Add a reducing agent and a dispersant to the solvent, stir evenly, and obtain solution B.
[0048] Specifically, the solvent can be added to the liquid preparation kettle II, and then the reducing agent can be added to the liquid preparation kettle II, and the reducing agent can be fully dissolved in the solvent by mechanical stirring, and then the dispersant can be added to the liquid preparation kettle II, and the mixed solution can be stirred evenly to obtain solution B. It can be understood that in other embodiments, the dispersant can be added first and then the reducing agent, or the dispersant and the reducing agent can be added at the same time, and this embodiment does not limit the order and method of adding the dispersant and the reducing agent.
[0049] In some preferred embodiments, the solvent may also be at least one of deionized water, ethanol, isopropanol, isopentanol, and ethylene glycol.
[0050] In addition, the content of the solvent may also preferably be 1000-2500 parts by mass, that is, the total solvent content required for this embodiment is 2000-5000 parts by mass, which is divided into two parts, one of which is used to mix with the silver-containing compound and the high-polarity surfactant to form solution A, and the other is used to mix with the reducing agent and the dispersant to form solution B.
[0051] In other preferred embodiments, the reducing agent is at least one of formaldehyde, sodium borohydride, hydrazine hydrate, ascorbic acid, sodium ascorbate, and glucose. In addition, the content of the reducing agent may preferably be 50-120 parts by mass, for example, 50 parts by mass, 70 parts by mass, 90 parts by mass, 100 parts by mass, 120 parts by mass, etc.
[0052] In other preferred embodiments, the dispersant is at least one of gelatin, gum arabic, polyvinyl pyrrolidone, sodium citrate, and polyvinyl alcohol. In addition, the content of the dispersant may preferably be 20-40 parts by mass, for example, 20 parts by mass, 30 parts by mass, 40 parts by mass, etc.
[0053] It can be understood that the preparation order of solution A and solution B can be adjusted according to the experimental requirements, that is, solution A can be prepared first and solution B can be prepared later, or solution B can be prepared first and solution A can be prepared later, or solution A and solution B can be prepared at the same time. This embodiment does not limit the preparation order of solution A and solution B.
[0054] S130, injecting solution A and solution B into a reaction container respectively, reacting at 20-40° C. for a period of time to obtain a reaction solution.
[0055] In step S130, when solution A and solution B are mixed, they can be injected separately at a constant speed to make the solutions mixed more evenly. The mixture is reacted at 20-40° C. for 8-12 minutes to obtain a yellowish brown reaction solution.
[0056] It should be understood that there is no specific limitation on the injection method, and any injection method used in conventional experiments can be used, for example, injecting it into a reactor using a syringe pump, etc. In addition, there is no specific limitation on the reaction vessel, for example, a reactor.
[0057] Specifically, solution A and solution B can be injected into the constant temperature reactor at a rate of 50-1000 mL / min by a syringe pump. Of course, in order to improve the reaction efficiency, stirring can also be used during the reaction.
[0058] In some preferred embodiments, the injection speed of the injection pump is preferably 100-200 mL / min. Within this injection speed range, solution A and solution B can be fully mixed and reacted completely.
[0059] S140, centrifuging the reaction solution at least once, removing the upper layer of the solution, and drying to obtain high-activity silver powder.
[0060] Specifically, the reaction solution can be centrifuged at a centrifugal speed of 1500-2000 r / min for 10-20 minutes, then the upper solution is poured out, and then 500 parts of anhydrous ethanol are added and stirred for 5-10 minutes. Then, the reaction solution is centrifuged at a centrifugal speed of 2000-3000 r / min for 10-20 minutes, and then the upper solution is poured out, and the reaction solution is placed in a drying oven and dried at 65° C. for 7-9 hours to obtain micron-level high-activity silver powder, which has a pore structure inside. The obtained high-activity silver powder has an average particle size of 0.5-2.0 μm and a tap density of 5.0-6.5 g / cm 3 , with a specific surface area of 0.5 to 1.2 m 2 / g.
[0061] The average size of the high-activity silver powder in this embodiment is at the micron level, and there are holes of different sizes inside it. Some spherical silver powders have multiple small holes inside, and some spherical silver powders have one large hole inside. Of course, some spherical silver powders have one large hole inside, and some small holes are formed around the large hole, which effectively increases the specific surface area and sintering activity of the silver powder.
[0062] In this embodiment, based on the addition of a high-polarity surfactant to the silver-containing solution in advance, the surfactant is coated in the silver crystal nucleus to form a silver-containing solution. When mixed with other components, spherical silver powder with a porous structure can be formed, and the pore size inside the spherical silver powder can also be adjusted, thereby improving the sintering activity of the silver powder and reducing the melting point of the silver powder. The melting point is lower than the melting point of the silver powder prepared by the conventional method, which solves the problem of low sintering activity of the existing silver powder and can help achieve a higher photoelectric conversion efficiency of solar cells when it is used in the silver paste of solar cells.
[0063] Another aspect of the present disclosure is to provide a high-activity silver powder, which is prepared by the preparation method mentioned above. For the specific process, please refer to the above description and will not be repeated here. The high-activity silver powder has an obvious pore structure inside; the average particle size of the high-activity silver powder is 0.5-2.0 μm, and the tap density is 5.0-6.5 g / cm 3 , with a specific surface area of 0.5 to 1.2 m 2 / g. The silver powder has a low melting point and high sintering activity, and can meet the application requirements of high-temperature silver paste for solar cells, high-temperature silver-aluminum paste for solar cells, low-temperature silver paste and other electronic pastes.
[0064] The preparation method of high-activity silver powder will be further described below in conjunction with several specific examples:
[0065] Example 1
[0066] The method for preparing the highly active silver powder in this example comprises the following steps:
[0067] S1. Add 1000 g of solvent into a liquid preparation kettle I, then add 100 g of silver nitrate, stir mechanically and fully dissolve, then add 60 g of a high-polarity surfactant, stir evenly, and obtain solution A.
[0068] Among them, the high polar surfactant is formed by the following process: 10 parts by mass of histamine acrylamide monomer, 10 parts by mass of 2-hydroxypropyl methacrylamide monomer, 0.005 parts by mass of chain transfer agent octadecyl mercaptan, 0.03 parts by mass of thermal initiator benzoyl peroxide, and 80 parts by mass of deionized water are added to a 250 mL round-bottom flask and mixed evenly, and free radical polymerization is carried out at 85° C. for 6 hours to obtain a copolymer emulsion of histamine acrylamide and 2-hydroxypropyl methacrylamide. The copolymer emulsion is diluted with 100 parts of methanol, precipitated in acetone 3 times, filtered and vacuum dried at room temperature for 48 hours to obtain a high polar surfactant copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide.
[0069] S2. Add 1000 g of solvent into the liquid preparation kettle II, then add 60 g of ascorbic acid, stir mechanically and fully dissolve, then add 20 g of sodium citrate, stir evenly, and obtain solution B.
[0070] S3. Solution A and solution B were injected into the thermostatic reactor at a constant speed of 100 mL / min by injection pumps, the reaction temperature was 30° C., and the reaction was stirred for 10 min to obtain a khaki reaction solution.
[0071] S4. The reaction solution was centrifuged at a centrifugal speed of 1500 r / min for 15 min, and then the upper layer solution was poured out, and then 1 part of anhydrous ethanol was added, and ultrasonication was performed for 30 seconds. Then, the reaction solution was centrifuged at a centrifugal speed of 2000 r / min for 15 min, and then the upper layer solution was poured out, and the reaction solution was placed in a drying oven and dried at 65°C for 8 hours to obtain micron-level high-activity silver powder, and its internal microscopic morphology is as follows: Figure 2 As shown, the average particle size is 1.7 μm and the tap density is 6.02 g / cm 3 , with a specific surface area of 0.67m 2 / g.
[0072] As shown in Table 1, the melting point of the high-activity silver powder obtained in Example 1 is 298°C. Figure 3 As shown, the black line represents the melting point result of Example 1, and the abscissa corresponding to the peak value is the melting point of the silver powder. The lower the melting point, the higher the sintering activity.
[0073] Comparative Example 1
[0074] The preparation method of the high-activity silver powder in this example is the same as that in Example 1, except that the content of the high-polarity surfactant is changed to 5 g, and other conditions remain unchanged. The average particle size of the obtained silver powder is 1.75 μm, and the tap density is 6.14 g / cm 3 , with a specific surface area of 0.63m 2 / g. The melting point is 353°C, as shown in Table 1 and Figure 3 shown.
[0075] Compared with Example 1, in Comparative Example 1, after reducing the content of the high-polarity surfactant, the melting point of the obtained high-activity silver powder increases to greater than 350° C., thereby reducing the sintering activity of the silver powder.
[0076] Comparative Example 2
[0077] The preparation method of the high-activity silver powder in this example is the same as that in Example 1, except that the content of the high-polarity surfactant is changed to 10 g, and other conditions remain unchanged. The average particle size of the obtained silver powder is 1.6 μm, and the tap density is 5.98 g / cm 3 , with a specific surface area of 0.72m 2 / g. The melting point is 346°C, as shown in Table 1 and Figure 3 shown.
[0078] Compared with Example 1, in this Comparative Example 2, after reducing the content of the high-polarity surfactant, the melting point of the obtained high-activity silver powder increases, thereby reducing the sintering activity of the silver powder. Compared with Comparative Example 1, after appropriately increasing the content of the high-polarity surfactant, the melting point of the obtained silver powder is slightly reduced, and its sintering activity is improved.
[0079] Comparative Example 3
[0080] The preparation method of the high-activity silver powder in this example is the same as that in Example 1, except that no high-polarity surfactant is added, that is, the content of this component is 0 g, and other conditions remain unchanged. The average particle size of the obtained silver powder is 1.8 μm, and the tap density is 6.32 g / cm 3 , with a specific surface area of 0.62m 2 / g. The melting point is 366°C, as shown in Table 1 and Figure 3 In addition, the silver powder obtained under the preparation conditions has a dense structure inside, and its internal microstructure is as follows Figure 4 shown.
[0081] Compared with Example 1 and Comparative Examples 1-2, in Comparative Example 3, after not adding the high-polarity surfactant component, the high-activity silver powder obtained has the highest melting point, especially compared with Example 1, the melting point of the silver powder increases by nearly 70°C, which shows that adding a high-polarity surfactant during the preparation process can effectively reduce the melting point of the silver powder and improve its sintering activity.
[0082] Table 1 Content of each component and melting point of silver powder
[0083]
[0084] The present disclosure proposes a high-activity silver powder and a preparation method thereof, which has the following beneficial effects compared to the prior art: the preparation method of the present disclosure is simple, and through the synergistic effect of a high-activity surfactant and other components, the morphology of the spherical silver powder can be adjusted during the preparation of the silver powder, so that holes are formed inside the spherical silver powder, and the prepared silver powder has a lower melting point and higher sintering activity, and is also conducive to making the electronic paste using the high-activity silver powder have good dispersibility and printability. When the high-activity silver powder is applied to solar cell silver paste, the sintering performance of the silver paste can also be improved, which helps to achieve a higher solar cell photoelectric conversion efficiency. In addition, the low melting point characteristics of the high-activity silver powder can also contribute to its application in low-temperature silver paste.
[0085] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.
Claims
1. A method for preparing highly active silver powder, characterized in that: The preparation method comprises: S110, adding a silver-containing compound and a high-polarity surfactant to a solvent, stirring evenly, to obtain a solution A; the high-polarity surfactant is a copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide; wherein the content of the silver-containing compound is 80-160 parts by mass; the content of the high-polarity surfactant is 40-100 parts by mass; and the content of the solvent is 1000-2500 parts by mass; S120, adding a reducing agent and a dispersing agent to the solvent, stirring evenly, to obtain a solution B; wherein the content of the reducing agent is 50-120 parts by mass; the content of the dispersing agent is 20-40 parts by mass; and the content of the solvent is 1000-2500 parts by mass; S130, injecting the solution A and the solution B into the reaction container at a rate of 50-1000 mL / min respectively, reacting at 20-40° C. to obtain a reaction solution; S140, centrifuging the reaction solution at least once, removing the upper layer of the solution, and drying to obtain a high-activity silver powder having pores inside.
2. The method for preparing a highly active silver powder according to claim 1, characterized in that: The silver-containing compound is at least one of silver nitrate and silver trifluoroacetate.
3. The method for preparing a highly active silver powder according to claim 1, characterized in that: The molecular weight of the copolymer is 10000-30000, and the molecular weight distribution is 1.2-2.
5.
4. The method for preparing a highly active silver powder according to claim 1, characterized in that: The highly polar surfactant is prepared by the following method: The histamine acrylamide monomer, 2-hydroxypropyl methacrylamide monomer, chain transfer agent, thermal initiator, methanol and deionized water are uniformly mixed, and free radical polymerization is carried out at 80-90° C. for 5-7 hours to obtain a copolymer solution of histamine acrylamide and 2-hydroxypropyl methacrylamide; The copolymer solution is diluted, settled, filtered and dried to obtain a copolymer of histamine acrylamide and 2-hydroxypropyl methacrylamide.
5. The method for preparing a highly active silver powder according to claim 1, characterized in that: The reducing agent is at least one of formaldehyde, sodium borohydride, hydrazine hydrate, ascorbic acid, sodium ascorbate and glucose.
6. The method for preparing a highly active silver powder according to claim 1, characterized in that: The dispersant is at least one of gelatin, gum arabic, polyvinyl pyrrolidone, sodium citrate and polyvinyl alcohol.
7. The method for preparing a highly active silver powder according to claim 1, characterized in that: The solution A and the solution B are injected into the reaction container at a constant speed and reacted for 8-12 minutes; wherein the constant speed is 50-1000 mL / min.
8. A high-activity silver powder prepared by the method for preparing a high-activity silver powder according to any one of claims 1 to 7, characterized in that: The high-activity silver powder has a pore structure inside; the high-activity silver powder has an average particle size of 0.5 to 2.0 μm and a tap density of 5.0 to 6.5 g / cm 3 , with a specific surface area of 0.5 to 1.2 m 2 / g.