Laser welding method, welding wire and preparation process of aluminum-silicon coated steel plate
By accurately controlling the composition and welding process of aluminum-plated silicon steel plate welding, the problem of difficult control of the quality of welding joints in laser welding of aluminum-plated silicon steel plates is solved, and the uniformity and stability of the welds are improved, meeting the mechanical performance requirements of industrial applications.
Patent Information
- Application Number
- CN202410964848.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-18
AI Technical Summary
During the laser welding process of aluminum-plated silicon steel plates, the quality of the weld joints is difficult to control. Traditional methods such as arc welding and resistance welding cause the metallographic structure of the weld and the mechanical properties are degraded. In addition, existing laser welding methods such as laser ablation and mechanical grinding The cutting efficiency is low and the cost is high, making it difficult to apply in large-scale industrial production.
By accurately controlling the proportion of elements in the welding wire components, laser wire fill welding method is adopted. The welding wire components include C, Si, Mn, Ni, Cu, B, P and other elements, combining rapid cooling, hot forging and hot extrusion processes to form fines To improve the grain structure and optimize the structure and performance of the weld.
It improves the uniformity and stability of the weld seam, enhances the tensile strength and elongation of the welded joints, improves welding performance, meets industrial application needs, and reduces production costs.
Smart Images

Figure CN118492629B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of welding technology, and in particular to a laser welding method for aluminum-silicon coated steel plates, welding wire and a preparation process. Background Art
[0002] In recent years, with the rapid development of manufacturing and industrial automation, laser welding technology has gradually become an efficient and precise connection method, which is widely used in automobile manufacturing, aerospace, electronic equipment and other fields. Among them, aluminum-silicon steel plates are increasingly being adopted due to their good corrosion resistance and high strength. However, in the laser welding process of aluminum-silicon steel plates, the quality of welded joints has always been a difficult problem to be solved. Traditional welding methods, such as arc welding and resistance welding, often lead to coarse weld metallographic structure and decreased mechanical properties of welded joints due to large heat input and wide welding heat affected zone. Laser welding has the advantages of high energy density, small heat affected zone and fast welding speed, which can overcome the defects of traditional welding methods to a certain extent. However, since the aluminum and silicon elements in the aluminum-silicon layer will melt and mix into the weld during the welding process, ferrite will be formed, resulting in the deterioration of weld structure and welded joint performance. Therefore, how to effectively control the weld quality of laser welding of aluminum-silicon steel plates has become the difficulty and focus of current research.
[0003] The existing technology has conducted a lot of research on laser welding of aluminum-silicon coated steel plates, mainly focusing on: removing the coating by methods such as laser ablation and mechanical grinding to eliminate the negative impact of the coating on the weld structure. For example: Chinese patent CN101426612A discloses a method for manufacturing a welding blank containing only intermetallic compounds as a pre-coating layer using aluminum-silicon coated steel plates as raw materials. Specifically, the aluminum alloy layer in the coating is removed by mechanical methods to prevent excessive aluminum from melting into the molten pool; the intermetallic compound layer in the coating is retained. Then the welding blank is welded and hot stamped; Chinese patent CN106334875A discloses a steel welding component with aluminum or aluminum alloy coating, which adopts a steel welding blank with aluminum or aluminum alloy coating, which is composed of a steel substrate and a coating, and the coating includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the coating of the to-be-welded area on at least one plated surface of the steel welding blank is removed by laser ablation or mechanical stripping, thereby ensuring the tensile strength, elongation and corrosion resistance of the welded joint after hot stamping. Laser ablation directly removes the aluminum-silicon layer through a high-energy laser beam to reduce the negative impact of aluminum on the weld structure. However, laser ablation equipment is expensive and complicated to operate, and it is easy to cause damage to the substrate, affecting the welding quality. In addition, the laser ablation process requires precise control of the laser power and scanning speed, otherwise it may lead to uneven removal of the coating, affecting the consistency of the welded joint; mechanical grinding removes the aluminum-silicon layer through physical contact, but this method is inefficient and easily causes scratches on the substrate surface, affecting the welding quality. In addition, the mechanical grinding process is cumbersome and difficult to apply in large-scale industrial production. It also reduces production efficiency and increases production costs.
[0004] Chinese patent CN111215751B discloses a steel differential welding component with aluminum or aluminum alloy coating and a manufacturing method thereof, wherein the composition weight percentage of the welding wire is: C0.1-0.25%, Si0.2-0.4%, Mn1.2-2%, P≤0.03%, S≤0.006%, Al<0.06%, Ti0.02-0.08%, Cr0.05-0.2%, and the balance is Fe and unavoidable impurities; the welding wire diameter is 0.8-1.4mm; the steel plate includes a substrate and at least one pure aluminum or aluminum alloy on its surface Gold plating, which includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the patent optimizes the composition in the welding wire, avoids the surface treatment of the welded parts by laser ablation and mechanical grinding, and is beneficial to prevent the weld from producing iron-aluminum intermetallic compounds and high-temperature ferrite phases, and ultimately ensures that the joint performance meets the requirements of the automotive industry. However, although the content of aluminum and chromium in the welding wire composition in this patent is optimized, under certain heat treatment conditions, a small amount of aluminum and chromium may be enriched at the grain boundaries to form brittle phases or intermetallic compounds, thereby affecting the performance of the welded parts.
[0005] This application proposes a method for solving the weld quality problem during laser welding of aluminum-silicon coated steel plates by designing the welding wire composition. By precisely controlling the proportion of each element in the welding wire composition, the influence of aluminum and other harmful elements on the weld structure can be effectively reduced during the welding process, thereby improving the uniformity and stability of the weld. Summary of the invention
[0006] The present application provides a welding wire for laser welding of aluminum-silicon-coated steel plates, wherein the welding wire components are as follows by weight: C 0.20-0.45%, Si 0.20-0.40%, Mn 2.0-5.0%, Ni 1.0-10.0%, Cu 0.5-5.0%, B 0.003-0.005%, P≤0.015%, S≤0.010%, and the balance is Fe and other unavoidable impurities;
[0007] As a preferred technical solution for a laser welding method of aluminum-silicon-coated steel plates, the welding wire has the following components in weight percentage: C 0.23%, Si 0.30%, Mn 3.5%, Ni 6.0%, Cu 3.0%, Mg 0.80, B 0.003%, P≤0.015%, S≤0.010%, and the remainder is Fe and other unavoidable impurities.
[0008] A preparation process of welding wire comprises the following steps:
[0009] S1.According to the designed composition ratio, accurately weigh the Si block, C block, Fe-Mn alloy block, Ni-Fe alloy block, Fe-Cu alloy block and Fe block;
[0010] S2. Place the weighed raw materials in a vacuum induction melting furnace and heat to 1550-1600°C to completely melt all the elements;
[0011] S3. Casting the molten metal into an ingot through a casting process, using a rapid cooling process to refine the grain structure, and after the ingot is cooled, performing a preliminary annealing treatment at 850-900° C. for 2-4 hours to eliminate internal stress and improve the ductility of the material; wherein the rapid cooling includes water cooling and / or oil cooling;
[0012] S4. The annealed ingot is hot forged and hot extruded to form a round bar or a square bar to ensure the density and uniformity of the material, and the extruded bar is subjected to secondary heat treatment;
[0013] S5. The heat-treated rod is initially cold-drawn to be drawn into a thicker wire rod, and then subjected to medium-temperature annealing to eliminate stress during the drawing process and improve the ductility of the welding wire. After multiple cold-drawing and intermediate annealing processes, the wire rod is gradually drawn into a welding wire of the required diameter. The diameter after each cold-drawing is reduced by no more than 20% to prevent material embrittlement. After drawing to the final diameter, the welding wire is subjected to low-temperature annealing to improve the plasticity and consistency of the welding wire; wherein the required diameter is 0.5 to 1.8 mm, and the temperature of the low-temperature annealing is 300 to 350°C;
[0014] S6. Use dilute acid solution to pickle the welding wire to remove surface oxides and impurities, use alkaline solution to neutralize the pickled welding wire, and thoroughly rinse it with pure water. According to specific application requirements, the surface of the welding wire is treated with anti-oxidation coating. Common methods include copper plating or nickel plating to enhance the corrosion resistance of the welding wire.
[0015] As a preferred technical solution for the preparation process of a welding wire, the secondary heat treatment comprises the following steps: keeping warm at 1050-1100°C for 2-4 hours, performing aging treatment at 450-500°C, and keeping warm for 4-6 hours.
[0016] As a preferred technical solution for a welding wire preparation process, in step S3, the rapid cooling includes water cooling and / or oil cooling.
[0017] As a preferred technical solution for the preparation process of a welding wire, in step S5, the temperature of the medium-temperature annealing treatment is 600-650°C, the required diameter is 0.5 to 1.8 mm, and the temperature of the low-temperature annealing treatment is 300 to 350°C.
[0018] A laser welding method for aluminum-silicon coated steel plates comprises the following steps:
[0019] S1. Preparation before welding of steel plates: The steel plates to be welded are flat steel plates, the steel plates to be welded include a substrate and at least one coating on its surface, the coating includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the coating of the welding area of the steel plates to be welded is not removed or thinned;
[0020] S2. Preset butt gap: Preset the butt gap between the two steel plates to be welded to 0.1 to 0.5 mm;
[0021] S3. Welding: The laser wire-filling welding process is used for welding. The welding gun and the wire-feeding mechanism are located above the steel plate to be welded. The welding gun and the wire-feeding mechanism are fed simultaneously to ensure the normal operation of the wire feeding system. The welding gun angle is adjusted so that the welding wire forms an inclination angle of 30° to 60° with the welding direction. The welding wire is moved 1 to 3 mm to one side from the arc center to form a misalignment between the welding wire and the arc. Among them, the laser wire-filling welding process uses a laser spot diameter of 0.8 to 2.0 mm, a defocus of -1 to 1 mm, a laser power controlled at 4 to 6 kW, and a welding speed controlled at 40 to 140 mm / s; the wire feeding speed is 2 to 8 m / min; the shielding gas is a shielding gas containing active gas;
[0022] As a preferred technical solution for the laser welding method of aluminum-silicon coated steel plates, the shielding gas is pure Ar, pure He or a combination of Ar+CO2.
[0023] As a preferred technical solution for the laser welding method of aluminum-silicon coated steel plates, the butt gap is in the shape of a convex letter, and the angle between the two sides of the convex letter is α, 30°≤α≤50°. A boss-shaped weld usually indicates that the weld joint is wider at the top, which helps to distribute stress more evenly. Under stress, the wider top can reduce stress concentration and reduce the risk of weld cracking due to excessive local stress. In addition, this shape helps to reduce defects that may occur during the welding process, such as pores, inclusions, and incomplete penetration. These defects can significantly weaken the tensile strength and elongation of the weld. The heat input during welding and the subsequent cooling rate have a significant impact on the microstructure of the weld metal. A boss-shaped weld usually means that there is more sufficient heat input and a slower cooling rate during the welding process, which helps to form The fine grains can enhance the mechanical properties of the metal, including tensile strength and plastic elongation. Boss-shaped welds can usually achieve better welding penetration and joint interface. When the weld and the base material are more tightly bonded, the overall strength and ductility of the weld joint are improved. This good combination not only provides a larger contact area, but also helps to reduce micro defects at the interface, such as incomplete penetration or inclusions. When the angle α is in the range of 30° to 50°, the optimal microstructure and stress distribution of the weld metal and the heat-affected zone can usually be achieved, thereby improving the tensile strength and elongation of the weld joint.
[0024] Beneficial effects of the present invention:
[0025] 1. Silicon is a deoxidizing element in welding wire, which can prevent iron from combining with oxygen and can reduce iron oxide in the molten pool; however, if silicon is used alone for deoxidation, the resulting silicon dioxide has a high melting point (about 1710°C), and the oxide particles are fine and difficult to float out of the molten pool, which can easily cause slag inclusions in the weld. Therefore, the weight percentage of silicon in this welding wire is controlled within the range of 0.20-0.40%.
[0026] 2. Manganese is an important hardenability element, which has a great influence on the toughness of the weld. It is also a deoxidizing element, but its deoxidizing ability is slightly worse than that of silicon. When deoxidized with manganese alone, the density of manganese oxide generated is relatively large, and it is not easy to float out of the molten pool. Therefore, this welding wire adopts silicon-manganese combined deoxidation, so that the deoxidation product is a composite silicate (MnO.SiO2), which has a low melting point (about 1270℃) and a small density. It can condense into a large piece of slag in the molten pool, which is conducive to floating and achieving a good deoxidation effect; manganese also has a desulfurization function, and combines with sulfur to form manganese sulfide, which can reduce the tendency of thermal cracking caused by sulfur; manganese forms carbides (such as Mn3C) with carbon, and these carbides are distributed in the matrix of steel, which significantly improves the strength and hardness of the material. Taking various factors into consideration, the weight percentage of manganese in this welding wire is controlled between 2.0 and 5.0%.
[0027] 3. Boron (B) Although the amount added to the alloy is usually very small, boron can segregate at the grain boundary, fill the vacancies or defects at the grain boundary, thereby enhancing the bonding force of the grain boundary. This strengthening effect can improve the material's crack resistance and creep resistance. Due to the effect of boron, the material's plastic deformation ability at high temperature is improved, the hot working performance is enhanced, and the tendency of cracks generated during hot working is reduced; when the boron content exceeds 0.005%, excessive boron will form borides at the grain boundary. These borides are brittle and will weaken the toughness of the grain boundary, making the grain boundary brittle, which will cause the material to easily break under stress. Excessive boron will form complex second phases with other elements (such as iron, chromium, etc.). These second phases are generally hard and brittle compounds that will reduce the overall toughness and impact resistance of the material. Therefore, the weight percentage of B in this welding wire is controlled between 0.003 and 0.005%;
[0028] 4. Nickel, as an important alloying element of welding wire, plays a key role in the performance of welding joints and the stability of welding process. Nickel is an austenite stabilizing element, which can stabilize and maintain the austenite phase in the weld. The austenite phase has high plasticity and toughness, so that the weld can still maintain good mechanical properties at low temperature and prevent brittle fracture. Nickel can refine the grain structure of the iron matrix. The fine grain structure has higher strength and toughness than the coarse grain, which significantly improves the mechanical properties of the material. In addition, the combination of nickel and iron can form a stable passivation film, which can effectively prevent the corrosion of corrosive media (such as oxygen, moisture, acid, alkali, chloride ions, etc.) on the base metal and significantly improve the corrosion resistance of the material; therefore, the weight percentage of Ni in this welding wire is controlled between 1.0 and 10.0%;
[0029] 5. Copper, as an important component of welding materials, has a significant impact on the welding process and the performance of the welded joint. The addition of copper can improve the toughness and ductility of the weld, reduce the crack tendency during welding, and maintain good mechanical properties, especially in low temperature environments. The weight percentage of Ni in this welding wire is controlled between 0.5 and 5.0%;
[0030] 6. The synergistic effect of Mn, Ni and Cu in the welding wire mainly improves the comprehensive performance of the weld by stabilizing the austenite phase, refining the grain structure, and achieving solid solution strengthening and precipitation strengthening. The austenite stabilization effect of Mn and Ni ensures that the phase change behavior during welding is suppressed, and the precipitation phase and solid solution of Cu enhance the strength and hardness of the weld. Through these phase changes, the weld exhibits excellent performance during laser welding and meets the needs of various industrial applications.
[0031] 7. Sulfur easily forms iron sulfide in the molten pool and is distributed in a network at the grain boundaries, which significantly reduces the toughness of the weld and causes hot brittleness of the steel. Therefore, sulfur in welding wire is harmful and its content must be strictly controlled.
[0032] 8. Phosphorus is second only to carbon in strengthening steel, increasing the strength and hardness of steel. Phosphorus can improve the corrosion resistance of steel, but significantly reduce its plasticity and toughness, especially at low temperatures, which will cause cold brittleness of steel. Therefore, phosphorus in welding wire is harmful and its content must be strictly controlled.
[0033] 9. When the welding wire forms an inclination angle of 30° to 60° with the welding direction, the melting of the welding wire and the stirring effect of the molten pool are enhanced. The inclination angle increases the contact area between the welding wire and the molten pool, promotes the flow and mixing of the metal, and makes the weld metal more uniform. The convection and stirring effect of the molten pool are enhanced, which helps to reduce component segregation and improve the uniformity and consistency of the weld, thereby improving the tensile strength and elongation; moving the welding wire 1 to 3 mm to one side from the center of the arc helps to form a wider molten pool and improve the weld formation. Such an operation can effectively avoid the generation of unfused and porosity defects in the weld. Appropriate dislocation makes it easier for bubbles in the molten pool to escape, reducing the generation of pores, thereby improving the density and strength of the weld;
[0034] 10. Appropriate tilt angle and staggered operation can disperse the thermal stress and residual stress generated during welding. The uniform distribution of thermal stress and residual stress helps to reduce the stress concentration points of the weld and prevent the occurrence of cracks and fractures. This can improve the toughness and elongation of the weld and enhance the overall performance of the welded joint. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a schematic diagram of the device of the welding process in this application scheme;
[0036] Figure 2 This is a microscopic metallographic structure diagram of the weld prepared in Comparative Example 1;
[0037] Figure 3 is a microscopic metallographic structure diagram of the weld prepared in Example 1;
[0038] Figure 4 It is the experimental data diagram of Example 4;
[0039] Figure 5 It is the experimental data diagram of Example 5;
[0040] Figure 6 is a structural schematic diagram of the weld;
[0041] Figure 7 It is the experimental data diagram of Example 6;
[0042] Figure numerals: 1. workbench; 2. steel plate; 3. fixture; 4. laser source; 5. welding wire; 6. welding seam. DETAILED DESCRIPTION
[0043] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0044] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0045] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0046] It should be noted that the steel plate to be welded in this application is 22MnB5, and its chemical composition is as shown in Table 1:
[0047] Table 1 shows the composition of the steel plates to be welded
[0048]
[0049] In addition, if Figure 1 As shown, the inclination angle formed by the welding wire and the welding direction in the present application is the angle between the straight line formed by the welding wire and the straight line formed by the weld between the two steel plates;
[0050] Please refer to Figure 6As shown, the cross-section of the weld after welding is convex (trapezoidal), and the distance of the butt gap is H. By machining one side of the steel plate to be welded, a weld with an angle of α can be formed, which has been specifically marked in the figure.
[0051] Example 1
[0052] Embodiment 1 provides a laser welding method for aluminum-silicon coated steel plates, welding wire and preparation process, wherein:
[0053] The welding wire components are as follows by weight: C 0.23%, Si 0.30%, Mn 3.5%, Ni 6.0%, Cu 3.0%, B0.003%, P≤0.015%, S≤0.010%, and the balance is Fe and other inevitable impurities.
[0054] Preparation process of welding wire: according to the designed composition ratio, accurately weigh Si block, Fe-C block, Fe-Mn alloy block, Fe-B alloy block, Ni-Fe alloy block, Fe-Cu alloy block and Fe block;
[0055] The weighed raw materials are placed in a vacuum induction melting furnace and heated to 1600°C to completely melt all the elements;
[0056] The molten metal is cast into an ingot through a casting process, and a rapid cooling process is adopted. After the ingot is cooled, a preliminary annealing treatment is performed, and the temperature is kept at 900°C for 4 hours;
[0057] The annealed ingot is hot forged and hot extruded to form round or square bars to ensure the density and uniformity of the material, and the extruded bars are subjected to secondary heat treatment;
[0058] The heat-treated rods are initially cold-drawn to be drawn into thicker wire rods, and then medium-temperature annealing is performed at 600°C to eliminate stress during the drawing process and improve the ductility of the welding wire. After multiple cold-drawing and medium-temperature annealing processes, the welding wire is gradually drawn into a welding wire with a diameter of 0.8 mm. The diameter after each cold drawing is reduced by no more than 20% to prevent material embrittlement. After drawing to the final diameter, the welding wire is subjected to low-temperature annealing at 350°C to improve the plasticity, toughness and consistency of the welding wire.
[0059] Use dilute acid solution to pickle the welding wire to remove surface oxides and impurities, use alkaline solution to neutralize the pickled welding wire, and thoroughly wash it with pure water. According to specific application requirements, copper is plated on the surface of the welding wire to enhance the corrosion resistance of the welding wire;
[0060] Welding method:
[0061] Preparation before welding of steel plates: The steel plates to be welded are flat steel plates, the steel plates to be welded include a substrate and at least one coating on its surface, the coating includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the coating of the welding area of the steel plates to be welded is not removed or thinned;
[0062] Preset butt gap: The butt gap between the two steel plates to be welded is preset to 0.3 mm. The butt gap is in a convex shape with an angle α of 30°.
[0063] Welding: According to Figure 1 As shown, the laser wire-filling welding process is used for welding. The welding gun and the wire-feeding mechanism are located above the steel plate to be welded. The welding gun and the wire-feeding mechanism are fed simultaneously to ensure the normal operation of the wire feeding system. The welding gun angle is adjusted so that the welding wire forms an inclined angle of 30° with the welding direction. The welding wire is moved 2mm to one side from the center of the arc to form a misalignment between the welding wire and the arc. Among them, the laser wire-filling welding process uses a laser spot diameter of 0.8mm, a defocus amount of 1mm, a laser power controlled at 6kW, and a welding speed controlled at 100mm / s; the wire feeding speed is 5m / min; the shielding gas is a shielding gas containing an active gas, the active gas is CO2, the volume percentage of Ar gas is 80%, and the rest is CO2.
[0064] Example 2
[0065] Embodiment 2 provides a laser welding method, welding wire and preparation process of aluminum-silicon coated steel plates, wherein:
[0066] The welding wire components are as follows by weight: C 0.20%, Si 0.40%, Mn 2.0%, Ni 9.0%, Cu 5.0%, B 0.005%, P ≤ 0.015%, S ≤ 0.010%, and the balance is Fe and other unavoidable impurities.
[0067] Preparation process of welding wire: accurately weigh Si block, Fe-C block, Fe-Mn alloy block, Fe-B alloy block, Ni-Fe alloy block, Fe-Cu alloy block and Fe block;
[0068] The weighed raw materials are placed in a vacuum induction melting furnace and heated to 1550°C to completely melt all elements;
[0069] The molten metal is cast into an ingot through a casting process, and a rapid cooling process is adopted. After the ingot is cooled, a preliminary annealing treatment is performed, and the temperature is kept at 900°C for 4 hours;
[0070] The annealed ingot is hot forged and hot extruded to form round or square bars to ensure the density and uniformity of the material, and the extruded bars are subjected to secondary heat treatment;
[0071] The heat-treated rods are initially cold-drawn to be drawn into thicker wire rods, and then medium-temperature annealing is performed at 650°C to eliminate stress during the drawing process and improve the ductility of the welding wire. After multiple cold-drawing and medium-temperature annealing processes, the welding wire is gradually drawn into a welding wire with a diameter of 1.8 mm. The diameter after each cold drawing is reduced by no more than 20% to prevent the material from becoming brittle. After being drawn to the final diameter, the welding wire is subjected to a low-temperature annealing treatment at 300°C to improve the plasticity, toughness and consistency of the welding wire.
[0072] Use dilute acid solution to pickle the welding wire to remove surface oxides and impurities, use alkaline solution to neutralize the pickled welding wire, and thoroughly wash it with pure water. According to specific application requirements, copper is plated on the surface of the welding wire to enhance the corrosion resistance of the welding wire;
[0073] Welding method:
[0074] Preparation before welding of steel plates: The steel plates to be welded are flat steel plates, the steel plates to be welded include a substrate and at least one coating on its surface, the coating includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the coating of the welding area of the steel plates to be welded is not removed or thinned;
[0075] Preset butt gap: The butt gap between the two steel plates to be welded is preset to 0.5 mm. The butt gap is in a convex shape with an angle α of 30°.
[0076] Welding: According to Figure 1 As shown, laser wire-filling welding is used for welding. The welding gun and wire-feeding mechanism are located above the steel plate to be welded. The welding gun and wire-feeding mechanism are fed simultaneously to ensure the normal operation of the wire feeding system. The welding gun angle is adjusted so that the welding wire forms a 45° inclination angle with the welding direction. The welding wire is moved 2mm to one side from the arc center to form a misalignment between the welding wire and the arc. Among them, the laser wire-filling welding process uses a laser spot diameter of 0.8mm, a defocus amount of 1mm, a laser power controlled at 6kW, and a welding speed controlled at 100mm / s; the wire feeding speed is 5m / min; and the shielding gas is pure Ar gas.
[0077] Example 3
[0078] Embodiment 3 provides a laser welding method for aluminum-silicon coated steel plates, welding wire and preparation process, wherein:
[0079] The welding wire components are as follows by weight: C 0.45%, Si 0.20%, Mn 5.0%, Ni 10.0%, Cu 0.5%, B 0.003%, P ≤ 0.015%, S ≤ 0.010%, and the balance is Fe and other inevitable impurities.
[0080] Preparation process of welding wire: according to the designed composition ratio, accurately weigh Si block, Fe-C block, Fe-Mn alloy block, Fe-B alloy block, Ni-Fe alloy block, Fe-Cu alloy block and Fe block;
[0081] The weighed raw materials are placed in a vacuum induction melting furnace and heated to 1600°C to completely melt all the elements;
[0082] The molten metal is cast into an ingot through a casting process, and a rapid cooling process is adopted. After the ingot is cooled, a preliminary annealing treatment is carried out, and the ingot is kept at 850°C for 4 hours to eliminate internal stress and improve the ductility of the material;
[0083] The annealed ingot is hot forged and hot extruded to form round or square bars to ensure the density and uniformity of the material, and the extruded bars are subjected to secondary heat treatment;
[0084] The heat-treated rods are initially cold-drawn to be drawn into thicker wire rods, and then medium-temperature annealing is performed at 600°C to eliminate the stress in the drawing process and improve the ductility of the welding wire. After multiple cold-drawing and medium-temperature annealing processes, the welding wire is gradually drawn into a welding wire with a diameter of 1.2 mm. The diameter after each cold drawing is reduced by no more than 20% to prevent the material from becoming brittle. After being drawn to the final diameter, the welding wire is subjected to a low-temperature annealing treatment at 350°C to improve the plasticity, toughness and consistency of the welding wire.
[0085] Use dilute acid solution to pickle the welding wire to remove surface oxides and impurities, use alkaline solution to neutralize the pickled welding wire, and thoroughly wash it with pure water. According to specific application requirements, nickel-plated the surface of the welding wire to enhance the corrosion resistance of the welding wire;
[0086] Welding method:
[0087] Preparation before welding of steel plates: The steel plates to be welded are flat steel plates, the steel plates to be welded include a substrate and at least one coating on its surface, the coating includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the coating of the welding area of the steel plates to be welded is not removed or thinned;
[0088] Preset butt gap: The butt gap between the two steel plates to be welded is preset to 0.3 mm, the butt gap is in a convex shape, and the angle α is 50°;
[0089] Welding: According to Figure 1As shown, the laser wire-filling welding process is used for welding. The welding gun and the wire-feeding mechanism are located above the steel plate to be welded. The welding gun and the wire-feeding mechanism are fed simultaneously to ensure the normal operation of the wire feeding system. The welding gun angle is adjusted so that the welding wire forms an inclined angle of 60° with the welding direction. The welding wire is moved 2mm to one side from the center of the arc to form a misalignment between the welding wire and the arc. Among them, the laser wire-filling welding process uses a laser spot diameter of 0.8mm, a defocus amount of 1mm, a laser power controlled at 6kW, and a welding speed controlled at 100mm / s; the wire feeding speed is 5m / min; the shielding gas is a shielding gas containing an active gas, the active gas is CO2, the volume percentage of Ar gas is 80%, and the rest is CO2.
[0090] Comparative Example 1
[0091] The welding wire composition used in this comparative example is the same as that in the embodiment, and the weight percentage of the welding wire composition is: C 0.23%, Si 0.30%, Mn 3.5%, Ni 6.0%, Cu 3.0%, B 0.003%, P≤0.015%, S≤0.010%, and the balance is Fe and other inevitable impurities.
[0092] The preparation process is the same as that in Example 1 and will not be described again here.
[0093] The difference between the welding process of this comparative example and that of Example 1 is that this comparative example does not use the filling wire process for welding, but directly uses two steel plates for laser welding. The specific laser welding process is the same as that of Example 1. The welding gun and the wire feeding mechanism are located above the steel plates to be welded. The welding gun and the wire feeding mechanism are fed simultaneously to ensure the normal operation of the wire feeding system. The welding gun angle is adjusted so that the welding wire forms an inclination angle of 30° with the welding direction, and the welding wire is moved 2mm to one side from the center of the arc to form a misalignment between the welding wire and the arc. Among them, the laser filling wire welding process uses a laser spot diameter of 0.8mm, a defocus amount of 1mm, a laser power controlled at 6kW, and a welding speed controlled at 100mm / s; the wire feeding speed is 5m / min; the shielding gas is a shielding gas containing an active gas, the active gas is CO2, the volume percentage of Ar gas is 80%, and the rest is CO2.
[0094] Comparative Example 2
[0095] The difference between this comparative example and Example 1 is that in this comparative example, only Mn element is contained among the three elements of Mn, Ni and Cu, and the specific composition contents thereof are shown in Table 2 below.
[0096] Comparative Example 3
[0097] The difference between this comparative example and Example 1 is that in this comparative example, only Ni element is contained among the three elements of Mn, Ni and Cu, and the specific composition contents thereof are shown in Table 2 below.
[0098] Comparative Example 4
[0099] The difference between this comparative example and Example 1 is that only Cu element is contained among the three elements of Mn, Ni and Cu, and the specific composition contents thereof are shown in Table 2 below.
[0100] Comparative Example 5
[0101] The difference between this comparative example and Example 1 is that only Mn and Ni elements are contained among the three elements of Mn, Ni and Cu, and their specific component contents are shown in Table 2 below.
[0102] Comparative Example 6
[0103] The difference between this comparative example and Example 1 is that only Mn and Cu elements are contained among the three elements of Mn, Ni and Cu, and their specific component contents are shown in Table 2 below.
[0104] Comparative Example 7
[0105] The difference between this comparative example and Example 1 is that only Ni and Cu elements are contained among the three elements of Mn, Ni and Cu, and their specific component contents are shown in Table 2 below.
[0106] Comparative Example 8
[0107] The difference between this comparative example and implementation 1 is that the butt gap between the steel plates to be welded is in a square structure.
[0108] Example 4
[0109] Embodiment 4 provides a laser welding method, welding wire and preparation process of aluminum-silicon coated steel plates, wherein:
[0110] The welding wire components are as follows by weight: C 0.21%, Si 0.30%, Mn 5.0%, Ni 1.0%, Cu 2.5%, B0.004%, P≤0.015%, S≤0.010%, and the balance is Fe and other inevitable impurities.
[0111] Preparation process of welding wire: according to the designed composition ratio, accurately weigh Si block, Fe-C block, Fe-Mn alloy block, Fe-B alloy block, Ni-Fe alloy block, Fe-Cu alloy block and Fe block;
[0112] The weighed raw materials are placed in a vacuum induction melting furnace and heated to 1550°C to completely melt all elements;
[0113] The molten metal is cast into an ingot through a casting process, and a rapid water cooling process is used to refine the grain structure. After the ingot is cooled, a preliminary annealing treatment is carried out at 900°C for 4 hours to eliminate internal stress and improve the ductility of the material;
[0114] The annealed ingot is hot forged and hot extruded to form round or square bars to ensure the density and uniformity of the material, and the extruded bars are subjected to secondary heat treatment;
[0115] The heat-treated rods are initially cold-drawn to be drawn into thicker wire rods, and then medium-temperature annealing is performed at 600°C to eliminate stress during the drawing process and improve the ductility of the welding wire. After multiple cold-drawing and medium-temperature annealing processes, the welding wire is gradually drawn into a welding wire with a diameter of 0.8 mm. The diameter after each cold drawing is reduced by no more than 20% to prevent material embrittlement. After drawing to the final diameter, the welding wire is subjected to low-temperature annealing at 350°C to improve the plasticity, toughness and consistency of the welding wire.
[0116] Use dilute acid solution to pickle the welding wire to remove surface oxides and impurities, use alkaline solution to neutralize the pickled welding wire, and thoroughly wash it with pure water. According to specific application requirements, nickel-plated the surface of the welding wire to enhance the corrosion resistance of the welding wire;
[0117] Welding method:
[0118] Preparation before welding of steel plate: Figure 1 The steel plate to be welded is a straight steel plate, and the steel plate to be welded includes a substrate and at least one coating layer on its surface, and the coating layer includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the coating layer in the welding area of the steel plate to be welded is not removed or thinned;
[0119] Preset butt gap: The butt gap between the two steel plates to be welded is preset to 0.3 mm, the butt gap is in a convex shape, and the angle α is 40°;
[0120] Welding: Laser wire-filling welding is used for welding. The welding gun and wire-feeding mechanism are located above the steel plate to be welded. The welding gun and wire-feeding mechanism are fed simultaneously to ensure the normal operation of the wire feeding system. The welding gun angle is adjusted so that the welding wire forms an inclination angle of 0°, 15°, 30°, 45°, 60°, 75°, 90°, 105°, 120°, 135°, 150°, 165°, and 180° with the welding direction. The welding wire is moved 2mm to one side from the center of the arc to form a misalignment between the welding wire and the arc. Among them, the laser wire-filling welding process uses a laser spot diameter of 0.8mm, a defocus of 1mm, a laser power controlled at 6kW, and a welding speed controlled at 100mm / s; the wire feeding speed is 5m / min; the shielding gas is a shielding gas containing active gas, the volume percentage of the active gas is 80%, and the active gas is CO2.
[0121] Example 5
[0122] Embodiment 5 provides a laser welding method, welding wire and preparation process of aluminum-silicon coated steel plate, wherein:
[0123] The welding wire components are as follows by weight: C 0.21%, Si 0.30%, Mn 5.0%, Ni 1.0%, Cu 2.5%, B0.004%, P≤0.015%, S≤0.010%, and the balance is Fe and other inevitable impurities.
[0124] Preparation process of welding wire: according to the designed composition ratio, accurately weigh Si block, Fe-C block, Fe-Mn alloy block, Fe-B alloy block, Ni-Fe alloy block, Fe-Cu alloy block and Fe block;
[0125] The weighed raw materials are placed in a vacuum induction melting furnace and heated to 1550°C to completely melt all elements;
[0126] The molten metal is cast into an ingot through a casting process, and a rapid water cooling process is used to refine the grain structure. After the ingot is cooled, a preliminary annealing treatment is carried out at 900°C for 4 hours to eliminate internal stress and improve the ductility of the material;
[0127] The annealed ingot is hot forged and hot extruded to form round or square bars to ensure the density and uniformity of the material, and the extruded bars are subjected to secondary heat treatment;
[0128] The heat-treated rods are initially cold-drawn to be drawn into thicker wire rods, and then medium-temperature annealing is performed at 600°C to eliminate stress during the drawing process and improve the ductility of the welding wire. After multiple cold-drawing and medium-temperature annealing processes, the welding wire is gradually drawn into a welding wire with a diameter of 0.8 mm. The diameter after each cold drawing is reduced by no more than 20% to prevent material embrittlement. After drawing to the final diameter, the welding wire is subjected to low-temperature annealing at 350°C to improve the plasticity, toughness and consistency of the welding wire.
[0129] Use dilute acid solution to pickle the welding wire to remove surface oxides and impurities, use alkaline solution to neutralize the pickled welding wire, and thoroughly wash it with pure water. According to specific application requirements, nickel-plated the surface of the welding wire to enhance the corrosion resistance of the welding wire;
[0130] Welding method:
[0131] Preparation before welding of steel plate: Figure 1 The steel plate to be welded is a straight steel plate, and the steel plate to be welded includes a substrate and at least one coating layer on its surface, and the coating layer includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the coating layer in the welding area of the steel plate to be welded is not removed or thinned;
[0132] Preset butt gap: The butt gap between the two steel plates to be welded is preset to 0.3 mm, the butt gap is in a convex shape, and the angle α is 40°;
[0133] Welding: Laser wire-filling welding is used for welding. The welding gun and wire-feeding mechanism are located above the steel plate to be welded. The welding gun and wire-feeding mechanism are fed simultaneously to ensure the normal operation of the wire feeding system. The welding gun angle is adjusted to form a 30° inclination angle between the welding wire and the welding direction. The welding wire is moved to one side from the arc center by 0mm, 1mm, 2mm, 3mm, 4mm, 5mm, and 6mm to form a misalignment between the welding wire and the arc.
[0134] Among them, the laser wire welding process adopts a laser spot diameter of 0.8mm, a defocus amount of 1mm, a laser power controlled at 6kW, a welding speed controlled at 100mm / s; the wire feeding speed is 5m / min; the shielding gas is a shielding gas containing active gas, the volume percentage of the active gas is 80%, and the active gas is CO2.
[0135] Example 6
[0136] Embodiment 6 provides a laser welding method, welding wire and preparation process of aluminum-silicon coated steel plates, wherein:
[0137] The welding wire components are as follows by weight: C 0.22%, Si 0.30%, Mn 5.0%, Ni 6.0%, Cu 2.5%, B0.004%, P≤0.015%, S≤0.010%, and the balance is Fe and other inevitable impurities.
[0138] Preparation process of welding wire: according to the designed composition ratio, accurately weigh Si block, Fe-C block, Fe-Mn alloy block, Fe-B alloy block, Ni-Fe alloy block, Fe-Cu alloy block and Fe block;
[0139] The weighed raw materials are placed in a vacuum induction melting furnace and heated to 1550°C to completely melt all elements;
[0140] The molten metal is cast into an ingot through a casting process, and a rapid water cooling process is used to refine the grain structure. After the ingot is cooled, a preliminary annealing treatment is carried out at 900°C for 4 hours to eliminate internal stress and improve the ductility of the material;
[0141] The annealed ingot is hot forged and hot extruded to form round or square bars to ensure the density and uniformity of the material, and the extruded bars are subjected to secondary heat treatment;
[0142] The heat-treated rods are initially cold-drawn to be drawn into thicker wire rods, and then medium-temperature annealing is performed at 600°C to eliminate stress during the drawing process and improve the ductility of the welding wire. After multiple cold-drawing and medium-temperature annealing processes, the welding wire is gradually drawn into a welding wire with a diameter of 0.8 mm. The diameter after each cold drawing is reduced by no more than 20% to prevent material embrittlement. After drawing to the final diameter, the welding wire is subjected to low-temperature annealing at 350°C to improve the plasticity, toughness and consistency of the welding wire.
[0143] Use dilute acid solution to pickle the welding wire to remove surface oxides and impurities, use alkaline solution to neutralize the pickled welding wire, and thoroughly wash it with pure water. According to specific application requirements, nickel-plated the surface of the welding wire to enhance the corrosion resistance of the welding wire;
[0144] Welding method:
[0145] Preparation before welding of steel plate: Figure 1 The steel plate to be welded is a straight steel plate, and the steel plate to be welded includes a substrate and at least one coating layer on its surface, and the coating layer includes an intermetallic compound alloy layer in contact with the substrate and a metal alloy layer thereon; the coating layer in the welding area of the steel plate to be welded is not removed or thinned;
[0146] Preset butt gap: The butt gap of the two steel plates to be welded is preset to 0.3 mm, the butt gap is in a convex shape, and the angle α is 0°, 10°, 20°, 30°, 40°, 50°, 60°, 70°, 80°, 90°;
[0147] Welding: Laser wire-filling welding is used for welding. The welding gun and wire-feeding mechanism are located above the steel plate to be welded. The welding gun and wire-feeding mechanism are fed simultaneously to ensure the normal operation of the wire feeding system. The welding gun angle is adjusted so that the welding wire forms a 30° inclination angle with the welding direction. The welding wire moves 4mm to one side from the arc center to form a misalignment between the welding wire and the arc.
[0148] Among them, the laser wire welding process adopts a laser spot diameter of 0.8mm, a defocus amount of 1mm, a laser power controlled at 6kW, a welding speed controlled at 100mm / s; the wire feeding speed is 5m / min; the shielding gas is a shielding gas containing active gas, the volume percentage of the active gas is 80%, and the active gas is CO2.
[0149] Table 2: Ratio of welding wire components in Examples 1 to 4 and Comparative Examples 1 to 7
[0150]
[0151] Performance Testing
[0152] Test method for tensile strength and elongation of welded joints: Cut standard tensile specimens from welded parts, ensure that the size and shape of the specimens meet the requirements of relevant standards, the weld area of the specimens should be located in the middle of the tensile specimens, mark the standard gauge length (usually 50mm or 200mm) on the parallel sections of the specimens, install the specimens in the fixture of the universal testing machine, ensure that the specimens are centered, avoid eccentric loading, start the testing machine, and load the specimens at a constant tensile speed (usually 1-5 mm / min) until the specimens break.
[0153] Table 3 is the experimental data of the embodiments and comparative examples.
[0154]
[0155] Combined with Example 1, Comparative Example 1, Table 3 and Figure 2 , Figure 3 It can be seen that the tensile strength and joint elongation of the weld prepared in Example 1 are slightly greater than those of the weld prepared in Comparative Example 1, mainly because a small amount of aluminum and chromium in Comparative Example 1 may be enriched at the grain boundaries to form brittle phases or intermetallic compounds, thereby affecting the performance of the welded parts; on the other hand, Figure 2 and 3 It can be proved that the local area of the weld in Comparative Example 1 contains a small amount of ferrite, while no ferrite is found in the weld in Example 1. The small amount of ferrite affects the welding performance.
[0156] It can be seen from Example 1, Comparative Examples 2 to 7 and Table 3 that Mn, Ni and Cu can synergistically enhance the tensile strength and joint elongation of the weld. The synergistic effect of Mn and Ni can form uniform and fine austenite grains in the weld. This structure helps to withstand higher external forces without breaking, thereby improving the tensile strength and elongation. The addition of Cu further improves the strength of the weld through solid solution strengthening and precipitation hardening, and its good plasticity helps to increase the elongation.
[0157] Combined with Example 4 and Figure 4 It can be seen that when the inclination angle formed by the welding wire and the welding direction gradually increases, the tensile strength and joint elongation of the weld gradually increase. When the inclination angle exceeds about 60°, the tensile strength and joint elongation of the weld gradually decrease as the inclination angle gradually increases. If the inclination angle is too large or too small, the weld formation, molten pool stirring, metal mixing, stress distribution and other aspects will be adversely affected, which will lead to a decrease in the tensile strength and elongation of the weld and increase the risk of defects.
[0158] Combined with Example 5 and Figure 5It can be seen that moving the welding wire a suitable distance from the arc center to one side improves the tensile strength of the weld, mainly because this misalignment distance helps to form a wider molten pool and improves weld formation. Such an operation can effectively avoid the occurrence of unfusion and porosity defects in the weld. Appropriate misalignment makes it easier for bubbles in the molten pool to escape, reducing the generation of pores, thereby improving the density and strength of the weld.
[0159] Combining Example 1, Comparative Example 8 and Table 3, it can be seen that the tensile strength of the weld prepared in Example 1 is greater than that in Comparative Example 8, so it can be known that the shape of the weld has a certain influence on the tensile strength and elongation.
[0160] Combined with Example 6 and Figure 7 It can be seen that as the angle α increases, the tensile strength and elongation of the weld gradually increase. When the angle α reaches a certain value, the tensile strength and elongation of the weld reach a maximum value. When the angle α exceeds a certain value, the tensile strength and elongation of the weld gradually decrease.
[0161] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing welding wire for laser welding of aluminum-silicon coated steel plates, characterized in that: The composition weight percentage of the welding wire is: C 0.23%, Si 0.30%, Mn 3.5%, Ni 6.0%, Cu 3.0%, B0.003%, P≤0.015%, S≤0.010%, and the balance is Fe and other unavoidable impurities; The preparation process comprises the following steps: S1. According to the designed composition ratio, accurately weigh the Si block, Fe-C block, Fe-Mn alloy block, Fe-B alloy block, Ni-Fe alloy block, Fe-Cu alloy block and Fe block; S2. Place the weighed raw materials in a vacuum induction melting furnace and heat to 1550-1600°C to completely melt all the elements; S3. Casting the molten metal into an ingot through a casting process, using a rapid cooling process to refine the grain structure, and after the ingot is cooled, performing a preliminary annealing treatment at 850-900° C. for 2-4 hours; S4. The annealed ingot is hot forged and hot extruded to form a round bar or a square bar, and the extruded bar is subjected to a secondary heat treatment; S5. The heat-treated rod is initially cold-drawn to be drawn into a thicker wire rod, and then subjected to medium-temperature annealing. After multiple cold-drawing and intermediate annealing processes, the wire rod is gradually drawn into a welding wire of the required diameter. The diameter after each cold-drawing is reduced by no more than 20%. After being drawn to the final diameter, the welding wire is subjected to low-temperature annealing; S6. Use dilute acid solution to pickle the welding wire to remove surface oxides and impurities, use alkaline solution to neutralize the pickled welding wire, and thoroughly rinse it with pure water. According to specific application requirements, the surface of the welding wire is treated with anti-oxidation coating.
2. The preparation process of the welding wire according to claim 1, characterized in that: The secondary heat treatment comprises the following steps: keeping the temperature at 1050-1100° C. for 2-4 hours, and performing aging treatment at 450-500° C. for 4-6 hours.
3. The preparation process of the welding wire according to claim 1, characterized in that: In step S3, the rapid cooling includes water cooling and / or oil cooling.
4. The preparation process of the welding wire according to claim 1, characterized in that: In step S5, the temperature of the medium temperature annealing treatment is 600-650°C, the required diameter is 0.5 to 1.8 mm, and the temperature of the low temperature annealing treatment is 300 to 350°C.