A polyurethane adhesive with high adhesion and its application in aluminum-plastic film
By using polyhydroxy DOPO benzoxazine intermediates to prepare polyurethane adhesives, the problems of insufficient bonding performance, heat resistance and flame retardancy of traditional adhesives in aluminum plastic films are solved, and high cross-linking degree and The improved flame retardant effect is suitable for the high-performance packaging needs of modern electronic products.
Patent Information
- Application Number
- CN202410958746.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The bonding performance, heat resistance and flame retardancy of traditional polyurethane adhesives in aluminum-plastic films are insufficient and cannot meet the high requirements of modern electronic products.
Polyhydroxy DOPO benzoxazine intermediate is used as a cross-linking agent and chain extender to prepare polyurethane adhesive through condensation, addition and Mannich reaction, forming a dense network structure with high cross-linking degree and increasing chemical bonds and hydrogen bonds. , improve bonding, heat resistance and flame retardant properties.
Significantly improves the bonding performance, heat resistance and flame retardant performance of polyurethane adhesive, and enhances its service life and safety performance in aluminum-plastic films.
Smart Images

Figure SMS_4 
Figure SMS_5 
Figure SMS_6
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, in particular to a polyurethane adhesive with high adhesion and application thereof in aluminum-plastic films. Background Art
[0002] Aluminum-plastic composite film, referred to as aluminum-plastic film, has good packaging effect and safety performance and has been widely used in electronic products such as mobile phones, laptops, digital cameras, etc. The bonding surface of the aluminum-plastic film packaging material is a decorative layer, which can protect the aluminum film from being scratched. The adhesive used to bond the decorative layer and the aluminum foil layer is a polyurethane adhesive. Polyurethane adhesives have high activity and polarity as well as excellent shear strength and impact resistance. Polyurethane adhesives form a soft-hard transition layer between the substrates, which not only has strong bonding strength but also has relatively excellent buffering and shock absorption functions. However, with the rapid development of science and technology, the bonding performance of traditional polyurethane adhesives can no longer meet the needs. Therefore, how to improve the bonding performance of polyurethane adhesives to increase their service life in aluminum-plastic films has become a hot topic in current research.
[0003] 9,10-Dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) is a flame retardant intermediate with good flame retardant properties and is widely used. For example, the patent with the authorization announcement number CN 110343496 B discloses an epoxidized modified lignin-based polyurethane adhesive. The prepared adhesive has good strength and bonding strength, but does not improve the heat resistance and flame retardant properties of the polyurethane adhesive. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies of the prior art, the present invention provides a polyurethane adhesive with high adhesion and application thereof in aluminum-plastic films. The polyurethane adhesive prepared by the present invention has excellent adhesion performance, heat resistance and flame retardancy.
[0006] (II) Technical solution
[0007] A polyurethane adhesive with high adhesion, the polyurethane adhesive comprising the following raw materials in parts by weight: 100 parts by weight of polycaprolactone diol, 50-80 parts by weight of isophorone diisocyanate, 0.02-0.03 parts by weight of dibutyltin dilaurate, 3-5 parts by weight of 1,4-butanediol, 7-9 parts by weight of 3,5-dimethylolpropionic acid, 2-10 parts by weight of polyhydroxy DOPO benzoxazine intermediate, and 4-10 parts by weight of triethylamine;
[0008] The preparation method of the polyurethane adhesive comprises the following steps:
[0009] Under nitrogen conditions, polycaprolactone diol, isophorone diisocyanate and dibutyltin dilaurate are added to a flask, stirred and mixed evenly, reacted at 45-55°C for 20-50min, heated to 65-75°C, continued to react for 1-3h, then added 1,4-butanediol, 3,5-dihydroxymethylpropionic acid and acetone, heated to 80-85°C, continued chain extension reaction for 2-4h, then added polyhydroxy DOPO benzoxazine intermediate, continued to react for 2-5h, cooled to 35-40°C, added triethylamine for neutralization for 20-40min, added deionized water at room temperature, stirred and emulsified for 20-40min, and distilled under reduced pressure to obtain a polyurethane adhesive with high adhesion.
[0010] Preferably, the preparation method of the polyhydroxy DOPO benzoxazine intermediate is:
[0011] (1) Add p-hydroxybenzaldehyde and tris(2-aminoethyl)amine to ethanol solvent, stir and disperse, heat to 65-80°C, react for 2-6 hours, and after the reaction is completed, cool to room temperature, rotary evaporate, filter, wash with deionized water, and dry to obtain intermediate 1, whose reaction formula is: .
[0012] (2) Add intermediate 1 and DOPO to ethanol solvent, stir and disperse, heat to 75-85°C, react for 2-4 hours, and after the reaction is completed, cool to room temperature, filter, wash with deionized water, and dry to obtain intermediate 2, whose reaction formula is: .
[0013] (3) Under nitrogen conditions, the intermediate 2, 2-(aminomethyl)propane-1,3-diol and formaldehyde are added to a toluene solvent, stirred and dispersed, heated to 90-100°C, and reacted for 4-8 hours. After the reaction is completed, the mixture is distilled under reduced pressure, washed with deionized water, and dried to obtain a polyhydroxy DOPO benzoxazine intermediate, the reaction formula of which is: .
[0014] Preferably, in step (1), the molar ratio of p-hydroxybenzaldehyde to tris(2-aminoethyl)amine is 3-5:1.
[0015] Preferably, in step (2), the molar ratio of intermediate 1 to DOPO is 1:3-5.
[0016] Preferably, in step (3), the molar ratio of the intermediate 2, 2-(aminomethyl)propane-1,3-diol, and formaldehyde is 1:3-4:6-8.
[0017] Preferably, the polyurethane adhesive with high adhesion is used in aluminum-plastic film.
[0018] 3. Beneficial technical effects
[0019] The present invention uses p-hydroxybenzaldehyde and tris (2-aminoethyl) amine as raw materials, undergoes a condensation reaction, obtains an intermediate 1, uses the PH bond in DOPO to react with the Schiff base in the intermediate 1 to obtain an intermediate 2, and then reacts the intermediate 2 with 2-(aminomethyl) propane-1,3-diol and formaldehyde to obtain a polyhydroxy DOPO benzoxazine intermediate. Finally, polycaprolactone diol, isophorone diisocyanate, dibutyltin dilaurate, polyhydroxy DOPO benzoxazine intermediates, etc. are used as raw materials to prepare a polyurethane adhesive with high adhesion.
[0020] The polyhydroxy DOPO benzoxazine intermediate prepared by a series of reactions of the present invention is used as a cross-linking agent to synthesize a polyurethane adhesive. Since it contains more hydroxyl groups, during the reaction, not only more chemical bonds are formed, but also more hydrogen bonds are formed due to the greater electronegativity of oxygen atoms. Therefore, due to the gradual increase of cross-linking sites, the cross-linking degree of the molecular chain is increased, a dense cross-linking network structure is quickly formed, the cohesive energy of the system is increased, and the adhesion of the adhesive is enhanced. In addition, the polyurethane adhesive of the present invention contains more polar groups, which are very easy to form an action force with the groups on the molecular chain, the molecular cross-linking is more compact, and the peel strength is increased.
[0021] The polyhydroxy DOPO benzoxazine intermediate prepared by the present invention contains a benzoxazine structure and a heat-resistant rigid structure, such as a benzene ring, etc., which is added to a polyurethane adhesive. When the temperature rises, the benzoxazine structure is heated, absorbs energy, and undergoes ring-opening crosslinking, thereby further increasing the crosslinking density of the polyurethane adhesive, thereby improving the heat resistance of the polyurethane adhesive.
[0022] The polyurethane adhesive prepared by the present invention contains more phosphorus and nitrogen elements, both of which are flame retardant elements and have excellent flame retardant effects. Adding them to the polyurethane adhesive can improve the flame retardant properties of the polyurethane adhesive. In addition, the polyhydroxy DOPO benzoxazine intermediate prepared by the present invention through condensation, addition, and Mannich reaction has a novel structure and a simple preparation method. The polyurethane adhesive prepared by using it as a chain extender has excellent flame retardant properties, heat resistance, and bonding properties. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Embodiment 1
[0024] (1) Add 0.2 mol of p-hydroxybenzaldehyde and 0.05 mol of tri(2-aminoethyl)amine to 250 mL of ethanol solvent, stir and disperse, heat to 65°C, react for 6 h. After the reaction is completed, cool to room temperature, evaporate, filter, wash with deionized water, and dry to obtain intermediate 1.
[0025] (2) Add 0.02 mol of intermediate 1 and 0.08 mol of DOPO into 200 mL of ethanol solvent, stir and disperse, heat to 80°C, react for 3 h. After the reaction is completed, cool to room temperature, filter, wash with deionized water, and dry to obtain intermediate 2.
[0026] (3) Under nitrogen conditions, 0.1 mol of intermediate 2, 0.35 mol of 2-(aminomethyl)propane-1,3-diol, and 0.7 mol of formaldehyde were added to 100 mL of toluene solvent, stirred and dispersed, and the temperature was raised to 95 °C. The reaction was carried out for 6 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a polyhydroxy DOPO benzoxazine intermediate.
[0027] (4) Under nitrogen conditions, 50 g of polycaprolactone diol, 35 g of isophorone diisocyanate, and 0.012 g of dibutyltin dilaurate were added to a flask, stirred and mixed evenly, reacted at 50 ° C for 30 min, heated to 70 ° C, and continued to react for 2 h. Then, 2 g of 1,4-butanediol, 4 g of 3,5-dihydroxymethylpropionic acid, and 20 mL of acetone were added thereto, and the temperature was raised to 85 ° C. The chain extension reaction was continued for 2 h. Then, 1 g of polyhydroxy DOPO benzoxazine intermediate was added thereto, and the reaction was continued for 4 h. The temperature was lowered to 40 ° C. 4 g of triethylamine was added thereto for neutralization for 30 min. Deionized water was added thereto at room temperature and stirred for emulsification for 40 min. The mixture was distilled under reduced pressure to obtain a polyurethane adhesive with high adhesion. Embodiment 2
[0028] (1) Add 0.15 mol of p-hydroxybenzaldehyde and 0.05 mol of tri(2-aminoethyl)amine to 250 mL of ethanol solvent, stir and disperse, heat to 80°C, react for 5 h. After the reaction is completed, cool to room temperature, rotary evaporate, filter, wash with deionized water, and dry to obtain intermediate 1.
[0029] (2) Add 0.02 mol of intermediate 1 and 0.08 mol of DOPO to 200 mL of ethanol solvent, stir and disperse, heat to 80°C, react for 4 h. After the reaction is completed, cool to room temperature, filter, wash with deionized water, and dry to obtain intermediate 2.
[0030] (3) Under nitrogen conditions, 0.1 mol of intermediate 2, 0.35 mol of 2-(aminomethyl)propane-1,3-diol, and 0.7 mol of formaldehyde were added to 100 mL of toluene solvent, stirred and dispersed, and the temperature was raised to 95°C for 8 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a polyhydroxy DOPO benzoxazine intermediate.
[0031] (4) Under nitrogen conditions, 50 g of polycaprolactone diol, 40 g of isophorone diisocyanate, and 0.015 g of dibutyltin dilaurate were added to a flask, stirred and mixed evenly, reacted at 50 ° C for 40 min, heated to 70 ° C, and continued to react for 2 h. Then, 2 g of 1,4-butanediol, 4.5 g of 3,5-dihydroxymethylpropionic acid, and 20 mL of acetone were added thereto, and the temperature was raised to 85 ° C. The chain extension reaction was continued for 3 h. Then, 2 g of polyhydroxy DOPO benzoxazine intermediate was added thereto, and the reaction was continued for 4 h. The temperature was lowered to 40 ° C. 4 g of triethylamine was added thereto for neutralization for 40 min. Deionized water was added thereto at room temperature and stirred for emulsification for 20 min. The mixture was distilled under reduced pressure to obtain a polyurethane adhesive with high adhesion. Embodiment 3
[0032] (1) Add 0.25 mol of p-hydroxybenzaldehyde and 0.05 mol of tri(2-aminoethyl)amine to 250 mL of ethanol solvent, stir and disperse, heat to 70°C, react for 6 h. After the reaction is completed, cool to room temperature, rotary evaporate, filter, wash with deionized water, and dry to obtain intermediate 1.
[0033] (2) Add 0.02 mol of intermediate 1 and 0.06 mol of DOPO to 200 mL of ethanol solvent, stir and disperse, heat to 80°C, react for 4 h. After the reaction is completed, cool to room temperature, filter, wash with deionized water, and dry to obtain intermediate 2.
[0034] (3) Under nitrogen conditions, 0.1 mol of intermediate 2, 0.35 mol of 2-(aminomethyl)propane-1,3-diol, and 0.8 mol of formaldehyde were added to 100 mL of toluene solvent, stirred and dispersed, and the temperature was raised to 90°C for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a polyhydroxy DOPO benzoxazine intermediate.
[0035] (4) Under nitrogen conditions, 50 g of polycaprolactone diol, 40 g of isophorone diisocyanate, and 0.012 g of dibutyltin dilaurate were added to a flask, stirred and mixed evenly, reacted at 45 ° C for 50 min, heated to 65 ° C, and continued to react for 1 h. Then, 2 g of 1,4-butanediol, 3 g of 3,5-dihydroxymethylpropionic acid, and 20 mL of acetone were added thereto, and the temperature was raised to 85 ° C. The chain extension reaction was continued for 2 h. Then, 3 g of polyhydroxy DOPO benzoxazine intermediate was added thereto, and the reaction was continued for 2 h. The temperature was lowered to 40 ° C. 5 g of triethylamine was added thereto for neutralization for 30 min. Deionized water was added thereto at room temperature and stirred and emulsified for 40 min. The mixture was distilled under reduced pressure to obtain a polyurethane adhesive with high adhesion. Embodiment 4
[0036] (1) Add 0.24 mol of p-hydroxybenzaldehyde and 0.05 mol of tri(2-aminoethyl)amine to 250 mL of ethanol solvent, stir and disperse, heat to 70°C, react for 5 h. After the reaction is completed, cool to room temperature, rotary evaporate, filter, wash with deionized water, and dry to obtain intermediate 1.
[0037] (2) Add 0.02 mol of intermediate 1 and 0.1 mol of DOPO to 200 mL of ethanol solvent, stir and disperse, heat to 75°C, react for 2 h, and after the reaction is completed, cool to room temperature, filter, wash with deionized water, and dry to obtain intermediate 2.
[0038] (3) Under nitrogen conditions, 0.1 mol of intermediate 2, 0.4 mol of 2-(aminomethyl)propane-1,3-diol, and 0.6 mol of formaldehyde were added to 100 mL of toluene solvent, stirred and dispersed, and the temperature was raised to 95°C for 8 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a polyhydroxy DOPO benzoxazine intermediate.
[0039] (4) Under nitrogen conditions, 50 g of polycaprolactone diol, 30 g of isophorone diisocyanate, and 0.015 g of dibutyltin dilaurate were added to a flask, stirred and mixed evenly, reacted at 55 ° C for 20 min, heated to 75 ° C, and continued to react for 2 h. Then, 2.5 g of 1,4-butanediol, 3.5 g of 3,5-dihydroxymethylpropionic acid, and 20 mL of acetone were added thereto, and the temperature was raised to 80 ° C. The chain extension reaction was continued for 3 h. Then, 4 g of polyhydroxy DOPO benzoxazine intermediate was added thereto, and the reaction was continued for 4 h. The temperature was lowered to 35 ° C. 2 g of triethylamine was added thereto for neutralization for 20 min. Deionized water was added thereto at room temperature, stirred and emulsified for 20 min, and distilled under reduced pressure to obtain a polyurethane adhesive with high adhesion. Embodiment 5
[0040] (1) Add 0.2 mol of p-hydroxybenzaldehyde and 0.05 mol of tri(2-aminoethyl)amine to 250 mL of ethanol solvent, stir and disperse, heat to 70°C, react for 4 h. After the reaction is completed, cool to room temperature, rotary evaporate, filter, wash with deionized water, and dry to obtain intermediate 1.
[0041] (2) Add 0.02 mol of intermediate 1 and 0.08 mol of DOPO into 200 mL of ethanol solvent, stir and disperse, heat to 85°C, react for 3 h. After the reaction is completed, cool to room temperature, filter, wash with deionized water, and dry to obtain intermediate 2.
[0042] (3) Under nitrogen conditions, 0.1 mol of intermediate 2, 0.3 mol of 2-(aminomethyl)propane-1,3-diol, and 0.8 mol of formaldehyde were added to 100 mL of toluene solvent, stirred and dispersed, heated to 100 °C, and reacted for 5 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with deionized water, and dried to obtain a polyhydroxy DOPO benzoxazine intermediate.
[0043] (4) Under nitrogen conditions, 50 g of polycaprolactone diol, 25 g of isophorone diisocyanate, and 0.01 g of dibutyltin dilaurate were added to a flask, stirred and mixed evenly, reacted at 50 ° C for 30 min, heated to 70 ° C, and continued to react for 3 h. Then, 1.5 g of 1,4-butanediol, 4.5 g of 3,5-dihydroxymethylpropionic acid, and 20 mL of acetone were added thereto, and the temperature was raised to 85 ° C. The chain extension reaction was continued for 4 h. Then, 5 g of polyhydroxy DOPO benzoxazine intermediate was added thereto, and the reaction was continued for 5 h. The temperature was lowered to 40 ° C. 4 g of triethylamine was added thereto for neutralization for 40 min. Deionized water was added thereto at room temperature, stirred and emulsified for 30 min, and distilled under reduced pressure to obtain a polyurethane adhesive with high adhesion.
[0044] The difference between Comparative Example 1 and Example 1 is that in step (4), no polyhydroxy DOPO benzoxazine intermediate is contained.
[0045] The adhesive was poured onto a 100 mm × 100 mm × 5 mm polytetrafluoroethylene plate and naturally cast into a film, which was then dried at room temperature for 12 h and then placed in an oven at 55° C. for 24 h to obtain an adhesive film.
[0046] Refer to GB / T531.1-2008 and use Shore A hardness tester to test the film hardness.
[0047] With reference to GB / T1040.3-2006, a universal tensile testing machine was used to test the mechanical properties of the film at a test rate of 50 mm / min.
[0048] The polyurethane adhesive was coated on a 20cm×8cm aluminum-plastic film with a coating thickness of 30μm. It was naturally dried and hot pressed at 160°C. The peel strength was tested using an electronic universal testing machine with a tensile rate of 300mm / min.
[0049] Table 1: Mechanical properties test results of various embodiments and comparative examples
[0050]
[0051] It can be seen from the table that the hardness of Examples 1-5 is greater than that of Comparative Example 1 and the tensile strength is greater. This is because Examples 1-5 contain polyhydroxy DOPO benzoxazine intermediates, and the hydroxyl groups contained therein can increase the degree of crosslinking between molecular chains, thereby increasing the hardness and tensile strength thereof. Moreover, as the amount of the polyhydroxy DOPO benzoxazine intermediate increases, the polyhydroxy DOPO benzoxazine intermediate provides more hydroxyl groups to the system, forming a larger crosslinked network structure, further increasing the degree of crosslinking between molecules, and improving the mechanical properties.
[0052] Polarity is an important factor affecting the bonding strength of an adhesive to a polar substrate. The stronger the polarity of the adhesive, the better the polar bonding effect and the greater the peel strength. As can be seen from the table, the peel strength of Examples 1-5 is greater than that of Comparative Example 1. This is because Examples 1-5 contain polyhydroxy DOPO benzoxazine intermediates, and as the amount of polyhydroxy DOPO benzoxazine intermediates increases, the polarity of the polyurethane system increases, the bonding strength increases, and the peel strength increases.
[0053] In a nitrogen atmosphere, a thermogravimetric analyzer was used to perform a thermal weight loss test on the film by heating the temperature from room temperature to 700°C at a heating rate of 10°C / min.
[0054] Table 2: Thermal stability performance test results of various embodiments and comparative examples
[0055]
[0056] As can be seen from the table, the thermal stability of Examples 1-5 is better than that of Comparative Example 1. This is because Examples 1-5 contain benzoxazine structures and heat-resistant rigid groups. When heated, such structures absorb heat, open rings and crosslink, and further improve the thermal stability of the polyurethane adhesive. The polyurethane adhesive prepared by the present invention has excellent thermal stability.
[0057] Refer to GB / T 2406.2-2009 and use the limiting oxygen index tester to test the limiting oxygen index of the material.
[0058] Refer to GB / T 2408-2021 and use a horizontal vertical burning tester to test the vertical burning grade of the material.
[0059] Table 3: Flame retardant performance test results of various embodiments and comparative examples
[0060]
[0061] It can be seen from the table that the flame retardant properties of Examples 1-5 are better than those of Comparative Example 1. This is because Examples 1-5 contain nitrogen and phosphorus flame retardant elements, which have good flame retardant effects, while Comparative Example 1 does not contain these elements, so its flame retardant effect is poor.
[0062] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A polyurethane adhesive with high adhesion, characterized in that: The polyurethane adhesive is prepared from the following raw materials in parts by weight: 100 parts by weight of polycaprolactone diol, 50-80 parts by weight of isophorone diisocyanate, 0.02-0.03 parts by weight of dibutyltin dilaurate, 3-5 parts by weight of 1,4-butanediol, 7-9 parts by weight of 3,5-dimethylolpropionic acid, 2-10 parts by weight of polyhydroxy DOPO benzoxazine intermediate, and 4-10 parts by weight of triethylamine; The preparation method of the polyurethane adhesive comprises the following steps: Under nitrogen conditions, polycaprolactone diol, isophorone diisocyanate, and dibutyltin dilaurate are added to a flask, stirred and mixed evenly, reacted at 45-55° C. for 20-50 minutes, heated to 65-75° C., continued to react for 1-3 hours, and then 1,4-butanediol, 3,5-dihydroxymethylpropionic acid, and acetone are added thereto, heated to 80-85° C., continued chain extension reaction for 2-4 hours, and then polyhydroxy DOPO benzoxazine intermediate is added thereto, continued to react for 2-5 hours, cooled to 35-40° C., triethylamine is added thereto for neutralization for 20-40 minutes, and deionized water is added thereto at room temperature, stirred and emulsified for 20-40 minutes, and distilled under reduced pressure to obtain a polyurethane adhesive with high adhesion; the preparation method of the polyhydroxy DOPO benzoxazine intermediate is as follows: (1) adding p-hydroxybenzaldehyde and tris(2-aminoethyl)amine to an ethanol solvent, wherein the molar ratio of p-hydroxybenzaldehyde to tris(2-aminoethyl)amine is 3-5:1, stirring and dispersing, heating to 65-80° C., reacting for 2-6 hours, cooling to room temperature after the reaction, rotary evaporation, suction filtration, washing with deionized water, and drying to obtain an intermediate 1; (2) adding intermediate 1 and DOPO to an ethanol solvent, wherein the molar ratio of intermediate 1 to DOPO is 1:3-5, stirring and dispersing, heating to 75-85° C., reacting for 2-4 hours, and cooling to room temperature after the reaction, filtering, washing with deionized water, and drying to obtain intermediate 2; (3) Under nitrogen conditions, the intermediate 2, 2-(aminomethyl)propane-1,3-diol and formaldehyde are added to a toluene solvent, wherein the molar ratio of the intermediate 2, 2-(aminomethyl)propane-1,3-diol and formaldehyde is 1:3-4:6-8, and the mixture is stirred and dispersed, and the temperature is raised to 90-100° C. and reacted for 4-8 hours. After the reaction is completed, the mixture is distilled under reduced pressure, washed with deionized water, and dried to obtain a polyhydroxy DOPO benzoxazine intermediate.
2. Application of the highly adhesive polyurethane adhesive according to claim 1 in aluminum-plastic films.