Functional polymer and preparation method and application thereof as well as tin powder modification method and tin paste

The functional polymer forms a dense layer on the surface of the tin powder, which solves the problem of easy oxidation and agglomeration of the tin powder, improves the high-temperature reflow performance and dispersion of the solder paste, and achieves low-cost and high-efficiency effects of tin powder modification.

CN118496435BActive Publication Date: 2024-10-01LINGWEI NEW MATERIALS (SHANTOU) CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410968298.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Existing tin powder modifiers are difficult to effectively adjust the molecular size and cannot form an optimal protective layer on the surface of the tin powder, causing the tin powder to easily oxidize and agglomerate, affecting the high-temperature reflow soldering performance and dispersion of the solder paste.

Method used

Using functional polymers, including maleic anhydride-styrene derivatives-fatty alcohol polyoxyethylene ether acrylate derivatives, by regulating the acid value and molecular weight of the polymer, a dense layer is formed to modify the surface of the tin powder and improve the solder paste antioxidant and dispersion properties.

Benefits of technology

It achieves efficient oxygen and water vapor barrier on the surface of the tin powder, improves the high-temperature reflow soldering performance and dispersion of the solder paste, is low-cost, and is suitable for the welding requirements of ultra-fine tin powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118496435B_ABST
    Figure CN118496435B_ABST
Patent Text Reader

Abstract

The present invention discloses a functional polymer, a preparation method and application thereof, a tin powder modification method and a tin paste, and belongs to the technical field of welding material preparation. The present invention provides a general structural formula of a functional polymer, wherein R1 represents phenyl, diphenyl, fluorophenyl, chlorophenyl, bromophenyl, tolyl, ethylphenyl, butylphenyl, octylphenyl, hydroxyphenyl, methoxyphenyl, ethoxyphenyl, acetoxyphenyl, nitrophenyl, aminophenyl or cyanophenyl, and R2 represents a hydrogen atom, C1-C 18 Alkyl, C1-C 18 Hydroxyalkyl or C1-C 18 Ether, R3 represents C1-C 22 The present invention also provides a method for preparing a functional polymer and a method for modifying the surface of tin powder using the functional polymer. The functional polymer can form a dense layer on the surface of the tin powder to effectively block oxygen and water vapor. The tin powder modified by the functional polymer has the characteristics of strong antioxidant ability, good stability and dispersibility, and is not easy to agglomerate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding material preparation, and in particular to a functional polymer and a preparation method and application thereof, as well as a tin powder modification method and tin paste. Background Art

[0002] Solder paste is a paste made of tin powder, flux and other additives. It is applied to a fixed position by printing, spraying and other methods, and then the electronic components are initially attached to the solder paste by surface mounting and other methods. At a certain temperature, as the solvent and some additives evaporate, the soldered components and the printed circuit pads are welded together to form a permanent connection. As electronic parts develop towards miniaturization, the packaging devices are shifting towards smaller, thinner and more reliable structures, which puts higher requirements on the performance of solder paste. The use of finer tin powder will become the trend of the industry. However, the smaller the particle size of tin powder, the larger the specific surface area of ​​the powder. The tin powder is easy to oxidize and agglomerate, making it difficult to disperse.

[0003] Common tin powder modifiers are unit organic acids, polybasic organic acids and their compound systems. Once the compound system is determined, its acid value and activity are determined. If the modifier activity is too high, the surface of the tin powder is easily corroded during storage. If the modifier activity is too low, it cannot be effectively adsorbed on the surface of the tin powder. Secondly, the function of the tin powder modifier is to adsorb on the surface of the tin powder to form a dense protective layer. Therefore, the molecular size of the modifier needs to be adjusted according to the size of the tin powder to achieve the optimal coating. Traditional modifiers are small molecules and cannot be adjusted in molecular size.

[0004] The invention patent CN107931891B uses acrylic resin to replace part of the rosin to wrap the tin powder. The carboxyl group on the acrylic resin has a chemical bonding effect with the surface of the tin powder alloy. By adjusting the length of the acrylic resin molecular chain, the tin powder can be prevented from being oxidized and the high-temperature reflow soldering performance of the solder paste can be improved. The invention patent CN111872599B uses organic polyacids, organic monoacids and corrosion inhibitors to form a coating layer on the surface of the tin powder, which can protect the solder powder from secondary oxidation and reduce the surface energy of the solder powder, reduce the agglomeration of the solder powder and facilitate the dispersion of the solder powder. The modified tin powder provided by the invention patent CN115609184B uses a silane compound containing a siloxy group as the first adhesion layer, which can reduce the oxidation of the tin powder before preparing the solder paste, and uses a polymer containing an amide group as the second adhesion layer to improve the dispersibility of the solder paste. The above patents improve the performance of the solder paste by modifying the surface of the tin powder in a variety of ways, so how to modify the surface of the tin powder in a cheaper and more efficient way is a concern of the industry. Summary of the invention

[0005] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a functional polymer and a preparation method and application thereof as well as a tin powder modification method and tin paste.

[0006] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] The first aspect of the present invention is to provide a functional polymer, comprising the general structural formula (I),

[0008]

[0009] (Ⅰ)

[0010] In formula (I), R1 represents phenyl, diphenyl, fluorophenyl, chlorophenyl, bromophenyl, tolyl, ethylphenyl, butylphenyl, octylphenyl, hydroxyphenyl, methoxyphenyl, ethoxyphenyl, acetoxyphenyl, nitrophenyl, aminophenyl or cyanophenyl, and R2 represents a hydrogen atom, a C1-C 18 Alkyl, C1-C 18 Hydroxyalkyl or C1-C 18 ether; R3 represents C1-C 22 Alkyl or alkylbenzene.

[0011] x represents any integer value between 1 and 2000, and y represents any integer value between 1 and 1000.

[0012] z represents any integer value from 1 to 50, and n represents any integer value from 1 to 40.

[0013] In some embodiments, in the general structural formula (I), z represents any integer value from 1 to 30, and n represents any integer value from 1 to 30; the total molecular weight of the functional polymer is less than 400,000.

[0014] It should be noted that the functional polymer provided by the present invention has a general structural formula of maleic anhydride-styrene derivative-fatty alcohol polyoxyethylene ether acrylate derivative, wherein the styrene derivative has a styrene group that can improve the thermal stability and solubility of the polymer; the maleic anhydride group can regulate the acid value of the polymer and realize efficient bonding reaction on the surface of tin powder at low temperature; the fatty alcohol polyoxyethylene ether acrylate derivative has a hydrophilic polyoxyethylene ether and a hydrophobic alkane segment or an alkylbenzene segment, so that it has better solubility adaptability in the solder paste formula.

[0015] Furthermore, the values ​​of the variable factors x, y, z and n in the general structural formula are 1-2000, 1-1000, 1-50 and 1-40 respectively. The values ​​of the above variable factors are within the appropriate range to ensure that the present invention can achieve the regulation of the polymer acid value, adsorption group, hydrophilic and hydrophobic segments and molecular weight, so that a dense layer can be formed on the surface of the modified tin powder to achieve efficient oxygen and water vapor blocking. At the same time, the solubility and compatibility of the polymer meet the solder paste component and process requirements.

[0016] The second aspect of the present invention is to provide a method for preparing a functional polymer, comprising the following preparation steps:

[0017] S1: dissolving a styrene derivative, maleic anhydride and a fatty alcohol polyoxyethylene ether acrylate derivative in toluene;

[0018] S2: introducing inert gas, and under the inert gas state, dropping the initiator into the S1 mixed system;

[0019] S3: After the temperature of the S2 system rises, the reaction begins. After the reaction is completed, the solvent is removed to obtain a functional polymer.

[0020] It should be noted that inert gas is introduced into S2 until the reaction is completed.

[0021] In some embodiments, the styrene derivative is selected from at least one of styrene, distyrene, 3-fluorostyrene, chlorostyrene, bromostyrene, toluene, ethylstyrene, butadiene, octylphenylvinyl alcohol, hydroxystyrene, methoxystyrene, ethoxystyrene, acetoxystyrene, nitrostyrene, aminostyrene or cyanostyrene; the fatty alcohol polyoxyethylene ether acrylate derivative is selected from at least one of docosyl polyoxyethylene ether methacrylate, octadecyl polyoxyethylene ether methacrylate, hexadecyl polyoxyethylene ether methacrylate, dodecyl polyoxyethylene ether methacrylate, diphenylethylphenol polyoxyethylene ether methacrylate, and triphenylphenol polyoxyethylene ether methacrylate; and the initiator is selected from at least one of an organic peroxide initiator or an azo initiator.

[0022] It should be noted that the initiator can be selected from at least one of dibenzoyl peroxide, tert-butyl perbenzoate, azobisisobutyronitrile, and dimethyl azobisisobutyrate.

[0023] In some embodiments, the molar ratio of styrene derivatives to maleic anhydride is 1-4:1, the relative molar content of fatty alcohol polyoxyethylene ether acrylate derivatives is 0.1-2.0%, the total mass of styrene derivatives, maleic anhydride and fatty alcohol polyoxyethylene ether acrylate derivatives accounts for 10-30% of the total mass of the solution; the amount of initiator used is 0.1-0.5% of the total mass of styrene derivatives, maleic anhydride and fatty alcohol polyoxyethylene ether acrylate derivatives.

[0024] In some embodiments, the temperature in S3 is raised to 40-90° C., and the reaction time is 2-12 h.

[0025] The third aspect of the present invention is to provide the use of a functional polymer as a tin powder modifier in the preparation of solder paste.

[0026] The fourth aspect of the present invention is to provide a method for modifying the surface of tin powder using a functional polymer, comprising the following steps:

[0027] (1) Ultrasonic stirring the functional polymer, organic solvent A and tin powder to obtain a mixed system;

[0028] (2) stirring the mixed system to react in a water bath;

[0029] (3) After the reaction is completed, the tin powder is centrifuged and washed with organic solvent B, and then vacuum dried to obtain modified tin powder.

[0030] It should be noted that the tin powder can be No. 5 tin powder, No. 6 tin powder, No. 7 tin powder or finer tin powder. The method of the present invention is applicable to various fine tin powders with a particle size of ≤15 μm.

[0031] In some embodiments, the water bath temperature is 25-60° C., the stirring reaction time in step (2) is 1-10 h, and the organic solvent A and the organic solvent B are both selected from at least one of methanol, ethanol, chloroform, tetrahydrofuran, toluene, xylene, and dimethyl sulfoxide.

[0032] It should be noted that the organic solvent A and the organic solvent B may be any solvent that can dissolve the functional polymer.

[0033] A fifth aspect of the present invention is to provide a solder paste comprising modified tin powder prepared by a method of modifying the surface of tin powder using a functional polymer.

[0034] It should be noted that the solder paste includes 70-90% modified tin powder and 10-30% flux, wherein the flux contains a solvent, an activator, a thixotropic agent, an antioxidant and a film-forming agent.

[0035] The present invention has the following beneficial effects:

[0036] 1. The present invention provides a functional polymer. By regulating the polymer acid value, adsorption group, hydrophilic and hydrophobic chain segments and molecular weight, the functional polymer can form a dense layer on the surface of tin powder to achieve efficient oxygen and water vapor barrier. At the same time, the solubility and compatibility of the polymer meet the requirements of solder paste components and processes, the cost is low, and it is easy to promote and apply on a large scale in the tin powder and solder paste industry.

[0037] 2. Compared with the modified compounds of traditional unit organic acids, polybasic organic acids and their composite systems, the monomer structure, proportion and molecular weight of the functional polymer provided by the present invention can be adjusted according to the type, particle size and solubility requirements of the tin powder alloy to achieve rapid adsorption and optimal coating of the modified polymer on the surface of the tin powder. The modified functional polymer has good oxygen barrier effect, small dosage, wide component applicability and simple preparation.

[0038] 3. Compared with acrylic resins using (meth) acrylic acid as chemical adsorption groups, the adsorption group of the functional polymer of the present invention, maleic anhydride, is a bidentate chelating mode, which can efficiently undergo bonding reaction on the surface of tin powder at low temperature.

[0039] 4. Compared with acrylic resins with (methyl) alkyl acrylate as physical adsorption groups, the fatty alcohol polyoxyethylene ether acrylate derivatives of the functional polymers of the present invention have hydrophilic polyoxyethylene ether and hydrophobic alkane or alkylbenzene segments, which make them have better solubility adaptability.

[0040] 5. The functional polymer provided by the present invention has the general structural formula of maleic anhydride-styrene derivative-fatty alcohol polyoxyethylene ether acrylate derivative. The tin powder modified by the functional polymer has the characteristics of strong antioxidant ability, good stability, good dispersibility, and not easy to agglomerate, and can meet the welding requirements of ultra-fine pitch. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the infrared spectrum of the functional polymer of Example 1 of the present invention. DETAILED DESCRIPTION

[0042] The present invention will be further described in detail below in conjunction with the accompanying drawings. The embodiments described with reference to the accompanying drawings are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.

[0043] Example

[0044] A method for preparing a functional polymer comprises the following steps:

[0045] S1: Measure the mass according to the requirements of Table 1, dissolve the styrene derivative, maleic anhydride and fatty alcohol polyoxyethylene ether acrylate derivative in toluene, and the total mass of the styrene derivative, maleic anhydride and fatty alcohol polyoxyethylene ether acrylate derivative accounts for 20% of the total mass of the solution;

[0046] S2: nitrogen is introduced into the S1 system, and then azobisisobutyronitrile is dripped in as an initiator, the initiator content of which is 0.2% of the total mass of styrene derivatives, maleic anhydride and fatty alcohol polyoxyethylene ether acrylate derivatives;

[0047] S3: The system obtained in S2 was heated to 40°C and reacted for 6 hours. After the reaction was completed, the temperature was cooled to room temperature and the solvent was removed by vacuum distillation to obtain a functional polymer.

[0048] In order to explore the influence of functional polymers synthesized from different monomer types on modified tin powder and solder paste, this embodiment uses maleic anhydride, styrene derivatives (styrene and 3-fluorostyrene) and fatty alcohol polyoxyethylene ether acrylate derivatives (dicosyl polyoxyethylene ether methacrylate and triphenyl phenol polyoxyethylene ether methacrylate) as reaction monomers. The functional polymer is obtained by changing the synthesis conditions by adjusting the monomer types. Table 1 shows the mass of monomers added in Examples 1-8, in g.

[0049] Table 1 Type and quality of monomers in Examples 1-8

[0050]

[0051] The functional polymer prepared in Example 1 was subjected to infrared spectroscopy analysis, and the results were as follows: Figure 1 shown. Figure 1 The infrared spectrum shows that at 1226 cm -1 is the absorption peak of COC symmetric stretching vibration in anhydride, 1776 cm -1 The absorption peaks are the symmetric and antisymmetric stretching vibrations of C=O on the cyclic anhydride group, the deformation vibration absorption peak of the C=C skeleton of the benzene ring appears at 1495, and the absorption peak at 1084 cm -1 The absorption peak of the CH in-plane bending vibration on the benzene ring is 704 cm -1 、760 cm -1 is the absorption peak of the out-of-plane bending vibration of CH on the benzene ring, 1219 cm -1 is the stretching vibration absorption peak of COC in the ester group, 1118 cm -1 is the stretching vibration absorption peak of the long-chain alkyl group, 1453 cm -1 is the bending vibration absorption peak of methyl group, 1558 cm -1 The peak of -COO asymmetric stretching vibration indicates that the polymer is a copolymer of the above three monomers. The total molecular weight of the functional polymer in Example 1 is ≤300,000, and the structure is as follows:

[0052] .

[0053] A method for modifying the surface of tin powder using the functional polymer prepared in the above embodiment comprises the following steps:

[0054] (1) Mix 2 g of the functional polymer and 50 mL of toluene, add 20 g of tin powder and stir to disperse evenly under ultrasonic conditions to obtain a mixed system;

[0055] (2) Stir the mixture in a water bath at 40°C for 2 h;

[0056] (3) After the reaction is completed, the tin powder is centrifuged and washed three times with toluene, and then vacuum dried to obtain modified tin powder.

[0057] A solder paste comprising the modified tin powder, wherein the following is a method for preparing the solder paste: adding flux to the modified tin powder, wherein the modified tin powder accounts for 85% of the total mass of the solder paste, and the flux accounts for 15% of the total mass of the solder paste; wherein the flux comprises a solvent, an activator, a thixotropic agent, an antioxidant and a film-forming agent.

[0058] Comparative Example

[0059] The preparation methods of the functional polymers, modified tin powders and solder pastes of Comparative Examples 1-3 are the same as those of Example 1, except for the type and mass of the reactive monomers. Table 2 shows the mass of the corresponding monomers added in Comparative Examples 1-3, in g.

[0060] Table 2 Comparative Examples 1-3 Reaction Monomer Types and Masses

[0061]

[0062] In order to explore the effect of modified tin powder on solder paste, comparative examples 4-7 were also set up, in which organic acid, acrylic acid and other modifying substances were added to replace the functional polymer of the present invention to modify the tin powder.

[0063] Table 3 Modified substances and quality of comparative examples 4-7

[0064]

[0065] The preparation method of the modified tin powder of Comparative Examples 4-7 is as follows: the modified substances are prepared according to Table 3 and dissolved in 50 ml of toluene, then 20 g of tin powder is added, stirred in a constant temperature water bath at 40° C. for 2 h, filtered, and vacuum dried to obtain the corresponding modified tin powder.

[0066] A solder paste comprising the modified tin powder of the above-mentioned comparative examples 4-7, and the following is a method for preparing the solder paste: adding flux to the modified tin powder, wherein the modified tin powder accounts for 85% of the total mass of the solder paste, and the flux accounts for 15% of the total mass of the solder paste; wherein the flux comprises a solvent, an activator, a thixotropic agent, an antioxidant and a film-forming agent.

[0067] Performance testing

[0068] The modified tin powder and tin paste obtained in Examples 1-8 and Comparative Examples 1-7 were tested, and the test items and methods were as follows:

[0069] (1) Oxygen content

[0070] The modified tin powder was placed in a drying oven at 35°C for 48 hours, and the oxygen content on the surface of the modified tin powder was tested by an oxygen and nitrogen tester to characterize the coating effect of the tin powder. The higher the oxygen content, the less ideal the coating effect of the adhesion layer is, and the tin powder cannot be completely isolated from oxidation.

[0071] (2) Dispersibility

[0072] The spectrophotometric test was conducted by weighing 2 g of modified tin powder, adding 10 ml of glycerol, stirring lightly and letting it stand for 20 minutes. The upper clear liquid was taken as the test sample and the absorbance of the sample was tested to judge the dispersion effect of the tin powder. The smaller the absorbance, the shorter the suspension time of the tin powder in the solvent and the poorer the dispersion performance.

[0073] (3) Solder ball test

[0074] Referring to the industry standard JIS Z3284 or IPC-TM-650 2.4.43, the prepared solder paste is melted and cooled to room temperature, and then printed on a substrate that cannot be wetted by solder. The solder balls are observed and statistically analyzed using a 20x microscope, and the evaluation is made with reference to the solder ball test evaluation table in Table 4 below to characterize the performance of tin powder in solder paste applications. The greater the solder aggregation, the more free solder balls there are, and the greater the impact on soldering performance. When the aggregation is 1, the effect is best.

[0075] Table 4 Solder ball test evaluation table

[0076]

[0077] (4) Adhesion change test

[0078] The prepared solder paste was placed in a 30℃ constant temperature box. After one week, the change in the sample adhesion was measured to characterize the stability of the solder paste. The greater the change in adhesion, the more serious the agglomeration problem of the sample during storage. The smaller the change in adhesion, the better the stability of the solder paste.

[0079] (5) Reflow test

[0080] The prepared solder paste was screen printed through steel meshes with different dot diameters (for example, 0.20mm, 0.22mm, 0.24mm, 0.26mm, 0.28mm, 0.30mm, 0.32mm, 0.34mm, 0.36mm, 0.38mm, 0.4mm), and the solder paste was observed after passing through the reflow oven to evaluate the minimum dot diameter allowed to pass when the solder joints avoid "grape-like" defects on the surface, so as to characterize the application effect of functional polymer modified tin powder in solder paste. The smaller the minimum dot diameter allowed to pass when "grape-like" defects appear on the solder joint surface, the better the soldering effect of the modified tin powder in the solder paste.

[0081] (6) Wettability test

[0082] Referring to the industry standard JISZ3284, solder paste is printed on a brass plate of size 50×50×0.5mm and then heated and soldered. The sample after soldering is cooled to room temperature to remove the residual flux, and then a 10x magnifying glass is used to judge the solder wettability grade evaluation table. The wettability grade of the solder paste should meet the judgment standard of level 1 or level 2 in Table 5.

[0083] Table 5 Solder wettability evaluation table

[0084]

[0085] The performance test results of the modified tin powder or solder paste obtained in Examples 1-8 and Comparative Examples 1-7 are shown in Table 6.

[0086] Table 6 Performance test results of modified tin powder or solder paste obtained in Examples 1-8 and Comparative Examples 1-7

[0087]

[0088] From the above performance test results, it can be seen that the antioxidant capacity, absorbance, tin bead test, adhesion stability, reflow test and wettability test of the modified tin powder of Examples 1-8 of the present invention are better than those of Comparative Examples 1-3; the stability of the solder paste in the embodiments of the present invention is better than that of Comparative Examples 1-3, which shows that the R1, R2 and R3 groups are beneficial to improving the performance of the modified tin powder and solder paste, and can form a dense layer on the surface of the tin powder to achieve efficient barrier against oxygen and water vapor. If any one group is missing, good comprehensive performance cannot be achieved.

[0089] Compared with Comparative Examples 4 and 5, the antioxidant capacity of 1-8 of Examples of the present invention is significantly improved, indicating that the rapid adsorption and dense coating of the functional polymer of the present invention on the surface of the tin powder can effectively prevent the oxidation of the surface of the tin powder; compared with Comparative Example 6, the antioxidant capacity, viscosity stability, reflow test and wettability test of 1-8 of Examples of the present invention all have certain advantages, indicating that the functional polymer of the present invention forms a denser barrier layer with the surface of the tin powder, and the hydrophilic and hydrophobic segments in the fatty alcohol polyoxyethylene ether acrylate are better matched with the solder paste formula and preparation process.

[0090] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. Application of functional polymers in the preparation of solder paste, It is characterized in that The functional polymer is used as a tin powder modifier; The functional polymer is prepared by the following steps: S1: dissolving styrene or a styrene derivative, maleic anhydride and a polyoxyethylene ether acrylate derivative in toluene; wherein the styrene derivative is selected from at least one of 3-fluorostyrene, chlorostyrene, bromostyrene, methylstyrene, ethylstyrene, butylstyrene, octylstyrene, hydroxystyrene, methoxystyrene, ethoxystyrene, acetoxystyrene, nitrostyrene, aminostyrene or cyanostyrene; the polyoxyethylene ether acrylate derivative is selected from at least one of docosyl polyoxyethylene ether methacrylate, octadecyl polyoxyethylene ether methacrylate, hexadecyl polyoxyethylene ether methacrylate, dodecyl polyoxyethylene ether methacrylate, diphenylethylphenol polyoxyethylene ether methacrylate or triphenethylphenol polyoxyethylene ether methacrylate; the molar ratio of the styrene or styrene derivative to the maleic anhydride is 1-4:1; the relative molar content of the polyoxyethylene ether acrylate derivative is 0.1-2.0%, and the total mass of the styrene or styrene derivative, maleic anhydride and polyoxyethylene ether acrylate derivative accounts for 10-30% of the total mass of the solution; S2: introducing an inert gas, and under the inert gas state, dropping an initiator into the S1 mixed system; wherein the amount of the initiator is 0.1-0.5% of the total mass of the styrene or styrene derivative, maleic anhydride and polyoxyethylene ether acrylate derivative; and the initiator is selected from at least one of an organic peroxide initiator and an azo initiator; S3: After the temperature of the S2 system is raised, the reaction begins. After the reaction is completed, the solvent is removed to obtain a functional polymer; wherein the temperature is raised to 40-90°C and the reaction time is 2-12h; The total molecular weight of the functional polymer is less than 400,000.

2. Method for modifying the surface of tin powder using functional polymers. It is characterized in that The following steps are involved: (1) Ultrasonic stirring the functional polymer, organic solvent A and tin powder to obtain a mixed system; (2) stirring the mixed system to react in a water bath; (3) After the reaction is completed, the tin powder is centrifuged and washed with an organic solvent B, and then vacuum dried to obtain modified tin powder; The functional polymer is prepared by the following steps: S1: dissolving styrene or a styrene derivative, maleic anhydride and a polyoxyethylene ether acrylate derivative in toluene; wherein the styrene derivative is selected from at least one of 3-fluorostyrene, chlorostyrene, bromostyrene, methylstyrene, ethylstyrene, butylstyrene, octylstyrene, hydroxystyrene, methoxystyrene, ethoxystyrene, acetoxystyrene, nitrostyrene, aminostyrene or cyanostyrene; the polyoxyethylene ether acrylate derivative is selected from at least one of docosyl polyoxyethylene ether methacrylate, octadecyl polyoxyethylene ether methacrylate, hexadecyl polyoxyethylene ether methacrylate, dodecyl polyoxyethylene ether methacrylate, diphenylethylphenol polyoxyethylene ether methacrylate or triphenethylphenol polyoxyethylene ether methacrylate; the molar ratio of the styrene or styrene derivative to the maleic anhydride is 1-4:1; the relative molar content of the polyoxyethylene ether acrylate derivative is 0.1-2.0%, and the total mass of the styrene or styrene derivative, maleic anhydride and polyoxyethylene ether acrylate derivative accounts for 10-30% of the total mass of the solution; S2: introducing an inert gas, and under the inert gas state, dropping an initiator into the S1 mixed system; wherein the amount of the initiator is 0.1-0.5% of the total mass of the styrene or styrene derivative, maleic anhydride and polyoxyethylene ether acrylate derivative; and the initiator is selected from at least one of an organic peroxide initiator and an azo initiator; S3: After the temperature of the S2 system is raised, the reaction begins. After the reaction is completed, the solvent is removed to obtain a functional polymer; wherein the temperature is raised to 40-90°C and the reaction time is 2-12h; The total molecular weight of the functional polymer is less than 400,000.

3. The method for modifying the surface of tin powder using a functional polymer according to claim 2, It is characterized in that The water bath temperature is 25-60° C., the stirring reaction time in step (2) is 1-10 h, and the organic solvent A and the organic solvent B are both selected from at least one of methanol, ethanol, chloroform, tetrahydrofuran, toluene, xylene, and dimethyl sulfoxide.

4. Solder paste, It is characterized in that The modified tin powder is prepared by the method of modifying the surface of tin powder using a functional polymer as described in claim 2.

Citation Information

Patent Citations

  • A solder paste flux

    CN107931891B

  • A modified tin powder and tin paste

    CN111872599B

  • Modified tin powder and its preparation method, tin paste

    CN115609184B

  • Solder paste scaling powder

    CN107931891A

  • Crumb-dewatering-process biting characteristic improver and method for producing rubber-like polymer