A method for preparing high-quality calcium oxide

By controlling the flue gas air volume and oxygen volume ratio during the calcium oxide preparation process, the problem of insufficient calcining and decomposition of limestone is solved, and high-purity and high-activity calcium oxide preparation is achieved to meet application needs in many fields.

CN118495832BActive Publication Date: 2024-10-15HANGZHOU HONGXIN CALCIUM IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970173.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-15
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

In the existing calcium oxide preparation method, insufficient calcining and decomposition of limestone results in poor purity and activity of calcium oxide, making it difficult to meet the requirements of high purity and high activity.

Method used

By continuously introducing air during the calcination process, the flue gas outlet volume is controlled to be greater than the air inlet volume, keeping the calcination at a slight negative pressure state, and increasing the proportion of oxygen volume during the heating process to ensure that the limestone is fully decomposed, reducing the CO2 concentration, and improving The purity and activity of calcium oxide.

Benefits of technology

It achieves the preparation of calcium oxide with high purity (≥92%) and high activity (≥350mL), meets the quality needs of chemical industry, food and other fields, and improves the application performance of calcium oxide.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of calcium oxide production. Aiming at the problem that the purity and activity of calcium oxide are poor due to insufficient calcination and decomposition of limestone, the present invention discloses a method for preparing high-quality calcium oxide, comprising the following steps: 1) preheating the limestone, and then heating it to a constant calcination temperature for calcination; 2) continuously introducing air during the calcination process, and continuously drawing out the flue gas generated by the calcination, the flue gas outlet volume is greater than the air intake volume, and the flue gas outlet volume does not exceed 1.15 times the air intake volume; 3) cooling the lime obtained after calcination, crushing and screening to obtain the undersize; 4) grinding the undersize to obtain calcium oxide. The calcium oxide prepared by the method of the present invention has a purity of ≥92% and an activity of ≥350mL.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of calcium oxide production, and in particular relates to a method for preparing high-quality calcium oxide. Background Art

[0002] Calcium oxide has important and extensive uses in modern industry. For example, industrial calcium oxide with a particle size of ≤4mm and a CaO mass content of ≥90% can be used in non-ferrous metal smelting, flue gas desulfurization, waste incineration, wastewater treatment, building materials and other fields. Ultrafine calcium oxide with a particle size of ≤20μm and a CaO content of ≥93% can be used as a moisture absorbent, moisture-proof agent, food additive, as well as in the fields of medicine, chemical synthesis and sucrose production. The quality of calcium oxide determines the application performance of calcium oxide. The purity and activity of calcium oxide are important quality indicators of calcium oxide. Among them, activity is the main indicator for measuring the quality of calcium oxide.

[0003] At present, the main method for industrial preparation of calcium oxide is high-temperature calcination and decomposition of limestone. Limestone generally begins to decompose at 900°C, but the decomposition speed is relatively slow. It only begins to decompose rapidly when the temperature reaches above 1100°C. During the slow decomposition process of limestone at elevated temperature, a porous loose layer is formed after the surface decomposes, which increases the thermal resistance and prevents heat from being transported to the interior of the limestone. On the one hand, the calcium oxide generated on the surface is prone to calcination at high temperature for too long, resulting in an increase in the degree of crystal decomposition and an increase in the density of crystal arrangement, causing a decrease in activity; on the other hand, the limestone is "burned on the skin but not on the inside", and there is a raw-burned core inside, which not only affects the purity of the lime, but also causes a decrease in the activity of the lime.

[0004] The applicant disclosed a method for preparing calcium oxide in Chinese patent CN117209171B. In this preparation method, the applicant sets a reflux pipe between the calcination zone and the preheating zone, and the reflux pipe is filled with liquid or gas, and a plurality of heat storage balls that circulate along the reflux pipe; and the thickness area of ​​the reflux pipe in the preheating zone is 1 / 3 or less of the entire preheating zone. The temperature between the limestone preheating zone and the calcination zone is smoothly transitioned by controlling the loop pipe, thereby improving the production efficiency and production capacity of lime, that is, improving the process efficiency. However, this method does not have a prominent effect on improving the quality and performance of calcium oxide. Therefore, how to prepare high-purity and high-activity high-quality calcium oxide is still a technical problem that must be faced. Summary of the invention

[0005] In view of the problem that the purity and activity of calcium oxide are poor due to insufficient calcination and decomposition of limestone during the calcination and decomposition process, the object of the present invention is to provide a method for preparing calcium oxide, so as to prepare high-quality calcium oxide with high purity and high activity.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing calcium oxide, comprising:

[0008] 1) Preheat the limestone and calcine it, then heat it to a constant calcination temperature and calcine it;

[0009] 2) During the calcination process, air is continuously introduced and the flue gas generated by the calcination is continuously discharged. The flue gas outlet volume is greater than the air inlet volume. During the calcination process at a constant calcination temperature, the flue gas outlet volume does not exceed 1.15 times the air inlet volume.

[0010] 3) Cooling and calcining the lime, crushing and screening to obtain the undersize;

[0011] 4) Grind the material under the sieve to obtain calcium oxide.

[0012] In the preparation method of the present invention, limestone is first preheated at 700-800°C, and then during the calcination process, that is, during the process of heating to a constant calcination temperature after preheating and maintaining the constant calcination temperature, fresh air is continuously introduced, and at the same time, a draft fan is used to forcibly discharge the flue gas generated by the calcination, and the flue gas outlet is greater than the air inlet, so that the calcination is carried out under a slightly negative pressure state, which not only ensures smooth calcination airflow, but also reduces the concentration of CO2, thereby increasing the decomposition rate of limestone, promoting the full decomposition of limestone, and improving the purity and activity of the prepared calcium oxide. Under optimized experimental conditions, calcium oxide with a purity of ≥92% and an activity of ≥350mL (4mol / L HCl, 40±1°C, 10min) can be obtained using limestone raw materials with a CaO mass content of ≥52% and a sediment content of ≤0.5%. It should be noted that when limestone is preheated by fuel combustion, the above preparation method does not exclude the forced extraction of flue gas during preheating. At this time, the flow rate of the forced extraction of flue gas is not particularly limited, but should not significantly exceed the air intake volume, such as 1.02-1.05 times.

[0013] As a preferred embodiment of the method of the present invention, during the calcination process at a constant calcination temperature, the flue gas outlet volume is 1.03 to 1.12 times the air inlet volume.

[0014] As a preferred embodiment of the method of the present invention, during the calcination process at a constant calcination temperature, the flue gas outlet volume is 1.05 to 1.1 times the air inlet volume.

[0015] In the preparation method of the present invention, it is necessary to reasonably control the flue gas outlet and the air intake. In particular, during the calcination process at a constant calcination temperature, excessive flue gas outlet will cause the air to be discharged without being fully calcined, and insufficient calcination atmosphere will result in insufficient calcination. If the flue gas outlet is relatively small, the effect is not obvious. According to the test, the flue gas outlet does not exceed 1.15 times the air intake, preferably 1.03 to 1.12 times, and more preferably 1.05 to 1.1 times.

[0016] As a preferred embodiment of the method of the present invention, during the calcination temperature is increased from 850 to 950°C, the flue gas outlet volume is increased to 1.2 to 1.28 times the air inlet volume, and the volume proportion of oxygen in the air is increased to ≥ 27%. Preferably, during the calcination temperature is increased from 900 to 950°C to the calcination temperature, the flue gas outlet volume is increased, and / or the volume proportion of oxygen in the air is increased to 27 to 35%.

[0017] The technicians of the present invention found in the experiment that, on the basis of ensuring a slight negative pressure throughout the calcination process, increasing the flue gas outlet volume during the calcination temperature rise and correspondingly increasing the volume percentage of oxygen in the air to a certain extent will help the rapid decomposition of limestone during the calcination process, and strengthen the full decomposition effect of limestone during calcination at a constant temperature, reduce the probability of the "burning skin but not inside" phenomenon, and further improve the purity and activity of calcium oxide. This is because the rapid extraction of flue gas reduces the CO2 concentration, while the increased oxygen percentage ensures the sufficiency of combustion, fully accelerates the degree of decomposition during the temperature rise process, and thus reduces the slow decomposition during the temperature rise process. The obstacle to improving product quality. The final results also show that in this process, the timing of increasing the flue gas outlet volume and the coordination with increasing the oxygen volume percentage have a greater impact on the final improvement effect.

[0018] As a preferred embodiment of the method of the present invention, the constant calcination temperature is 1100-1250° C., the calcination time is 7-9 hours, and / or the preheating temperature is 700-800° C. A sufficiently high constant calcination temperature is conducive to the full calcination and decomposition of the limestone.

[0019] As a preferred embodiment of the method of the present invention, air is continuously introduced and smoke is extracted during cooling, and the amount of air introduced is 1.02 to 1.05 times the amount of smoke extracted. The lime is cooled quickly to prevent the lime from overburning due to residual heat.

[0020] As a preferred embodiment of the method of the present invention, the particle size of the limestone is 40-80 mm; and / or the CaO content of the limestone is ≥52%. The sediment content of the limestone is ≤0.5%.

[0021] As a preferred embodiment of the method of the present invention, the fuel used for calcination is one of anthracite, clean coal or semi-coke, and the mass ratio of the limestone to the fuel is 1000:100-130.

[0022] As a preferred embodiment of the method of the present invention, the undersize material is obtained by passing lime through a 70-80 mesh sieve.

[0023] As a preferred embodiment of the method of the present invention, the particle size of the calcium oxide obtained after grinding in step 3) is ≤50 μm.

[0024] The beneficial effects of the present invention are:

[0025] The present invention improves the calcium oxide preparation process and uses limestone with a CaO content of ≥52% as a raw material to prepare calcium oxide. The activity of the obtained calcium oxide is ≥350 mL and the purity of the calcium oxide is ≥92%, thereby achieving the dual high goals of high purity and high activity and being able to meet the calcium oxide quality requirements of different application fields such as chemical synthesis, pesticides, food, petrochemicals, leather making, desiccant, waste incineration, and sewage treatment. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below with reference to specific examples. Unless otherwise specified, the raw materials used in the examples of the present invention are all commercially available or available to those skilled in the art; unless otherwise specified, the methods used in the examples of the present invention are all methods known to those skilled in the art.

[0027] In order to maintain the consistency of preparation conditions, the following embodiments and comparative examples are all carried out in a mechanical shaft kiln. The mechanical shaft kiln uses combustion-supporting air to be blown into the kiln from the bottom and then countercurrently flow upward to contact the limestone and fuel. The smoke generated by the combustion of the fuel enters the flue along the smoke outlets on both sides of the top of the shaft kiln, and is then drawn by the induced draft fan to the dust removal and desulfurization device, or is naturally discharged from the flue to the desulfurization device.

[0028] The limestone used is limestone blocks uniformly crushed to a particle size range of 40mm-80mm. The calcium oxide content in the limestone is 52.9% and the mass content of sediment impurities is 0.3%.

[0029] Example 1 (the smoke outlet volume is 1.07 times the air inlet volume)

[0030] A method for preparing high-quality calcium oxide, the steps are as follows:

[0031] 1) Mix limestone lumps and anthracite at a mass ratio of 1000:120 and then feed them into a mechanical shaft kiln. Lower the bell cap of the mechanical shaft kiln and continuously introduce fresh air from the bottom of the mechanical shaft kiln to assist the combustion of anthracite. Control the amount of air introduced so that the limestone is preheated at 750°C first, and then heated to a constant calcination temperature of 1200°C for calcination and decomposition for 8 hours;

[0032] 2) During the process of preheating the kiln and heating it to a constant calcining temperature and maintaining it, the flue gas generated by the combustion in the kiln is continuously extracted from the flue through the induced draft fan and sent to the desulfurization device. The flue gas outlet volume is 1.07 times the fresh air inlet volume;

[0033] 3) After the limestone is calcined and decomposed, air is continuously introduced into the mechanical kiln and smoke is extracted to quickly cool the generated lime. The amount of air introduced is 1.02 times the amount of smoke extracted. The cooled lime is then sent to a jaw crusher for crushing and screened by a 70-mesh drum screen, which is the screened material.

[0034] 4) The sieve material was ground by Raymond mill to a particle size of ≤50 μm to obtain the target calcium oxide product. After testing, the purity of calcium oxide was 92.5% and the activity was 358 mL.

[0035] Example 2 (the flue gas outlet volume is 1.10 times the air inlet volume)

[0036] A method for preparing high-quality calcium oxide, the steps are as follows:

[0037] 1) Mix limestone and anthracite at a mass ratio of 1000:100 and then feed them into a mechanical shaft kiln. Put down the bell cap of the mechanical shaft kiln and continuously introduce fresh air from the bottom of the mechanical shaft kiln to assist the combustion of anthracite. Control the amount of air introduced to preheat the limestone at 700℃, then heat it to a constant calcination temperature of 1100℃ and calcine and decompose it for 9 hours;

[0038] 2) During the process of preheating the kiln and raising the temperature to a constant calcining temperature and maintaining it, the flue gas generated by the combustion in the kiln is continuously extracted from the flue through the induced draft fan and sent to the desulfurization device. The flue gas outlet volume is 1.10 times the fresh air inlet volume;

[0039] 3) After the limestone is calcined and decomposed, air is continuously introduced into the mechanical kiln and smoke is extracted to quickly cool the generated lime. The amount of air introduced is 1.03 times the amount of smoke extracted. The lime is then cooled and sent to a jaw crusher for crushing, and then screened by a 70-mesh drum screen, which is the screened material.

[0040] 4) The sieve material was ground by Raymond mill to a particle size of ≤50 μm to obtain the target calcium oxide product. After testing, the purity of calcium oxide was 92.2% and the activity was 353 mL.

[0041] Example 3 (the flue gas outlet volume is 1.05 times the air inlet volume)

[0042] A method for preparing high-quality calcium oxide, the steps are as follows:

[0043] 1) Mix limestone lumps and anthracite at a mass ratio of 1000:130 and then feed them into a mechanical shaft kiln. Lower the bell cap of the mechanical shaft kiln and continuously introduce fresh air from the bottom of the mechanical shaft kiln to assist the combustion of anthracite. Control the air intake to preheat the limestone at 800°C, then heat it to a constant calcination temperature of 1250°C and calcine and decompose for 7 hours;

[0044] 2) During the process of preheating and heating the kiln to a constant calcining temperature and maintaining it, the flue gas generated by the combustion in the kiln is continuously extracted from the flue through the induced draft fan and sent to the desulfurization device. The flue gas outlet volume is 1.05 times the fresh air inlet volume;

[0045] 3) After the limestone is calcined and decomposed, air is continuously introduced into the mechanical kiln and smoke is extracted to quickly cool the generated lime. The amount of air introduced is 1.05 times the amount of smoke extracted. The lime is then cooled and sent to a jaw crusher for crushing. The undersize is then screened by a 70-mesh drum screen.

[0046] 4) The material under the sieve was ground by Raymond mill to a particle size of ≤50 μm to obtain the target calcium oxide product. After testing, the purity of the calcium oxide was 93.0% and the activity was 364 mL.

[0047] Comparative Example 1 (Smoke is discharged naturally)

[0048] The difference from Example 1 is that during the preheating temperature rise and constant temperature calcination process, the flue gas is naturally discharged from the flue and transported to the desulfurization device without forced extraction by an induced draft fan. After testing, the purity of the prepared calcium oxide is 69.4% and the activity is 278mL. It can be seen from the test results that since the flue gas cannot be removed in time, the CO2 atmosphere content in the flue is high, which hinders the decomposition of calcium carbonate, resulting in relatively low purity and activity of calcium oxide.

[0049] Comparative Example 2 (Excessive flue gas output)

[0050] The difference from Example 1 is that during the calcination process, the flue gas outlet volume is 1.25 times the air inlet volume. After testing, the purity of the prepared calcium oxide is 63.4% and the activity is 236mL. From the test results, it can be seen that when the flue gas outlet volume is too large, the air in the kiln is insufficient, resulting in the inability to fully calcine and decompose the limestone, and the quality of the prepared calcium oxide cannot meet the requirements.

[0051] Example 4 (Increasing the flue gas output and oxygen concentration during the heating process)

[0052] A method for preparing high-quality calcium oxide, which is different from Example 1 in that in the process of raising the temperature in the kiln from 900° C. to 1200° C. in step (2), the flue gas outlet volume is increased to 1.28 times the air inlet volume, and industrial oxygen and air are mixed and fed into the kiln, and the volume proportion of oxygen in the air is increased to 35%.

[0053] After testing, the purity of the prepared calcium oxide was 93.1% and the activity was 389 mL. Compared with Example 1, the purity of calcium oxide was slightly increased and the activity was significantly increased by 8.7%.

[0054] Example 5 (Increasing the flue gas output and oxygen concentration during the heating process)

[0055] A method for preparing high-quality calcium oxide, which is different from Example 1 in that in step (2), when the temperature in the kiln is raised from 950° C. to 1200° C., the flue gas outlet volume is increased to 1.2 times the air inlet volume, and industrial oxygen and air are mixed and fed into the kiln, and the volume proportion of oxygen in the air is increased to 27%.

[0056] After testing, the purity of the prepared calcium oxide was 92.8% and the activity was 381 mL. Compared with Example 1, the purity of calcium oxide was slightly increased and the activity was significantly increased by 6.4%.

[0057] Comparative Example 3 (Only increase the proportion of oxygen)

[0058] The difference from Example 1 is that in step (2), when the temperature in the kiln is raised from 900° C. to 1200° C., the flue gas outlet and air inlet remain unchanged, but the volume proportion of oxygen in the air increases to 35%.

[0059] After testing, the purity of the prepared calcium oxide was 92.7% and the activity was 360 mL. Theoretically, compared with Example 1, increasing the oxygen concentration should be able to significantly increase the activity of calcium oxide, but in fact, the increase in the purity and activity of calcium oxide was not obvious. This may be because the combustion is sufficient after the oxygen volume ratio increases, and the CO2 concentration in the kiln also increases significantly, but the flue gas air volume does not change significantly, CO2 cannot be removed in time, and the side effects of the increase in CO2 concentration are prominent. In addition, because the fresh air cannot contact the limestone and anthracite in time, the local temperature is too high.

[0060] Comparative Example 4 (Only increase the exhaust air volume)

[0061] The difference from Example 1 is that in step (2), when the temperature in the kiln furnace is raised from 900° C. to 1200° C., the flue gas outlet volume increases to 1.28 times the air inlet volume, but the volume percentage of oxygen in the air remains unchanged.

[0062] After testing, the purity of the prepared calcium oxide was 91.2% and the activity was 352 mL, which was slightly lower than that in Example 1. This may be because the heating process was also accompanied by the decomposition of limestone. Due to insufficient air volume, the oxygen concentration decreased, resulting in a decrease in the degree of limestone decomposition in the process.

[0063] Comparative Example 5 (Increase process forward movement)

[0064] The difference from Example 1 is that in step (2), when the temperature in the kiln is increased from 750°C to 900°C, the flue gas outlet volume increases to 1.28 times the air inlet volume, and the volume proportion of oxygen in the air increases to 35%.

[0065] After testing, the purity of the prepared calcium oxide was 92.6%, and the activity was 357 mL, which was not significantly changed compared with Example 1. This may be because the quicklime had not yet decomposed during the heating process, so it had no reinforcing effect.

[0066] Comparative Example 6 (adding air induction under natural ventilation state)

[0067] The difference from Example 1 is that in step 2), except for the process in which the calcination temperature is increased from 900°C to 1200°C, the flue gas outlet volume increases to 1.28 times the air inlet volume, and the volume proportion of oxygen in the air increases to 35%. In the remaining processes, the flue gas is naturally discharged from the smoke duct to the desulfurization device.

[0068] After testing, the purity of the prepared calcium oxide was 72.4% and the activity was 298 mL, which was lower than the result of Example 1. This may be because the CO2 concentration could not be reduced in time during the entire calcination process, and the oxygen partial pressure accounted for a relatively small proportion, which ultimately led to incomplete decomposition of the limestone and failure to obtain high-quality calcium oxide.

[0069] It can be seen from the above embodiments and comparative examples that, during the calcination and decomposition of limestone, maintaining a slight negative pressure in the kiln while continuously introducing air is conducive to obtaining high-quality calcium oxide. On this basis, increasing the exhaust volume and the oxygen concentration in the intake air during the heating stage can further improve the quality of calcium oxide.

[0070] The methods for determining the activity and purity of calcium oxide in this application are as follows:

[0071] The method for determining the activity of calcium oxide refers to the manual hydrochloric acid titration method in YB / T105-997 "Metallurgical Lime Physical Test Method", which is as follows: add 10 drops of phenolphthalein indicator solution (5g / L) to 2000mL of 40℃ water, add 50g of calcium oxide sample to the water for digestion, and calculate the digestion time. When the water begins to turn red, titrate with hydrochloric acid solution (4mol / L) until the red color just disappears, and when the red color reappears, continue to titrate the hydrochloric acid solution until the red color just disappears. Record the milliliters of hydrochloric acid consumed in the 10th minute, and titrate each sample twice (if the color change is not obvious in the later stage of titration, add 2 to 4 drops of phenolphthalein indicator solution appropriately). When the absolute value of the volume difference of the hydrochloric acid solution consumed twice is not greater than 4% of the average value, take the volume average of the two hydrochloric acid solutions as the activity of calcium oxide.

[0072] The method for determining the purity of calcium oxide refers to the sucrose calcium-hydrochloric acid titration method in GB / T 5762-2024 "Chemical analysis methods for limestone, quicklime and slaked lime for building materials".

Claims

1. A method for preparing calcium oxide, characterized in that: include: 1) Preheat the limestone and then heat it to a constant calcination temperature for calcination; 2) During the calcination process, air is continuously introduced and the flue gas generated by the calcination is continuously discharged. The flue gas outlet volume is greater than the air inlet volume. During the calcination process at a constant calcination temperature, the flue gas outlet volume does not exceed 1.15 times the air inlet volume. 3) The lime obtained after cooling and calcination is crushed and sieved to obtain the undersize; 4) Grinding the undersize to obtain calcium oxide; The preheating temperature is 700 to 800 ℃; The constant calcination temperature is 1100 ~ 1250 ℃; After preheating, when the temperature rises from 900-950°C to a constant calcination temperature, the flue gas outlet volume is increased to 1.2-1.28 times the air inlet volume, and the volume percentage of oxygen in the air is increased to ≥27%; The calcination is carried out in a mechanical shaft kiln.

2. The preparation method according to claim 1, characterized in that: During the calcination process at a constant calcination temperature, the flue gas outlet volume is 1.03 to 1.12 times the air inlet volume.

3. The preparation method according to claim 1 or 2, characterized in that: During the calcination process at a constant calcination temperature, the flue gas outlet volume is 1.05 to 1.1 times the air inlet volume.

4. The preparation method according to claim 1, characterized in that: After preheating, the volume proportion of oxygen in the air is increased to 27-35% during the process of heating from 900-950°C to a constant calcination temperature.

5. The preparation method according to claim 1 or 4, characterized in that: The calcination time is 7 to 9 hours.

6. The preparation method according to claim 1, characterized in that: The particle size of the limestone is 40-80 mm; and / or the mass content of CaO in the limestone is ≥52%.

7. The preparation method according to claim 1 or 6, characterized in that: The fuel used for calcination is one of anthracite, clean coal or blue carbon, and the mass ratio of the limestone to the fuel is 1000:100-130.

8. The preparation method according to claim 1, characterized in that: Step 3) The sieved material is obtained by passing the lime through a 70-80 mesh sieve.

9. The preparation method according to claim 1, characterized in that: Step 4) The particle size of calcium oxide after grinding is ≤50 μm.