A PP composite insulation board for cold storage and its production method
By using functional fibers and inorganic composite flame retardant fillers in PP composite insulation boards, the problem of insufficient strength and flame retardant performance is solved, and the high strength and high flame retardant performance is improved, which extends the service life and reduces the Safety hazards.
Patent Information
- Application Number
- CN202410442198.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-04-12
AI Technical Summary
The strength and flame retardant properties of the existing PP composite insulation boards are insufficient, and they are prone to deformation, bending and fracture, and polypropylene is flammable, which poses safety hazards.
Functional fibers and inorganic composite flame retardant fillers are used to modify mica powder through plasma treatment and intercalation method to form a mesh structure and expand flame retardant effect, and improve the strength and flame retardant performance of the material.
It effectively enhances the mechanical properties and flame retardant properties of PP composite insulation board, avoids deformation and fracture caused by external impact and load, and improves flame retardant performance and extends service life.
Smart Images

Figure CN118496550B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal insulation boards, and in particular to a PP composite thermal insulation board for refrigeration and a production method thereof. Background Art
[0002] Refrigeration insulation board is a commonly used material to isolate the internal environment of refrigeration equipment from the external environment. It is a very important component of refrigeration equipment. Ordinary insulation board usually adopts traditional insulation materials, such as glass fiber, mineral wool, etc., and no foaming agent is required during the preparation process. It is easily affected by factors such as ambient temperature and humidity, resulting in unstable thermal insulation performance. PP composite insulation board uses polypropylene as the base material of the composite material. In the production process, tiny pores are formed by adding foaming agent, so that the insulation board has good thermal insulation performance, and other functional additives are added on this basis to prepare high-performance PP composite insulation board, which has good chemical stability, corrosion resistance, insulation and other excellent properties, and has good development prospects.
[0003] In practical applications, PP composite insulation boards for cold storage need to withstand various pressures and loads. If the strength of the PP composite insulation board is insufficient, it is easy to deform, bend, break and other problems, affecting its insulation effect and service life. In addition, polypropylene is a flammable material. When it encounters open flames or high temperatures, it is easy to burn and release a large amount of heat and toxic gases, posing a serious threat to people's life and property safety. Therefore, it is necessary to improve the strength and flame retardant properties of the PP composite insulation board and extend its service life. The patent with announcement number CN105948606B discloses a polypropylene reinforced modified expanded perlite insulation board and a production method thereof. By adding modified expanded perlite, PP fiber and other organic and inorganic substances as raw materials, the fire resistance, strength, crack resistance, flexibility and water absorption of the insulation board are improved. However, the added inorganic substances are not highly dispersed in the matrix and are prone to agglomeration. In addition, due to the addition of multiple raw materials, the production process is complicated, and it is necessary to strictly control the ratio of each component and the processing temperature and other parameters, otherwise it is easy to affect the performance and quality of the insulation board. Based on this, it is of great significance for the present invention to develop a PP composite insulation board with high strength and high flame retardancy. Summary of the invention
[0004] The purpose of the present invention is to provide a PP composite insulation board for cold storage and a production method thereof, which solves the following technical problems:
[0005] (1) Solved the problem of poor strength of PP insulation board;
[0006] (2) The problem of poor flame retardancy of PP insulation board has been solved.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A method for producing a PP composite insulation board for cold storage comprises the following steps:
[0009] (1) By weight, 20 to 40 parts of polypropylene, 20 to 30 parts of polyacrylate emulsion, 10 to 15 parts of talc, 5 to 8 parts of sodium carboxymethyl cellulose, 8 to 10 parts of hollow glass microspheres, 5 to 8 parts of functionalized fibers and 3 to 9 parts of inorganic composite flame retardant filler are mixed and stirred to obtain a premix;
[0010] (2) The premix obtained in step (1) is put into a stirrer, and then 5 to 10 parts of a foaming agent, 6 to 9 parts of a surfactant and 40 to 70 parts of deionized water are added, and after stirring and mixing evenly, the mixture is heated to 65 to 75° C., kept warm and stirred for 15 to 25 minutes, and then poured into a mold for pressure-maintaining molding. After molding, the mixture is demolded, and then naturally cured, sawed, polished and packaged to obtain a PP composite insulation board.
[0011] Furthermore, the production method of the functionalized fiber comprises the following steps:
[0012] S1: placing the ultra-high molecular weight polyethylene fiber in distilled water, ultrasonically cleaning it for 20 to 40 minutes, placing the cleaned fiber in an oven at 50 to 70° C. and drying it to constant weight to obtain the pretreated ultra-high molecular weight polyethylene fiber;
[0013] S2: placing the pretreated ultra-high molecular weight polyethylene fiber in a plasma treatment apparatus, evacuating the system to 8-10 Pa, and then injecting air for plasma treatment to obtain modified ultra-high molecular weight polyethylene fiber;
[0014] S3: Add modified ultra-high molecular weight polyethylene fiber to toluene, ultrasonically disperse for 10 to 30 minutes, then add maleic anhydride grafted EPDM rubber, mechanically stir and mix evenly, add p-toluenesulfonic acid, pass nitrogen protection, increase the system temperature to 80 to 90°C, keep warm for 4 to 8 hours, wait for the material to cool, filter, wash and dry to obtain functionalized fiber.
[0015] Furthermore, in step S1, the ultra-high molecular weight polyethylene fiber has a length of 0.2 to 0.8 mm and a diameter of 8 to 12 μm.
[0016] Furthermore, in step S2, during the plasma treatment, the discharge power is set to 70-90 W, the gas pressure is set to 10-30 Pa, the gas flow rate is set to 20-30 ml / min, and the treatment time is set to 2-4 min.
[0017] Furthermore, in step S3, the mass ratio of the maleic anhydride grafted EPDM rubber to the modified ultra-high molecular weight polyethylene fiber is 1:1-2.
[0018] Through the above technical scheme, the pretreated ultra-high molecular weight polyethylene fiber is subjected to plasma treatment to introduce hydroxyl groups on the fiber surface. Then, under the action of the catalyst p-toluenesulfonic acid, the maleic anhydride groups in the maleic anhydride grafted EPDM rubber can undergo ring-opening condensation with the hydroxyl groups on the fiber surface, and the maleic anhydride grafted EPDM rubber is grafted onto the surface of the ultra-high molecular weight polyethylene fiber to obtain functionalized fibers.
[0019] Furthermore, the production method of the inorganic composite flame retardant filler comprises the following steps:
[0020] Ⅰ: Add mica powder to distilled water, stir to make it dispersed evenly, obtain mica powder suspension, add chitosan to acetic acid solution, stir and mix for 3-5h, then start to drop sodium hydroxide solution, adjust the pH value of the system to 4-5, obtain chitosan solution, then add the chitosan solution to the mica powder suspension, stir at 45-55°C for 6-10h, finally wash with distilled water, filter, and vacuum dry to obtain intercalated modified mica powder;
[0021] Ⅱ: Add the intercalated modified mica powder to N,N-dimethylformamide, stir to mix evenly, then add hexachlorocyclotriphosphazene, heat to 85-95°C, add pyridine, react for 3-5 hours, after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain an inorganic composite flame retardant filler.
[0022] Furthermore, in step I, the fineness of the mica powder is 3000-4000 mesh.
[0023] Furthermore, in step I, the mass fraction of the acetic acid solution is 1%; the mass fraction of the sodium hydroxide solution is 10%.
[0024] Furthermore, in step (2), the foaming agent is any one of n-pentane, n-hexane or n-heptane; and the surfactant is any one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate or hydroxypropyl methylcellulose ether.
[0025] Through the above technical scheme, chitosan is introduced into the interlayer of mica powder by an in-situ intercalation method to obtain intercalation modified mica powder, and then under the action of pyridine, the chitosan in the intercalation modified mica powder contains active group amino groups that can react with PC 1 in hexachlorocyclotriphosphazene, thereby grafting hexachlorocyclotriphosphazene into the intercalation modified mica powder to obtain an inorganic composite flame retardant filler.
[0026] Beneficial effects of the present invention:
[0027] (1) The present invention uses functionalized fibers to fill and modify polypropylene. Since the rubber molecular chains grafted on the fiber surface have good compatibility with the polypropylene matrix, the functionalized fibers are firmly embedded in the polypropylene matrix to form a polypropylene composite material with a network structure. After foaming, the functional fibers can be evenly distributed in the polypropylene foam. By utilizing the high strength of the fibers themselves and the stress dispersion effect of the network structure, the deformation, bending, and fracture of the insulation board caused by external impact and long-term load can be effectively avoided, thereby effectively enhancing the mechanical properties of the PP composite insulation board.
[0028] (2) The inorganic composite flame retardant filler prepared by the present invention is organically modified mica powder. After modification, the compatibility between the mica powder and the polypropylene matrix can be improved, so that it can be dispersed more evenly in the matrix, and its own lamellar structure can produce a physical barrier effect to isolate oxygen and heat, thereby improving the flame retardant properties of the PP composite insulation board. At the same time, the chitosan and hexachlorocyclotriphosphazene contained in the modified structure of the mica powder can produce an expansion flame retardant effect, thereby effectively improving the flame retardant properties of the polypropylene composite insulation board.
[0029] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0031] Figure 1 This is an infrared spectrum test chart of the functionalized fiber prepared in Example 1 of the present invention.
[0032] Figure 2 This is an infrared spectrum test chart of the inorganic composite flame retardant filler prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] 1. Functionalized Fiber
[0036] S1: placing the ultra-high molecular weight polyethylene fiber in distilled water, ultrasonically cleaning it for 30 minutes, and placing the cleaned fiber in an oven at 60° C. to dry it to constant weight, thereby obtaining the pretreated ultra-high molecular weight polyethylene fiber;
[0037] S2: placing the pretreated ultra-high molecular weight polyethylene fiber in a plasma treatment apparatus with a discharge power of 80 W, evacuating the system to 10 Pa, and then injecting air for plasma treatment for 3 min to obtain modified ultra-high molecular weight polyethylene fiber;
[0038] S3: Add 5g of modified ultra-high molecular weight polyethylene fiber to toluene, ultrasonically disperse for 20 minutes, then add 4.2g of maleic anhydride grafted EPDM rubber, stir mechanically to mix evenly, add 0.3g of p-toluenesulfonic acid, pass nitrogen protection, raise the system temperature to 85°C, keep warm for 6 hours, wait for the material to cool, filter, wash and dry to obtain functionalized fiber.
[0039] The modified ultra-high molecular weight polyethylene fiber and functionalized fiber were tested by infrared spectrometer Nicolet-Nexus 670. Figure 1 As shown, the sample was prepared by potassium bromide tablet method, and the spectral scanning range was 4000cm -1 ~500cm -1 , the analysis shows that in the infrared spectrum of the modified ultra-high molecular weight polyethylene fiber, 3279cm -1 The peak at 1712 cm is the stretching vibration peak of the hydroxyl group. -1 The stretching vibration peak of the carboxyl group C=O is at 1752cm. This is because after the pretreated ultra-high molecular weight polyethylene fiber is treated with plasma, hydroxyl and carboxyl groups are introduced on the fiber surface. In the infrared spectrum of the functionalized fiber, 1752cm -1 The stretching vibration peak of the ester group C=O is 1718 cm -1 The center is the stretching vibration peak of the carboxyl group C=O, and the absorption peak intensity of the carboxyl group is enhanced. This is because the maleic anhydride group in the maleic anhydride grafted EPDM rubber can undergo ring-opening condensation with the hydroxyl group on the surface of the modified ultra-high molecular weight polyethylene fiber to produce ester groups and carboxyl groups, which indicates that the grafting is successful.
[0040] 2. Inorganic composite flame retardant filler
[0041] Ⅰ: Add 5g of mica powder to distilled water, stir to disperse it evenly, and obtain a mica powder suspension. Add 1g of chitosan to a 1% acetic acid solution, stir and mix for 3 to 5h, then start to drop a 20% sodium hydroxide solution, adjust the pH value of the system to 4.9, and obtain a chitosan solution. Then, add the chitosan solution to the mica powder suspension, stir at 50°C for 8h, and finally wash with distilled water, filter, and vacuum dry to obtain intercalated modified mica powder;
[0042] Ⅱ: Add 10g of intercalated modified mica powder to N,N-dimethylformamide, stir to mix evenly, then add 3.5g of hexachlorocyclotriphosphazene, heat to 90°C, add 0.4g of pyridine, react for 4h, after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain an inorganic composite flame retardant filler.
[0043] The infrared test of inorganic composite flame retardant filler was carried out using Nicolet-Nexus 670 Fourier infrared spectrometer. Figure 2 As shown, the sample was prepared by potassium bromide tablet method, and the spectral scanning range was 4000cm -1 ~500cm -1 According to the infrared spectrum of inorganic composite flame retardant filler, at 1189cm -1 The characteristic absorption peak of P=N appears at 892cm -1 The characteristic absorption peak of PN appears at 3298cm -1 The characteristic absorption peak of OH appears at 3421cm -1 The characteristic absorption peak of NH appears at 1112 cm -1 The characteristic absorption peak of CO appears at
[0044] 3. Preparation of PP composite insulation board
[0045] (1) By weight, 20 parts of polypropylene, 20 parts of polyacrylate emulsion, 10 parts of talc, 5 parts of sodium carboxymethyl cellulose, 8 parts of hollow glass microspheres, 5 parts of functionalized fibers and 3 parts of inorganic composite flame retardant filler are mixed and stirred to obtain a premix;
[0046] (2) The premix obtained in step (1) is put into a stirrer, and then 5 parts of n-hexane, 6 parts of sodium dodecylbenzene sulfonate and 40 parts of deionized water are added, and after stirring and mixing, the temperature is raised to 65° C., and the mixture is stirred and kept warm for 15 minutes. Then, the mixture is poured into a mold for pressure-maintaining molding, and after molding, demolding treatment is performed, and then natural curing, sawing, grinding, and packaging are performed to obtain a PP composite insulation board.
[0047] Example 2
[0048] Preparation of PP composite insulation board
[0049] (1) By weight, 30 parts of polypropylene, 25 parts of polyacrylate emulsion, 12 parts of talc, 6 parts of sodium carboxymethyl cellulose, 9 parts of hollow glass microspheres, 6 parts of functionalized fibers and 5 parts of inorganic composite flame retardant filler are mixed and stirred to obtain a premix;
[0050] (2) The premix obtained in step (1) is put into a stirrer, and then 8 parts of n-hexane, 7 parts of sodium dodecylbenzene sulfonate and 60 parts of deionized water are added, and after stirring and mixing evenly, the mixture is heated to 70° C. and stirred for 20 minutes. The mixture is then poured into a mold for pressure-maintaining molding, and after molding, demolding treatment is performed, and then natural curing, sawing, grinding and packaging are performed to obtain a PP composite insulation board.
[0051] The preparation method of the functionalized fiber and the inorganic composite flame retardant filler is the same as that in Example 1.
[0052] Example 3
[0053] Preparation of PP composite insulation board
[0054] (1) By weight, 40 parts of polypropylene, 30 parts of polyacrylate emulsion, 15 parts of talc, 8 parts of sodium carboxymethyl cellulose, 10 parts of hollow glass microspheres, 8 parts of functionalized fibers and 9 parts of inorganic composite flame retardant filler are mixed and stirred to obtain a premix;
[0055] (2) The premix obtained in step (1) is put into a stirrer, and then 10 parts of n-hexane, 9 parts of sodium dodecylbenzene sulfonate and 70 parts of deionized water are added, and after stirring and mixing, the temperature is raised to 75° C., and the mixture is kept warm and stirred for 25 minutes. Then, the mixture is poured into a mold for pressure-maintaining molding, and after molding, demolding treatment is performed, and then natural curing, sawing, grinding, and packaging are performed to obtain a PP composite insulation board.
[0056] The preparation method of the functionalized fiber and the inorganic composite flame retardant filler is the same as that in Example 1.
[0057] Comparative Example 1
[0058] Preparation of PP composite insulation board
[0059] (1) By weight, 30 parts of polypropylene, 25 parts of polyacrylate emulsion, 12 parts of talc, 6 parts of sodium carboxymethyl cellulose, 9 parts of hollow glass microspheres, and 6 parts of functionalized fibers were mixed and stirred to obtain a premix;
[0060] (2) The premix obtained in step (1) is put into a stirrer, and then 8 parts of n-hexane, 7 parts of sodium dodecylbenzene sulfonate and 60 parts of deionized water are added, and after stirring and mixing evenly, the mixture is heated to 70° C. and stirred for 20 minutes. The mixture is then poured into a mold for pressure-maintaining molding, and after molding, demolding treatment is performed, and then natural curing, sawing, grinding and packaging are performed to obtain a PP composite insulation board.
[0061] The preparation method of the functionalized fiber is the same as that in Example 1.
[0062] Comparative Example 2
[0063] Preparation of PP composite insulation board
[0064] (1) By weight, 30 parts of polypropylene, 25 parts of polyacrylate emulsion, 12 parts of talc, 6 parts of sodium carboxymethyl cellulose, 9 parts of hollow glass microspheres, and 5 parts of inorganic composite flame retardant filler are mixed and stirred to obtain a premix;
[0065] (2) The premix obtained in step (1) is put into a stirrer, and then 8 parts of n-hexane, 7 parts of sodium dodecylbenzene sulfonate and 60 parts of deionized water are added, and after stirring and mixing evenly, the mixture is heated to 70° C. and stirred for 20 minutes. The mixture is then poured into a mold for pressure-maintaining molding, and after molding, demolding treatment is performed, and then natural curing, sawing, grinding and packaging are performed to obtain a PP composite insulation board.
[0066] The preparation method of the inorganic composite flame retardant filler is the same as that in Example 1.
[0067] Comparative Example 3
[0068] Preparation of PP composite insulation board
[0069] (1) By weight, 30 parts of polypropylene, 25 parts of polyacrylate emulsion, 12 parts of talc, 6 parts of sodium carboxymethyl cellulose, and 9 parts of hollow glass microspheres were mixed and stirred to obtain a premix;
[0070] (2) The premix obtained in step (1) is put into a stirrer, and then 8 parts of n-hexane, 7 parts of sodium dodecylbenzene sulfonate and 60 parts of deionized water are added, and after stirring and mixing evenly, the mixture is heated to 70° C. and stirred for 20 minutes. The mixture is then poured into a mold for pressure-maintaining molding, and after molding, demolding treatment is performed, and then natural curing, sawing, grinding and packaging are performed to obtain a PP composite insulation board.
[0071] Performance Testing
[0072] The PP composite insulation boards prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were sheeted to prepare test specimens that met the specifications. The tensile strength of the samples was tested according to GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets"; the bending strength of the samples was tested according to GB / T 8812.2-2007 "Determination of flexural properties of rigid foam plastics Part 2: Determination of flexural strength and apparent flexural modulus of elasticity"; the impact strength of the samples was tested according to GB / T 1043.1-2008 "Determination of impact properties of simply supported beams of plastics Part 1: Non-instrumented impact test"; the combustion performance of the samples was tested according to GB / T2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test" to determine the flame retardant properties of the samples. The specific test results are shown in the following table:
[0073]
[0074] From the data in the above table, it can be concluded that the samples prepared in Examples 1 to 3 of the present invention have high limiting oxygen index, tensile strength, flexural strength and impact strength values, and have excellent flame retardant properties, mechanical properties and high strength; the sample prepared in Comparative Example 1 adds functionalized fibers, and the sample has good mechanical properties and high strength, but the sample prepared in Comparative Example 1 does not add inorganic composite flame retardant fillers, and compared with the embodiments, the limiting oxygen index is lower, and the flame retardant properties of the sample are poor; the sample prepared in Comparative Example 2 adds inorganic composite flame retardant fillers, has a high limiting oxygen index, and has good flame retardant properties, but the sample prepared in Comparative Example 1 does not add functionalized fibers, and compared with the embodiments, the tensile strength, flexural strength and impact strength values of the sample decrease, and the mechanical properties and strength performance of the sample are poor; the sample prepared in Comparative Example 3 does not add either functionalized fibers or inorganic composite flame retardant fillers, and the flame retardant properties, mechanical properties and strength performance of the sample are poor.
[0075] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for producing a PP composite insulation board for cold storage, characterized in that: The following steps are involved: (1) By weight, 20 to 40 parts of polypropylene, 20 to 30 parts of polyacrylate emulsion, 10 to 15 parts of talc, 5 to 8 parts of sodium carboxymethyl cellulose, 8 to 10 parts of hollow glass microspheres, 5 to 8 parts of functionalized fibers and 3 to 9 parts of inorganic composite flame retardant filler are mixed and stirred to obtain a premix; (2) adding the premix obtained in step (1) into a stirrer, and then adding 5 to 10 parts of a foaming agent, 6 to 9 parts of a surfactant and 40 to 70 parts of deionized water, stirring and mixing evenly, heating to 65 to 75° C., stirring and keeping warm for 15 to 25 minutes, and then pouring into a mold for pressure-maintaining molding, demolding after molding, and then performing natural curing, sawing, grinding, and packaging to obtain a PP composite insulation board; The production method of the functionalized fiber comprises the following steps: S1: placing the ultra-high molecular weight polyethylene fiber in distilled water, ultrasonically cleaning it for 20 to 40 minutes, placing the cleaned fiber in an oven at 50 to 70° C. and drying it to constant weight to obtain the pretreated ultra-high molecular weight polyethylene fiber; S2: placing the pretreated ultra-high molecular weight polyethylene fiber in a plasma treatment apparatus, evacuating the system to 8-10 Pa, and then injecting air for plasma treatment to obtain modified ultra-high molecular weight polyethylene fiber; S3: adding the modified ultra-high molecular weight polyethylene fiber to toluene, ultrasonically dispersing for 10 to 30 minutes, then adding maleic anhydride grafted EPDM rubber, mechanically stirring and mixing evenly, adding p-toluenesulfonic acid, passing nitrogen protection, raising the system temperature to 80 to 90° C., keeping warm for 4 to 8 hours, cooling the material, filtering, washing, and drying to obtain functionalized fiber; The production method of the inorganic composite flame retardant filler comprises the following steps: Ⅰ: Add mica powder to distilled water, stir to make it dispersed evenly, obtain mica powder suspension, add chitosan to acetic acid solution, stir and mix for 3-5h, then start to drop sodium hydroxide solution, adjust the pH value of the system to 4-5, obtain chitosan solution, then add the chitosan solution to the mica powder suspension, stir at 45-55°C for 6-10h, finally wash with distilled water, filter, and vacuum dry to obtain intercalated modified mica powder; Ⅱ: Add the intercalated modified mica powder to N,N-dimethylformamide, stir to mix evenly, then add hexachlorocyclotriphosphazene, heat to 85-95°C, add pyridine, react for 3-5 hours, after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain an inorganic composite flame retardant filler.
2. The method for producing a PP composite insulation board for cold storage according to claim 1, characterized in that: In step S1, the ultra-high molecular weight polyethylene fiber has a length of 0.2 to 1 mm and a diameter of 8 to 12 μm.
3. The method for producing a PP composite insulation board for cold storage according to claim 1, characterized in that: In step S2, during the plasma treatment, the discharge power is set to 70-90 W, the gas pressure is set to 10-30 Pa, the gas flow rate is set to 20-30 ml / min, and the treatment time is set to 2-4 min.
4. The method for producing a PP composite insulation board for cold storage according to claim 1, characterized in that: In step S3, the mass ratio of the maleic anhydride grafted EPDM rubber to the modified ultra-high molecular weight polyethylene fiber is 1:1-2.
5. The method for producing a PP composite insulation board for cold storage according to claim 1, characterized in that: In step I, the fineness of the mica powder is 3000-4000 mesh.
6. The method for producing a PP composite insulation board for cold storage according to claim 1, characterized in that: In step I, the mass fraction of the acetic acid solution is 1%; the mass fraction of the sodium hydroxide solution is 10%.
7. The method for producing a PP composite insulation board for cold storage according to claim 1, characterized in that: In step (2), the foaming agent is any one of n-pentane, n-hexane or n-heptane; the surfactant is any one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate or hydroxypropyl methylcellulose ether.
8. A PP composite insulation board for cold storage, characterized in that: The method is produced according to claim 1.