Method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate
By dropping the combination of decomposition precipitant and pre-prepared extraction agent in the lithium battery leaching liquid, the problem of recycling nickel-cobalt-manganese under strong acid environment in the prior art is solved, efficient recycling in a neutral environment is achieved, and waste acid liquid is reduced Generation and process complexity.
Patent Information
- Application Number
- CN202410946863.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The prior art needs to be carried out in a strong acid environment when recycling nickel, cobalt and manganese in waste lithium batteries, resulting in a large amount of waste acid liquid, and the pH requirement of the acid soak liquid is high, which increases the difficulty of the process.
By adding decomposition and decomposition agent to the lithium battery, precipitation and decomposition of iron ions are completed, and gradual extraction is performed using the pre-prepared first, second and third extraction agents, co-solvents and auxiliary separation agents, saponification and strong acids are avoided Assist to achieve efficient extraction.
It realizes efficient recycling of nickel, cobalt and manganese in a neutral environment, reduces the generation of waste acid liquid, simplifies the process, and improves the recovery efficiency of metal ions.
Smart Images

Figure CN118497503B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource recovery, and in particular relates to a method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate. Background Art
[0002] At present, waste lithium batteries contain a large amount of valuable metals and are important secondary resources. The main methods for recovering metal cobalt from waste lithium batteries include precipitation, ion exchange, electrolytic salting out, solvent extraction, etc. Among them, solvent extraction has the advantages of simple operation, high metal recovery rate, and high purity of the obtained product, and is the main means of metal ion recovery at this stage.
[0003] Chinese patent CN116121544A discloses an extraction method for recovering organic metals from waste ternary lithium batteries, the method comprising the following steps: step 1, crushing the recovered waste ternary lithium batteries, grinding the negative electrode thereof to obtain negative electrode powder; step 2, enriching the negative electrode powder with metals by acid leaching, and obtaining an acid leaching solution; step 3, separating the acid leaching solution by using an extractant to obtain an organic phase containing cobalt and manganese metal elements and an aqueous phase containing nickel and lithium metal elements; step 4, stripping the organic phase containing cobalt and manganese metal elements by using a sulfuric acid solution, so that the cobalt and manganese metal elements are transferred to the aqueous phase again; however, in the steps of this method, the acid leaching solution is separated by using an extractant to obtain an organic phase containing cobalt and manganese metal elements and an aqueous phase containing nickel and lithium metal elements, and the separation coefficient of the extractant for cobalt and manganese is low, so that the cobalt and manganese metals cannot be selectively analyzed, which increases the metal elements. Recycling process and difficulty, and Chinese patent CN111334664B discloses a method for comprehensive recovery of valuable metals from ternary lithium battery positive electrode materials based on magnesium salt circulation. The method first mixes magnesium sulfate and ternary lithium battery positive electrode powder in proportion and then roasts them under anaerobic conditions to obtain a roasted material, and the roasted material is filtered through water leaching to obtain a lithium-containing filtrate and a water-leached residue. The lithium-containing filtrate is subjected to alkali precipitation to achieve preferential recovery of lithium, and the water-leached residue is sequentially subjected to acid leaching and extraction to achieve effective separation and recovery of Ni, Co, Mn, and Mg; however, when this method uses P204 and P507 for synergistic extraction, it is necessary to recover the metal elements under a strong acid environment. During extraction, the synergistic operation of P204 and P507 will produce a large amount of waste acid liquid, and the extraction has high requirements on the pH value of the acid leaching liquid. In response to the above problems, we propose a method for synchronously recovering nickel, cobalt, and manganese from waste lithium battery leachate. Summary of the invention
[0004] The purpose of the present invention is to provide a method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate in view of the shortcomings of the prior art.
[0005] At present, when the existing method uses P204 and P507 for synergistic extraction, it is necessary to recover the metal elements under a strong acid environment. During the extraction, the synergistic operation of P204 and P507 will produce a large amount of waste acid liquid. At the same time, the extraction has high requirements on the pH value of the acid leaching solution. In view of the above problems, we propose a method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate. In short, the method includes adding an impurity removal precipitant to the lithium battery leachate to complete the precipitation and impurity removal of iron ions, performing a first extraction on the precipitate residue with a first extractant to obtain a first loaded organic phase and a first aqueous phase, performing a second extraction on the first aqueous phase with a first extractant, a second extractant and an auxiliary separation agent, performing a third extraction on the second aqueous phase with a third extractant, a co-solvent and an auxiliary separation agent, adding a co-solvent and an auxiliary separation agent to the third aqueous phase, performing a fourth extraction on the third aqueous phase, and finally adding a third extractant and an auxiliary separation agent to the fourth aqueous phase, and performing a fifth extraction on the fourth aqueous phase. In the present invention, when extracting the battery leachate, the pre-prepared first extractant, the second extractant, the third extractant, the co-solvent and the auxiliary separation agent cooperate with each other to realize the gradual extraction of the battery leachate, and the extraction system composed of the first extractant, the second extractant and the third extractant can realize the efficient extraction of metal ions without the need for additional saponification and strong acid assistance, and can also avoid the problem that the emulsification degree of the battery leachate during extraction is difficult to control due to saponification, affecting the extraction efficiency.
[0006] The present invention is achieved by providing a method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate, wherein the method comprises:
[0007] Obtaining a lithium battery leachate, wherein the lithium battery leachate contains nickel, cobalt, manganese, iron, copper, and lithium ions, and adding an impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C. to complete precipitation and impurity removal of iron ions to obtain a precipitated residual liquid;
[0008] Obtaining the precipitated residual liquid, pre-preparing a first extractant, a second extractant, a third extractant, a co-solvent and an auxiliary separation agent, performing a first extraction on the precipitated residual liquid with the first extractant to obtain a first loaded organic phase and a first aqueous phase, wherein the first loaded organic phase is a manganese loaded organic phase;
[0009] Performing a second extraction on the first aqueous phase using a first extractant, a second extractant, and an auxiliary separation agent to obtain a second loaded organic phase and a second aqueous phase, wherein the second loaded organic phase is a copper loaded organic phase;
[0010] Obtaining a second aqueous phase, performing a third extraction on the second aqueous phase using a third extractant, a co-solvent, and an auxiliary separation agent to obtain a third loaded organic phase and a third aqueous phase, wherein the third loaded organic phase is a cobalt loaded organic phase;
[0011] Obtain the third aqueous phase, add a co-solvent and an auxiliary separation agent to the third aqueous phase, perform a fourth extraction on the third aqueous phase, mix and stir the third aqueous phase, the co-solvent and the auxiliary separation agent at 80-120° C. for 20-40 minutes to obtain a fourth loaded organic phase and a fourth aqueous phase, wherein the fourth loaded organic phase is a nickel loaded organic phase.
[0012] The fourth aqueous phase is obtained, the third extractant and the auxiliary separation agent are added to the fourth aqueous phase, and the fourth aqueous phase is subjected to a fifth extraction to obtain a fifth loaded organic phase and a fifth aqueous phase, wherein the fifth loaded organic phase is a lithium loaded organic phase.
[0013] Preferably, the method of performing a first extraction on the precipitated residual liquid by using a first extractant specifically comprises:
[0014] The precipitated residual liquid is injected into the extraction tank, and the pH value of the precipitated residual liquid is adjusted by 30% NaOH so that the pH value of the precipitated residual liquid is controlled to be 5.8-6.2;
[0015] Compounding the first extractant, taking the first extractant and the diluent, compounding the first extractant and the diluent so that the volume fraction of the first extractant is 40-45%, and then performing the first extraction with the ratio of the organic phase to the aqueous phase being 1-3:2, the extraction temperature being controlled at 30-45° C., and the extraction time being 40-50 min;
[0016] After the first extraction is completed, the mixture is allowed to stand for 10-15 minutes and then separated to obtain a first loaded organic phase and a first aqueous phase, wherein the first loaded organic phase is a manganese loaded organic phase, and the first loaded organic phase is subjected to five-stage countercurrent water washing with a manganese acid solution containing 0.1-0.4 g / L to obtain a manganese-rich organic phase and a manganese-poor aqueous phase, and the manganese-poor aqueous phase is refluxed to the first aqueous phase;
[0017] Obtaining a manganese-rich organic phase, and stripping the manganese-rich organic phase with an organic acid, wherein the stripping time is 20-30 minutes, the stripping temperature is 30-40° C., and the ratio of the manganese-rich organic phase to the organic acid is controlled to be 8-10:1, to obtain a manganese-rich aqueous phase and a manganese-poor organic phase;
[0018] Obtain a manganese-rich aqueous phase, inject the manganese-rich aqueous phase into a precipitation tank, maintain the temperature of the precipitation tank at 65-70°C, adjust the pH value of the manganese-rich aqueous phase to 5.5-6 with an organic acid, and simultaneously add magnesium carbonate and an auxiliary separation agent into the precipitation tank to precipitate a manganese-enriched product.
[0019] Preferably, the method of performing a second extraction on the first aqueous phase using a first extractant, a second extractant, and an auxiliary separation agent specifically comprises:
[0020] Inject the first aqueous phase into the extraction tank, and adjust the pH value of the first aqueous phase by 30% NaOH so that the pH value of the first aqueous phase is controlled to be 6-6.4;
[0021] Compounding the first extractant, the second extractant, and the auxiliary separation agent, taking the first extractant, the second extractant, the auxiliary separation agent and the diluent, compounding the first extractant, the second extractant, the auxiliary separation agent and the diluent, so that the volume fraction of the first extractant, the second extractant and the auxiliary separation agent is 55-65% of the total volume, and then performing the second extraction with the ratio of the organic phase to the aqueous phase being 4-8:1, the extraction temperature being controlled at 60-75° C., and the extraction time being 20-40 min;
[0022] After the second extraction is completed, the mixture is allowed to stand for 20-25 minutes and then separated to obtain a second loaded organic phase and a second aqueous phase, wherein the second loaded organic phase is a copper loaded organic phase, and the second loaded organic phase is subjected to a three-stage countercurrent water wash with a copper acid solution containing 0.1-0.4 g / L to obtain a copper-rich organic phase and a copper-poor aqueous phase, and the copper-poor aqueous phase is refluxed to the second aqueous phase;
[0023] A copper-rich organic phase is obtained, and an organic acid is used to perform three-stage stripping on the copper-rich organic phase, wherein the stripping time is 40-50 minutes, the stripping temperature is 55-60° C., and the ratio of the copper-rich organic phase to the organic acid is controlled to be 5-6:1, to obtain a copper-rich aqueous phase and a copper-poor organic phase.
[0024] Preferably, the method of performing a third extraction on the second aqueous phase using a third extractant, a co-solvent and an auxiliary separation agent specifically comprises:
[0025] The second aqueous phase is injected into the extraction tank, and the pH value of the second aqueous phase is adjusted by 30% NaOH so that the pH value of the second aqueous phase is controlled to be 7-7.4;
[0026] Compounding a third extractant, a co-solvent and an auxiliary separation agent, taking a third extractant, a co-solvent, an auxiliary separation agent and a diluent, compounding the third extractant, a co-solvent, an auxiliary separation agent and a diluent, so that the volume fraction of the third extractant, the co-solvent and the auxiliary separation agent is 50-55% of the total volume, and then performing a third extraction with a ratio of organic phase to aqueous phase of 2-3:1, an extraction temperature of 70-75° C., and an extraction time of 40-50 min;
[0027] After the third extraction is completed, the mixture is allowed to stand for 20-25 minutes and then separated to obtain a third loaded organic phase and a third aqueous phase, wherein the third loaded organic phase is a cobalt loaded organic phase, and the third loaded organic phase is subjected to five-stage countercurrent water washing with a cobalt acid solution containing 0.5-1 g / L to obtain a cobalt-rich organic phase and a cobalt-depleted aqueous phase, and the cobalt-depleted aqueous phase is refluxed to the third aqueous phase;
[0028] A cobalt-rich organic phase is obtained, and the cobalt-rich organic phase is subjected to three-stage stripping with an organic acid, wherein the stripping time is 15-20 minutes, the stripping temperature is 75-80° C., and the ratio of the cobalt-rich organic phase to the organic acid is controlled to be 2:1, to obtain a cobalt-rich aqueous phase and a cobalt-poor organic phase.
[0029] Preferably, the impurity removal precipitant comprises the following raw materials in parts by weight: 10-20 parts of magnesium carbonate, 15-25 parts of magnesium oxide, 10-15 parts of hydrophilic rhamnolipid, 20-30 parts of hydroxysulfobetaine, and 20-40 parts of ethanol;
[0030] Wherein, the preparation method of the impurity removal precipitant specifically comprises:
[0031] Obtain rhamnolipid, dissolve the rhamnolipid in ethanol at 60-70° C., add 2% by volume concentrated sulfuric acid to the rhamnolipid solution, react for 1-2 hours, then adjust the pH value of the rhamnolipid solution to 6.8-7.5 with 30% NaOH, centrifuge the rhamnolipid solution, and obtain hydrophilic rhamnolipid;
[0032] Sodium 3-chloro-2-hydroxypropane sulfonate is synthesized by a ring-opening reaction of sodium bisulfite and epichlorohydrin, and then dodecylbenzyl chloride is reacted with dimethylolamine to obtain dodecylbenzyl dimethanolamine, and dodecylbenzyl dimethanolamine and sodium 3-chloro-2-hydroxypropane sulfonate are reacted in the presence of a palladium catalyst at 120°C for 2h to prepare hydroxysulfobetaine;
[0033] Take the prepared hydroxysulfobetaine and hydrophilic rhamnolipid, mix the hydroxysulfobetaine and hydrophilic rhamnolipid with ethanol, and heat and stir at 60° C.;
[0034] After the hydroxysulfobetaine and the hydrophilic rhamnolipid are mixed, the mixture is cooled to room temperature, and magnesium carbonate, magnesium oxide, the hydroxysulfobetaine and the hydrophilic rhamnolipid are mixed to obtain an impurity removal precipitant.
[0035] Preferably, the method of adding a de-impurity precipitant to the lithium battery leachate to complete the precipitation and de-impurity of iron ions specifically comprises:
[0036] Obtain lithium battery leachate, add ethanol to the lithium battery leachate, mix by ultrasonication for 30 minutes, and then place in a water bath at 65° C. for 20 minutes;
[0037] Add the pre-prepared impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C., while maintaining a stirring speed of 200-250 r / min, and stop adding the impurity removal precipitant when the pH value of the lithium battery leachate reaches 5.2-5.5;
[0038] The stirring speed was reduced to 100-150 r / min, and after aging for 50 minutes, the stirring was stopped. After standing for 20 minutes, the lithium battery leachate was filtered and separated to obtain precipitated iron slag and precipitated residual liquid.
[0039] Preferably, the first extractant comprises the following raw materials in parts by weight: 1-10 parts of coconut glucoside, 2-15 parts of octylphenol polyoxyethylene ether, 1-20 parts of cinnamic acid, - 10-20 parts of hydroxy acid;
[0040] The second extractant comprises the following raw materials in parts by weight: 1-7 parts of coconut glucoside, 12-25 parts of octylphenol polyoxyethylene ether, and 10-20 parts of diacetyl oxime;
[0041] The third extractant comprises the following raw materials in parts by weight: 10-20 parts of octylphenol polyoxyethylene ether, 1-9 parts of cinnamic acid, unsaturated -hydroxy acid 3-20 parts, dimethylglyoxime 1-10 parts, pyridine-3,5-dicarboxylate 1-10 parts, gemini sulfonate 10-30 parts.
[0042] Preferably, the method for preparing the third extractant specifically comprises:
[0043] Take toluene and butene, put them into the reactor, carry out nuclear olefination reaction, generate 1,3-dimethyl-4-vinylbenzene, and then cinnamic acid, unsaturated -Hydroxy acid is put into the reactor and the reactor is heated at a temperature of 70-80°C;
[0044] The obtained 1,3-dimethyl-4-vinylbenzene is reacted with catechol to generate an intermediate of octylphenol polyoxyethylene ether, and then the octylphenol polyoxyethylene ether intermediate is subjected to a dehydration reaction to obtain octylphenol polyoxyethylene ether;
[0045] Mix dimethylglyoxime and pyridine-3,5-dicarboxylate, then add tetrahydrofuran to the mixture, mix at 80-90° C. for 2-3 hours, wash the mixture, evaporate the solvent, and vacuum dry at 90-100° C. for 3 hours to obtain an extractant intermediate;
[0046] Taking sodium 2-chloroethylsulfonate, 1,3-propylenediamine and epichlorohydrin as raw materials for synthesizing gemini sulfonate, using sodium 2-chloroethylsulfonate as a substituent, carrying out a substitution reaction on 1,3-propylenediamine with the assistance of a palladium catalyst, then adding epichlorohydrin for a ring-opening reaction to obtain a sulfonate intermediate, and then adding sulfuric acid for a sulfonation reaction to obtain gemini sulfonate;
[0047] Octylphenol polyoxyethylene ether, gemini sulfonate and the extractant intermediate are mixed in a nitrogen-deoxygenated reactor, and then aviation kerosene is added and mixed at 65-70° C. for 3 hours to obtain a third extractant.
[0048] Preferably, the co-solvent comprises the following raw materials in weight percentage:
[0049] Propylene glycol: 10%
[0050] Glycol: 5%
[0051] Tridecylmethylammonium bromide: 15%
[0052] Tetrabutylammonium hydrogen sulfate: 30%
[0053] Eucalyptus oil: 20%
[0054] L-Menthol: 20%.
[0055] The auxiliary separation agent is a mixture of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate, and the mass ratio of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate is 1:2:1.
[0056] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0057] In the present invention, when extracting the battery leachate, the pre-prepared first extractant, the second extractant, the third extractant, the co-solvent and the auxiliary separation agent cooperate with each other to realize the gradual extraction of the battery leachate, and the extraction system composed of the first extractant, the second extractant and the third extractant can realize the efficient extraction of metal ions without the need for additional saponification and strong acid assistance, and can also avoid the problem that the emulsification degree of the battery leachate during extraction is difficult to control due to saponification, affecting the extraction efficiency.
[0058] In the embodiment of the present invention, an impurity removal precipitant and a preparation method for efficiently precipitating iron ions in a lithium battery leachate are provided. Compared with the prior art, the raw materials of the impurity removal precipitant are composed of magnesium carbonate, magnesium oxide, hydrophilic rhamnolipid, hydroxysulfonyl betaine, and ethanol. The hydrophilic rhamnolipid, hydroxysulfonyl betaine, and ethanol act on magnesium carbonate and magnesium oxide, which can ensure the effect of magnesium carbonate and magnesium oxide as neutralizers to precipitate and adsorb iron ions, and can also avoid nickel, cobalt, and manganese ions from adsorbing iron precipitates, thereby achieving the stripping of nickel, cobalt, and manganese ions from iron precipitates, thereby improving the recovery efficiency of nickel, cobalt, and manganese ions.
[0059] In the embodiment of the present invention, during extraction, the extraction efficiency of nickel and cobalt ions can be improved by adding a co-solvent and an auxiliary separation agent to the battery leachate. At the same time, the co-solvent can be fully miscible with the third extractant, so that the co-solvent can cooperate with the third extractant to perform the extraction operation, and the auxiliary separation agent can ensure that the organic phase is evenly dispersed in the aqueous phase, thereby improving the extraction and separation speed of the nickel and cobalt ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 The present invention provides a schematic diagram of the implementation process of the method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate.
[0061] Figure 2 The present invention is a schematic diagram of the process for preparing the impurity-removing precipitant provided by the present invention.
[0062] Figure 3 The present invention provides a schematic flow chart of a method for implementing the precipitation and impurity removal of iron ions by adding an impurity removal precipitant to a lithium battery leachate.
[0063] Figure 4 A schematic diagram of the process of implementing the first extraction of the precipitated residual liquid by the first extractant is shown.
[0064] Figure 5 The schematic diagram shows the process of implementing the second extraction of the first aqueous phase by using the first extractant, the second extractant and the auxiliary separation agent.
[0065] Figure 6 A schematic diagram of the process for implementing the third extraction of the second aqueous phase using a third extractant, a co-solvent and an auxiliary separation agent is shown.
[0066] Figure 7 It is a schematic flow chart of the preparation method of the third extractant provided by the present invention.
[0067] Figure 8 This is a graph of the test results of precipitated iron provided by the present invention.
[0068] Fig. 9 It is a graph showing the interfacial tension and contact angle test results of the third extractant prepared in Examples 1-5 of the present invention and Comparative Examples 1-5.
[0069] Fig.10 The test results of cobalt ion extraction of Examples 1-5 of the present invention and Comparative Examples 1-5 are shown.
[0070] Fig.11 The test results of nickel ion extraction of Examples 1-5 of the present invention and Comparative Examples 1-5 are shown.
[0071] Fig.12 The graphs show the test results of lithium ion extraction of Examples 1-5 of the present invention and Comparative Examples 1-5. DETAILED DESCRIPTION
[0072] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.
[0073] At present, when the existing method uses P204 and P507 for synergistic extraction, it is necessary to recover the metal elements under a strong acid environment. During the extraction, the synergistic operation of P204 and P507 will produce a large amount of waste acid liquid. At the same time, the extraction has high requirements on the pH value of the acid leaching solution. In view of the above problems, we propose a method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate. In short, the method includes adding an impurity removal precipitant to the lithium battery leachate to complete the precipitation and impurity removal of iron ions, performing a first extraction on the precipitate residue with a first extractant to obtain a first loaded organic phase and a first aqueous phase, performing a second extraction on the first aqueous phase with a first extractant, a second extractant and an auxiliary separation agent, performing a third extraction on the second aqueous phase with a third extractant, a co-solvent and an auxiliary separation agent, adding a co-solvent and an auxiliary separation agent to the third aqueous phase, performing a fourth extraction on the third aqueous phase, and finally adding a third extractant and an auxiliary separation agent to the fourth aqueous phase, and performing a fifth extraction on the fourth aqueous phase. In the present invention, when extracting the battery leachate, the pre-prepared first extractant, the second extractant, the third extractant, the co-solvent and the auxiliary separation agent cooperate with each other to realize the gradual extraction of the battery leachate, and the extraction system composed of the first extractant, the second extractant and the third extractant can realize the efficient extraction of metal ions without the need for additional saponification and strong acid assistance, and can also avoid the problem that the emulsification degree of the battery leachate during extraction is difficult to control due to saponification, affecting the extraction efficiency.
[0074] Example 1
[0075] The embodiment of the present invention provides a method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate. Figure 1 The schematic diagram of the process of realizing the simultaneous recovery of nickel, cobalt and manganese from waste lithium battery leachate is shown, wherein the simultaneous recovery of nickel, cobalt and manganese from waste lithium battery leachate specifically includes:
[0076] Step S10, obtaining a lithium battery leachate, wherein the lithium battery leachate contains nickel, cobalt, manganese, iron, copper, and lithium ions, and adding an impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C. to complete precipitation and impurity removal of iron ions to obtain a precipitated residual liquid.
[0077] It should be noted that the lithium battery leachate can be immersed in a strong acid, and one or more combinations of nitric acid, hydrochloric acid, and sulfuric acid are used for leaching during immersion, which can ensure the leaching rate of metal ions. At the same time, it can also be immersed under pressure at 120-150°C to further improve the recovery rate of metal ions. Table 1 shows the content of metal ions in the battery leachate.
[0078] Table 1
[0079]
[0080] Step S20, obtaining the precipitated residual liquid, pre-preparing a first extractant, a second extractant, a third extractant, a co-solvent and an auxiliary separation agent, performing a first extraction on the precipitated residual liquid with the first extractant to obtain a first loaded organic phase and a first aqueous phase, wherein the first loaded organic phase is a manganese loaded organic phase;
[0081] Step S30, performing a second extraction on the first aqueous phase using a first extractant, a second extractant, and an auxiliary separation agent to obtain a second loaded organic phase and a second aqueous phase, wherein the second loaded organic phase is a copper loaded organic phase;
[0082] Step S40, obtaining a second aqueous phase, performing a third extraction on the second aqueous phase using a third extractant, a co-solvent and an auxiliary separation agent to obtain a third loaded organic phase and a third aqueous phase, wherein the third loaded organic phase is a cobalt loaded organic phase;
[0083] Step S50, obtaining the third aqueous phase, adding a co-solvent and an auxiliary separation agent to the third aqueous phase, performing a fourth extraction on the third aqueous phase, mixing and stirring the third aqueous phase, the co-solvent and the auxiliary separation agent at 80-120°C for 20-40 minutes to obtain a fourth loaded organic phase and a fourth aqueous phase, wherein the fourth loaded organic phase is a nickel loaded organic phase.
[0084] Step S60, obtaining a fourth aqueous phase, adding a third extractant and an auxiliary separation agent to the fourth aqueous phase, performing a fifth extraction on the fourth aqueous phase to obtain a fifth loaded organic phase and a fifth aqueous phase, wherein the fifth loaded organic phase is a lithium loaded organic phase.
[0085] The impurity removal precipitant comprises the following raw materials in parts by weight: 10 parts of magnesium carbonate, 15 parts of magnesium oxide, 10 parts of hydrophilic rhamnolipid, 30 parts of hydroxysulfobetaine, and 40 parts of ethanol.
[0086] Among them, Figure 2As shown, the method for preparing the impurity-removing precipitant specifically comprises:
[0087] Step S101, obtaining rhamnolipid, dissolving the rhamnolipid in ethanol at 60-70° C., adding 2% by volume concentrated sulfuric acid to the rhamnolipid solution, reacting for 1-2 hours, then adjusting the pH value of the rhamnolipid solution to 6.8-7.5 with 30% NaOH, and centrifuging the rhamnolipid solution to obtain hydrophilic rhamnolipid;
[0088] Step S102, synthesizing sodium 3-chloro-2-hydroxypropane sulfonate by ring-opening reaction of sodium bisulfite and epichlorohydrin, then reacting dodecylbenzyl chloride with dimethylolamine to obtain dodecylbenzyl dimethanolamine, and reacting dodecylbenzyl dimethanolamine and sodium 3-chloro-2-hydroxypropane sulfonate under a palladium catalyst at 120° C. for 2 h to prepare hydroxysulfobetaine;
[0089] Step S103, taking the prepared hydroxysulfobetaine and hydrophilic rhamnolipid, mixing the hydroxysulfobetaine and hydrophilic rhamnolipid with ethanol, and heating and stirring at 60° C.;
[0090] Step S104, after the hydroxysulfobetaine and the hydrophilic rhamnolipid are mixed, they are cooled to room temperature, and magnesium carbonate, magnesium oxide, hydroxysulfobetaine and the hydrophilic rhamnolipid are mixed to obtain an impurity removal precipitant.
[0091] In the embodiment of the present invention, an impurity removal precipitant and a preparation method for efficiently precipitating iron ions in a lithium battery leachate are provided. Compared with the prior art, the raw materials of the impurity removal precipitant are composed of magnesium carbonate, magnesium oxide, hydrophilic rhamnolipid, hydroxysulfonyl betaine, and ethanol. The hydrophilic rhamnolipid, hydroxysulfonyl betaine, and ethanol act on magnesium carbonate and magnesium oxide, which can ensure the effect of magnesium carbonate and magnesium oxide as neutralizers to precipitate and adsorb iron ions, and can also avoid nickel, cobalt, and manganese ions from adsorbing iron precipitates, thereby achieving the stripping of nickel, cobalt, and manganese ions from iron precipitates, thereby improving the recovery efficiency of nickel, cobalt, and manganese ions.
[0092] In this embodiment, if Figure 3 As shown, the method of adding a de-impurity precipitant to the lithium battery leachate to complete the precipitation and de-impurity of iron ions specifically includes:
[0093] Step S501, obtaining a lithium battery leachate, adding ethanol to the lithium battery leachate, ultrasonically mixing for 30 minutes, and then placing the mixture in a 65° C. water bath for 20 minutes;
[0094] Step S502, adding a pre-prepared impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C., while maintaining a stirring speed of 200-250 r / min, and stopping the addition of the impurity removal precipitant when the pH value of the lithium battery leachate is 5.2-5.5;
[0095] Step S503, reducing the stirring speed to 100-150r / min, aging for 50 minutes, stopping the stirring, standing for 20 minutes, filtering and separating the lithium battery leachate to obtain precipitated iron slag and precipitated residual liquid.
[0096] In the embodiment of the present invention, the first extractant comprises the following raw materials in parts by weight: 1 part of coconut glucoside, 2 parts of octylphenol polyoxyethylene ether, 1 part of cinnamic acid, 1 part of unsaturated - 10 parts of hydroxy acid;
[0097] The second extractant comprises the following raw materials in parts by weight: 1 part of coconut glucoside, 12 parts of octylphenol polyoxyethylene ether, and 10 parts of diacetyl oxime;
[0098] The third extractant comprises the following raw materials in parts by weight: 10 parts of octylphenol polyoxyethylene ether, 1 part of cinnamic acid, -hydroxy acid 3 parts, dimethylglyoxime 1 part, pyridine-3,5-dicarboxylate 1 part, gemini sulfonate 10 parts.
[0099] It should be noted that the first extractant, the second extractant and the third extractant are all neutral / slightly acidic extractants. Compared with the extractants in the prior art, the first extractant, the second extractant and the third extractant provided by the present invention have lower requirements on the extraction environment. Therefore, a large amount of acid waste liquid will not be generated during extraction, thereby ensuring the environmental protection and energy saving of the extraction process.
[0100] In the embodiment of the present invention, the first extractant is colorless and has a density of 0.8-0.85 g / cm 3 , viscosity is 0.08-0.15mPa·s, freezing point is -45℃, the second extractant is light yellow, and its density is 2.1-2.5g / cm 3 , viscosity is 1.5-2mPa·s, freezing point is -35°C, the third extractant is amber, and its density is 1.5-1.75g / cm 3 , viscosity is 4.5-5.1mPa·s, and freezing point is -38℃.
[0101] In this embodiment, if Figure 7 As shown, the preparation method of the third extractant specifically comprises:
[0102] Step S601, taking toluene and butene, putting the toluene and butene into a reactor, performing a nuclear olefination reaction to generate 1,3-dimethyl-4-vinylbenzene, and then reacting cinnamic acid, unsaturated -Hydroxy acid is put into the reaction kettle, and the reaction kettle is heated, and the heating temperature is maintained at 70-80°C; in this embodiment, the heating time of the reaction kettle can be 20-30 minutes.
[0103] Step S602, reacting the obtained 1,3-dimethyl-4-vinylbenzene with catechol to generate an intermediate of octylphenol polyoxyethylene ether, and then dehydrating the intermediate of octylphenol polyoxyethylene ether to obtain octylphenol polyoxyethylene ether;
[0104] Step S603, mixing dimethylglyoxime and pyridine-3,5-dicarboxylate, then adding tetrahydrofuran to the mixture, mixing at 80-90° C. for 2-3 hours, washing the mixture, evaporating the solvent, and vacuum drying at 90-100° C. for 3 hours to obtain an extractant intermediate;
[0105] Step S604, taking sodium 2-chloroethyl sulfonate, 1,3-propylenediamine, and epichlorohydrin as raw materials for synthesizing gemini sulfonate, using sodium 2-chloroethyl sulfonate as a substituent, subjecting 1,3-propylenediamine to a substitution reaction with the aid of a palladium catalyst, then adding epichlorohydrin to carry out a ring-opening reaction to obtain a sulfonate intermediate, and then adding sulfuric acid to carry out a sulfonation reaction to obtain gemini sulfonate;
[0106] In the embodiment of the present invention, the activity of the third extractant can be improved by preparing the gemini sulfonate, so that the third extractant can be fully miscible with the co-solvent, and the co-solvent can cooperate with the third extractant to perform extraction.
[0107] Step S605, octylphenol polyoxyethylene ether, gemini sulfonate and the extractant intermediate are mixed in a nitrogen-deoxygenated reactor, and then aviation kerosene is added, and mixed at 65-70° C. for 3 hours to obtain a third extractant.
[0108] In an embodiment of the present invention, the co-solvent includes the following raw materials in weight percentage: propylene glycol: 10%, glycol: 5%, tridecylmethylammonium bromide: 15%, tetrabutylammonium hydrogen sulfate: 30%, eucalyptus oil: 20%, and L-menthol: 20%.
[0109] The auxiliary separation agent is a mixture of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate, and the mass ratio of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate is 1:2:1.
[0110] In the embodiment of the present invention, during extraction, the extraction efficiency of nickel and cobalt ions can be improved by adding a co-solvent and an auxiliary separation agent to the battery leachate. At the same time, the co-solvent can be fully miscible with the third extractant, so that the co-solvent can cooperate with the third extractant to perform the extraction operation, and the auxiliary separation agent can ensure that the organic phase is evenly dispersed in the aqueous phase, thereby improving the extraction and separation speed of the nickel and cobalt ions.
[0111] In the present invention, when extracting the battery leachate, the pre-prepared first extractant, the second extractant, the third extractant, the co-solvent and the auxiliary separation agent cooperate with each other to realize the gradual extraction of the battery leachate, and the extraction system composed of the first extractant, the second extractant and the third extractant can realize the efficient extraction of metal ions without the need for additional saponification and strong acid assistance, and can also avoid the problem that the emulsification degree of the battery leachate during extraction is difficult to control due to saponification, affecting the extraction efficiency.
[0112] Example 2
[0113] The embodiment of the present invention provides a method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate, wherein the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is the same as that in Example 1.
[0114] The impurity-removing precipitant comprises the following raw materials in parts by weight: 20 parts of magnesium carbonate, 25 parts of magnesium oxide, 15 parts of hydrophilic rhamnolipid, 30 parts of hydroxysulfobetaine, and 40 parts of ethanol.
[0115] In this embodiment, if Figure 3 As shown, the method of adding a de-impurity precipitant to the lithium battery leachate to complete the precipitation and de-impurity of iron ions specifically includes:
[0116] Step S501, obtaining a lithium battery leachate, adding ethanol to the lithium battery leachate, ultrasonically mixing for 30 minutes, and then placing the mixture in a 65° C. water bath for 20 minutes;
[0117] Step S502, adding a pre-prepared impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C., while maintaining a stirring speed of 200-250 r / min, and stopping the addition of the impurity removal precipitant when the pH value of the lithium battery leachate is 5.2-5.5;
[0118] Step S503, reducing the stirring speed to 100-150r / min, aging for 50 minutes, stopping the stirring, standing for 20 minutes, filtering and separating the lithium battery leachate to obtain precipitated iron slag and precipitated residual liquid.
[0119] In the embodiment of the present invention, the first extractant comprises the following raw materials in parts by weight: 10 parts of coconut glucoside, 15 parts of octylphenol polyoxyethylene ether, 20 parts of cinnamic acid, 20 parts of unsaturated - 20 parts of hydroxy acid;
[0120] The second extractant comprises the following raw materials in parts by weight: 7 parts of coconut glucoside, 25 parts of octylphenol polyoxyethylene ether, and 20 parts of diacetyl oxime;
[0121] The third extractant comprises the following raw materials in parts by weight: 20 parts of octylphenol polyoxyethylene ether, 9 parts of cinnamic acid, -hydroxy acid 20 parts, dimethylglyoxime 10 parts, pyridine-3,5-dicarboxylate 10 parts, gemini sulfonate 30 parts.
[0122] In an embodiment of the present invention, the co-solvent includes the following raw materials in weight percentage: propylene glycol: 10%, glycol: 5%, tridecylmethylammonium bromide: 15%, tetrabutylammonium hydrogen sulfate: 30%, eucalyptus oil: 20%, and L-menthol: 20%.
[0123] The auxiliary separation agent is a mixture of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate, and the mass ratio of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate is 1:2:1.
[0124] Example 3
[0125] The embodiment of the present invention provides a method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate, wherein the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is the same as that in Example 1.
[0126] The impurity removal precipitant comprises the following raw materials in parts by weight: 11 parts of magnesium carbonate, 16 parts of magnesium oxide, 12 parts of hydrophilic rhamnolipid, 22 parts of hydroxysulfobetaine, and 23 parts of ethanol;
[0127] In this embodiment, if Figure 3 As shown, the method of adding a de-impurity precipitant to the lithium battery leachate to complete the precipitation and de-impurity of iron ions specifically includes:
[0128] Step S501, obtaining a lithium battery leachate, adding ethanol to the lithium battery leachate, ultrasonically mixing for 30 minutes, and then placing the mixture in a 65° C. water bath for 20 minutes;
[0129] Step S502, adding a pre-prepared impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C., while maintaining a stirring speed of 200-250 r / min, and stopping the addition of the impurity removal precipitant when the pH value of the lithium battery leachate is 5.2-5.5;
[0130] Step S503, reducing the stirring speed to 100-150r / min, aging for 50 minutes, stopping the stirring, standing for 20 minutes, filtering and separating the lithium battery leachate to obtain precipitated iron slag and precipitated residual liquid.
[0131] In the embodiment of the present invention, the first extractant comprises the following raw materials in parts by weight: 2 parts of coconut glucoside, 3 parts of octylphenol polyoxyethylene ether, 2 parts of cinnamic acid, and 2 parts of unsaturated - 12 parts of hydroxy acid;
[0132] The second extractant comprises the following raw materials in parts by weight: 2 parts of coconut glucoside, 14 parts of octylphenol polyoxyethylene ether, and 11 parts of diacetyl oxime;
[0133] The third extractant comprises the following raw materials in parts by weight: 12 parts of octylphenol polyoxyethylene ether, 2 parts of cinnamic acid, and unsaturated -hydroxy acid 4 parts, dimethylglyoxime 2 parts, pyridine-3,5-dicarboxylate 2 parts, gemini sulfonate 13 parts.
[0134] In an embodiment of the present invention, the co-solvent includes the following raw materials in weight percentage: propylene glycol: 10%, glycol: 5%, tridecylmethylammonium bromide: 15%, tetrabutylammonium hydrogen sulfate: 30%, eucalyptus oil: 20%, and L-menthol: 20%.
[0135] The auxiliary separation agent is a mixture of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate, and the mass ratio of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate is 1:2:1.
[0136] Example 4
[0137] The embodiment of the present invention provides a method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate, wherein the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is the same as that in Example 1.
[0138] The impurity removal precipitant comprises the following raw materials in parts by weight: 18 parts of magnesium carbonate, 22 parts of magnesium oxide, 14 parts of hydrophilic rhamnolipid, 28 parts of hydroxysulfobetaine, and 38 parts of ethanol;
[0139] In this embodiment, if Figure 3 As shown, the method of adding a de-impurity precipitant to the lithium battery leachate to complete the precipitation and de-impurity of iron ions specifically includes:
[0140] Step S501, obtaining a lithium battery leachate, adding ethanol to the lithium battery leachate, ultrasonically mixing for 30 minutes, and then placing the mixture in a 65° C. water bath for 20 minutes;
[0141] Step S502, adding a pre-prepared impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C., while maintaining a stirring speed of 200-250 r / min, and stopping the addition of the impurity removal precipitant when the pH value of the lithium battery leachate is 5.2-5.5;
[0142] Step S503, reducing the stirring speed to 100-150r / min, aging for 50 minutes, stopping the stirring, standing for 20 minutes, filtering and separating the lithium battery leachate to obtain precipitated iron slag and precipitated residual liquid.
[0143] In the embodiment of the present invention, the first extractant comprises the following raw materials in parts by weight: 9 parts of coconut glucoside, 14 parts of octylphenol polyoxyethylene ether, 18 parts of cinnamic acid, 18 parts of unsaturated - 18 parts of hydroxy acid;
[0144] The second extractant comprises the following raw materials in parts by weight: 6 parts of coconut glucoside, 22 parts of octylphenol polyoxyethylene ether, and 18 parts of diacetyl oxime;
[0145] The third extractant comprises the following raw materials in parts by weight: 18 parts of octylphenol polyoxyethylene ether, 9 parts of cinnamic acid, -hydroxy acid 20 parts, dimethylglyoxime 1 part, pyridine-3,5-dicarboxylate 1 part, gemini sulfonate 30 parts.
[0146] In an embodiment of the present invention, the co-solvent includes the following raw materials in weight percentage: propylene glycol: 10%, glycol: 5%, tridecylmethylammonium bromide: 15%, tetrabutylammonium hydrogen sulfate: 30%, eucalyptus oil: 20%, and L-menthol: 20%.
[0147] The auxiliary separation agent is a mixture of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate, and the mass ratio of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate is 1:2:1.
[0148] Example 5
[0149] The embodiment of the present invention provides a method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate, wherein the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is the same as that in Example 1.
[0150] The impurity removal precipitant comprises the following raw materials in parts by weight: 15 parts of magnesium carbonate, 20 parts of magnesium oxide, 12 parts of hydrophilic rhamnolipid, 23 parts of hydroxysulfobetaine, and 30 parts of ethanol;
[0151] In this embodiment, if Figure 3As shown, the method of adding a de-impurity precipitant to the lithium battery leachate to complete the precipitation and de-impurity of iron ions specifically includes:
[0152] Step S501, obtaining a lithium battery leachate, adding ethanol to the lithium battery leachate, ultrasonically mixing for 30 minutes, and then placing the mixture in a 65° C. water bath for 20 minutes;
[0153] Step S502, adding a pre-prepared impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C., while maintaining a stirring speed of 200-250 r / min, and stopping the addition of the impurity removal precipitant when the pH value of the lithium battery leachate is 5.2-5.5;
[0154] Step S503, reducing the stirring speed to 100-150r / min, aging for 50 minutes, stopping the stirring, standing for 20 minutes, filtering and separating the lithium battery leachate to obtain precipitated iron slag and precipitated residual liquid.
[0155] The impurity removal precipitant prepared in Examples 1-5 of the present invention and the commercially available neutralizer (raw materials are magnesium carbonate and magnesium oxide) were used to precipitate iron in the lithium battery leachate. Table 2 and Figure 8 Precipitated iron test results are shown.
[0156] Table 2
[0157]
[0158] From Table 2 and Figure 8 It can be concluded that, compared with commercially available products, the impurity removal precipitant prepared in Examples 1-5 of the present invention can also achieve efficient precipitation of iron ions under weak acidity conditions. At the same time, when precipitating iron ions, it can also inhibit the adsorption and precipitation of other metal ions, thereby improving the recovery efficiency of metal ions.
[0159] In the embodiment of the present invention, the first extractant comprises the following raw materials in parts by weight: 5 parts of coconut glucoside, 10 parts of octylphenol polyoxyethylene ether, 11 parts of cinnamic acid, and 10 parts of unsaturated - 15 parts of hydroxy acid;
[0160] The second extractant comprises the following raw materials in parts by weight: 3 parts of coconut glucoside, 20 parts of octylphenol polyoxyethylene ether, and 20 parts of diacetyl oxime;
[0161] The third extractant comprises the following raw materials in parts by weight: 15 parts of octylphenol polyoxyethylene ether, 4 parts of cinnamic acid, -hydroxy acid 12 parts, dimethylglyoxime 5 parts, pyridine-3,5-dicarboxylate 6 parts, gemini sulfonate 15 parts.
[0162] In an embodiment of the present invention, the co-solvent includes the following raw materials in weight percentage: propylene glycol: 10%, glycol: 5%, tridecylmethylammonium bromide: 15%, tetrabutylammonium hydrogen sulfate: 30%, eucalyptus oil: 20%, and L-menthol: 20%.
[0163] The auxiliary separation agent is a mixture of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate, and the mass ratio of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate is 1:2:1.
[0164] Comparative Example 1
[0165] In this comparative example, the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is similar to that in Example 5. The difference from Example 5 is that the third extractant raw material does not contain octylphenol polyoxyethylene ether, and the third extractant includes the following raw materials in parts by weight: 1 part of cinnamic acid, 1 part of unsaturated -hydroxy acid 3 parts, dimethylglyoxime 1 part, pyridine-3,5-dicarboxylate 1 part, gemini sulfonate 10 parts.
[0166] Comparative Example 2
[0167] In this comparative example, the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is similar to that in Example 5. The difference from Example 5 is that the third extractant raw material does not contain pyridine-3,5-dicarboxylate, and the third extractant includes the following raw materials in parts by weight: 12 parts of octylphenol polyoxyethylene ether, 4 parts of cinnamic acid, and unsaturated -10 parts of hydroxy acid, 8 parts of diacetyl oxime, and 30 parts of gemini sulfonate.
[0168] Comparative Example 3
[0169] In this comparative example, the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is similar to that in Example 5. The difference from Example 5 is that the third extractant raw material does not contain gemini sulfonate, and the third extractant includes the following raw materials in parts by weight: 20 parts of octylphenol polyoxyethylene ether, 9 parts of cinnamic acid, and unsaturated -hydroxy acid 12 parts, dimethylglyoxime 8 parts, pyridine-3,5-dicarboxylate 10 parts.
[0170] Comparative Example 4
[0171] In this comparative example, the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is similar to that in Example 5. The difference from Example 5 is that the third extractant raw material does not contain octylphenol polyoxyethylene ether, pyridine-3,5-dicarboxylate and gemini sulfonate, and the third extractant includes the following raw materials in parts by weight: 1 part of cinnamic acid, 1 part of unsaturated -12 parts of hydroxy acid and 6 parts of diacetyl oxime.
[0172] Comparative Example 5
[0173] In this comparative example, the method for simultaneously recovering nickel, cobalt and manganese from waste lithium battery leachate is similar to that in Example 5. The difference from Example 5 is that in the embodiment of the present invention, the first extractant and the second extractant are P204 extractant, and the third extractant is P507 extractant.
[0174] In an embodiment of the present invention, a method for performing a first extraction on the precipitated residual liquid by using a first extractant is also provided. Figure 4 The schematic diagram of the process of performing the first extraction on the precipitated residual liquid by the first extractant is shown. The method of performing the first extraction on the precipitated residual liquid by the first extractant specifically includes:
[0175] Step S201, injecting the precipitated residual liquid into the extraction tank, and adjusting the pH value of the precipitated residual liquid by 30% NaOH so that the pH value of the precipitated residual liquid is controlled to be 5.8-6.2;
[0176] Step S202, compounding the first extractant, taking the first extractant and the diluent, compounding the first extractant and the diluent so that the volume fraction of the first extractant is 40-45%, and then performing the first extraction with the ratio of the organic phase to the aqueous phase being 1-3:2, the extraction temperature being controlled at 30-45° C., and the extraction time being 40-50 min;
[0177] It should be noted that when the first extractant and the diluent are compounded, the diluent may be No. 3 solvent oil or aviation kerosene.
[0178] Step S203, after the first extraction is completed, the mixture is allowed to stand for 10-15 minutes and then separated to obtain a first loaded organic phase and a first aqueous phase, wherein the first loaded organic phase is a manganese loaded organic phase, and the first loaded organic phase is subjected to five-stage countercurrent water washing with a manganese acid solution containing 0.1-0.4 g / L to obtain a manganese-rich organic phase and a manganese-poor aqueous phase, and the manganese-poor aqueous phase is refluxed to the first aqueous phase;
[0179] It should be noted that the manganese acid solution containing 0.1-0.4 g / L can be a mixed solution of acetic acid, malic acid or citric acid and manganese ions, and the concentration of the manganese acid solution can be 100-200 g / L. Using a weak acid to wash the first loaded organic phase can avoid strong acid corrosion to the equipment and the generation of acid waste liquid, making the extraction process more green and environmentally friendly.
[0180] Step S204, obtaining a manganese-rich organic phase, and stripping the manganese-rich organic phase with an organic acid, wherein the stripping time is 20-30 min, the stripping temperature is 30-40° C., and the ratio of the manganese-rich organic phase to the organic acid is controlled to be 8-10:1, to obtain a manganese-rich aqueous phase and a manganese-poor organic phase;
[0181] In this embodiment, the organic acid may be malic acid, tartaric acid or citric acid, and the concentration of the organic acid may be 450 g / L.
[0182] Step S205, obtaining a manganese-rich aqueous phase, injecting the manganese-rich aqueous phase into a precipitation tank, maintaining the temperature of the precipitation tank at 65-70°C, adjusting the pH value of the manganese-rich aqueous phase to 5.5-6 with an organic acid, and adding magnesium carbonate and an auxiliary separation agent into the precipitation tank to precipitate a manganese-enriched product.
[0183] In the embodiment of the present invention, manganese ions can be fully extracted when the first extraction is performed on the precipitate residue by the first extractant. Compared with the existing acidic extractants and alkaline extractants that have too high requirements on the pH value of the precipitate residue, the first extractant in the present invention can achieve efficient recovery of manganese ions only in a weakly acidic environment. In order to verify the extraction performance of the first extractant on manganese ions in the embodiment of the present invention, the first extractant prepared in Examples 1-5 of the present invention is taken, and then commercially available products P204 and P507 are used as the control group, and the process of steps S201-S205 is used to extract manganese ions respectively. Table 3 shows the manganese ion recovery test results.
[0184] Table 3
[0185]
[0186] It can be concluded from Table 3 that, compared with commercially available products, the first extractant prepared in Examples 1-5 of the present invention can fully recover manganese ions in a weakly acidic environment. At the same time, the first extractant has low selectivity for nickel, cobalt and lithium ions, thereby avoiding interference of impurity ions with the recovery of manganese ions during extraction.
[0187] In an embodiment of the present invention, a method for performing a second extraction on the first aqueous phase using a first extractant, a second extractant, and an auxiliary separation agent is also provided. Figure 5 The schematic diagram of the process of performing the second extraction on the first aqueous phase by using the first extractant, the second extractant, and the auxiliary separation agent is shown. The method of performing the second extraction on the first aqueous phase by using the first extractant, the second extractant, and the auxiliary separation agent specifically includes:
[0188] Step S301, injecting the first aqueous phase into an extraction tank, and adjusting the pH value of the first aqueous phase by 30% NaOH so that the pH value of the first aqueous phase is controlled to be 6-6.4;
[0189] Step S302, compounding the first extractant, the second extractant, and the auxiliary separation agent, taking the first extractant, the second extractant, the auxiliary separation agent and the diluent, compounding the first extractant, the second extractant, the auxiliary separation agent and the diluent, so that the volume fraction of the first extractant, the second extractant and the auxiliary separation agent is 55-65% of the total volume, and then performing the second extraction with the ratio of the organic phase to the aqueous phase being 4-8:1, the extraction temperature being controlled at 60-75° C., and the extraction time being 20-40 min;
[0190] Step S303, after the second extraction is completed, the mixture is allowed to stand for 20-25 minutes and then separated to obtain a second loaded organic phase and a second aqueous phase, wherein the second loaded organic phase is a copper loaded organic phase, and the second loaded organic phase is subjected to three-stage countercurrent water washing with a copper acid solution containing 0.1-0.4 g / L to obtain a copper-rich organic phase and a copper-poor aqueous phase, and the copper-poor aqueous phase is refluxed to the second aqueous phase;
[0191] Step S304, obtaining a copper-rich organic phase, and performing three-stage stripping on the copper-rich organic phase with an organic acid, wherein the stripping time is 40-50 min, the stripping temperature is 55-60° C., and the ratio of the copper-rich organic phase to the organic acid is controlled to be 5-6:1, to obtain a copper-rich aqueous phase and a copper-poor organic phase.
[0192] Different from the extraction of manganese, in the embodiment of the present invention, the first extractant, the second extractant, and the auxiliary separation agent cooperate with each other to achieve accurate extraction of copper ions when the first aqueous phase contains multiple metal ions. The auxiliary separation agent synergistically acts with the first extractant and the second extractant to inhibit the complexation of nickel and cobalt ions with the organic phase, while forming a low interfacial tension, thereby increasing the extraction rate of copper ions. On the one hand, it ensures the recovery rate of copper ions and avoids the recovery and extraction of other metal ions.
[0193] Another aspect of the present invention provides a method for performing a third extraction on the second aqueous phase using a third extractant, a co-solvent and an auxiliary separation agent. Figure 6 A schematic flow diagram of the implementation of the third extraction of the second aqueous phase by a third extractant, a co-solvent and an auxiliary separation agent is shown. The method of performing the third extraction of the second aqueous phase by a third extractant, a co-solvent and an auxiliary separation agent specifically includes:
[0194] Step S401, injecting the second aqueous phase into the extraction tank, and adjusting the pH value of the second aqueous phase by 30% NaOH so that the pH value of the second aqueous phase is controlled to be 7-7.4;
[0195] Step S402, compounding a third extractant, a co-solvent and an auxiliary separation agent, taking a third extractant, a co-solvent, an auxiliary separation agent and a diluent, compounding the third extractant, a co-solvent, an auxiliary separation agent and a diluent, so that the volume fraction of the third extractant, the co-solvent and the auxiliary separation agent is 50-55% of the total volume, and then performing a third extraction with a ratio of organic phase to aqueous phase of 2-3:1, an extraction temperature of 70-75° C., and an extraction time of 40-50 min;
[0196] Step S403, after the third extraction is completed, the mixture is allowed to stand for 20-25 minutes and then separated to obtain a third loaded organic phase and a third aqueous phase, wherein the third loaded organic phase is a cobalt loaded organic phase, and the third loaded organic phase is subjected to five-stage countercurrent water washing with a cobalt acid solution containing 0.5-1 g / L to obtain a cobalt-rich organic phase and a cobalt-depleted aqueous phase, and the cobalt-depleted aqueous phase is refluxed to the third aqueous phase;
[0197] Step S404, obtaining a cobalt-rich organic phase, and performing three-stage stripping on the cobalt-rich organic phase with an organic acid, wherein the stripping time is 15-20 min, the stripping temperature is 75-80° C., and the ratio of the cobalt-rich organic phase to the organic acid is controlled to be 2:1, to obtain a cobalt-rich aqueous phase and a cobalt-poor organic phase.
[0198] In this embodiment, the cobalt ions are efficiently extracted by compounding a third extractant, a co-solvent and an auxiliary separation agent, and the co-solvent acts on the third extractant to increase the surface activity of the third extractant and reduce the interfacial tension of the third extractant, so that the third extractant and the auxiliary separation agent cooperate with each other to achieve efficient extraction of cobalt ions in a neutral environment.
[0199] In this example, in order to characterize the interaction force between organic phase molecules and the influence of the organic phase interface stability in the examples of the present invention, the third extractant prepared in Examples 1-5 of the present invention and Comparative Examples 1-5 were characterized by using an interfacial tension meter, and the contact angles of the third extractant prepared in Examples 1-5 of the present invention and Comparative Examples 1-5 were measured. The interfacial tension and contact angle test results are shown in Table 4 and Fig. 9 shown.
[0200] Table 4
[0201]
[0202] From Table 4 and Fig. 9 It can be concluded that the third extractant prepared in Examples 1-5 of the present invention has lower interfacial tension and a moderate contact angle than that of Comparative Examples 1-5, thereby increasing the activity of the third extractant and increasing the stability during extraction. However, the interfacial tension of Comparative Examples 1-5 is too large, which makes the organic phase unstable during extraction and affects the extraction of various metal ions.
[0203] In order to verify the extraction and recovery efficiency of cobalt, nickel and lithium ions in Examples 1-5 of the present invention, the first extractant, the second extractant and the third extractant prepared in Examples 1-5 of the present invention and Comparative Examples 1-5 were used to extract and recover the waste lithium battery leachate. The extraction results are shown in Table 5 and Figure 10-12 As shown, Fig.10 The results of the cobalt ion extraction tests of Examples 1-5 and Comparative Examples 1-5 of the present invention are shown. Fig.11 The test results of nickel ion extraction of Examples 1-5 and Comparative Examples 1-5 of the present invention are shown. Fig.12 The test results of lithium ion extraction of Examples 1-5 of the present invention and Comparative Examples 1-5 are shown. From Table 5, it can be seen that the first extractant, the second extractant, and the third extractant prepared in Examples 1-5 of the present invention have higher extraction recovery rates for cobalt, nickel, and lithium metal ions than those in Comparative Examples 1-5.
[0204] Table 5
[0205]
[0206] In summary, the present invention provides a method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate. In the present invention, when the battery leachate is extracted, the pre-prepared first extractant, the second extractant, the third extractant, the co-solvent and the auxiliary separation agent cooperate with each other to realize the gradual extraction of the battery leachate, and the extraction system composed of the first extractant, the second extractant and the third extractant does not require additional saponification and strong acid assistance to achieve efficient extraction of metal ions, and can also avoid the problem that the emulsification degree of the battery leachate during extraction is difficult to control due to saponification, affecting the extraction efficiency.
[0207] It should be noted that, for the above-mentioned embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the described order of actions, because according to the present invention, some steps may be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present invention.
[0208] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.
Claims
1. Method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate. It is characterized in that The method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate comprises: Obtaining a lithium battery leachate, wherein the lithium battery leachate contains nickel, cobalt, manganese, iron, copper, and lithium ions, and adding an impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C. to complete precipitation and impurity removal of iron ions to obtain a precipitated residual liquid; Obtaining the precipitated residual liquid, pre-preparing a first extractant, a second extractant, a third extractant, a co-solvent and an auxiliary separation agent, performing a first extraction on the precipitated residual liquid with the first extractant to obtain a first loaded organic phase and a first aqueous phase, wherein the first loaded organic phase is a manganese loaded organic phase; Performing a second extraction on the first aqueous phase using a first extractant, a second extractant, and an auxiliary separation agent to obtain a second loaded organic phase and a second aqueous phase, wherein the second loaded organic phase is a copper loaded organic phase; Obtaining a second aqueous phase, performing a third extraction on the second aqueous phase using a third extractant, a co-solvent, and an auxiliary separation agent to obtain a third loaded organic phase and a third aqueous phase, wherein the third loaded organic phase is a cobalt loaded organic phase; Obtaining a third aqueous phase, adding a co-solvent and an auxiliary separation agent to the third aqueous phase, performing a fourth extraction on the third aqueous phase, mixing and stirring the third aqueous phase, the co-solvent and the auxiliary separation agent at 80-120° C. for 20-40 minutes to obtain a fourth loaded organic phase and a fourth aqueous phase, wherein the fourth loaded organic phase is a nickel loaded organic phase; The impurity removal precipitant comprises the following raw materials in parts by weight: 10-20 parts of magnesium carbonate, 15-25 parts of magnesium oxide, 10-15 parts of hydrophilic rhamnolipid, 20-30 parts of hydroxysulfobetaine, and 20-40 parts of ethanol; Wherein, the preparation method of the impurity removal precipitant specifically comprises: Obtain rhamnolipid, dissolve the rhamnolipid in ethanol at 60-70° C., add 2% by volume concentrated sulfuric acid to the rhamnolipid solution, react for 1-2 hours, then adjust the pH value of the rhamnolipid solution to 6.8-7.5 with 30% NaOH, centrifuge the rhamnolipid solution, and obtain hydrophilic rhamnolipid; Sodium 3-chloro-2-hydroxypropane sulfonate is synthesized by a ring-opening reaction of sodium bisulfite and epichlorohydrin, and then dodecylbenzyl chloride is reacted with dimethylolamine to obtain dodecylbenzyl dimethanolamine, and dodecylbenzyl dimethanolamine and sodium 3-chloro-2-hydroxypropane sulfonate are reacted in the presence of a palladium catalyst at 120°C for 2h to prepare hydroxysulfobetaine; Take the prepared hydroxysulfobetaine and hydrophilic rhamnolipid, mix the hydroxysulfobetaine and hydrophilic rhamnolipid with ethanol, and heat and stir at 60° C.; After the hydroxysulfobetaine and the hydrophilic rhamnolipid are mixed, the mixture is cooled to room temperature, and magnesium carbonate, magnesium oxide, the hydroxysulfobetaine and the hydrophilic rhamnolipid are mixed to obtain an impurity removal precipitant; The first extractant comprises the following raw materials in parts by weight: 1-10 parts of coconut glucoside, 2-15 parts of octylphenol polyoxyethylene ether, 1-20 parts of cinnamic acid, - 10-20 parts of hydroxy acid; The second extractant comprises the following raw materials in parts by weight: 1-7 parts of coconut glucoside, 12-25 parts of octylphenol polyoxyethylene ether, and 10-20 parts of diacetyl oxime; The third extractant comprises the following raw materials in parts by weight: 10-20 parts of octylphenol polyoxyethylene ether, 1-9 parts of cinnamic acid, unsaturated -hydroxy acid 3-20 parts, dimethylglyoxime 1-10 parts, pyridine-3,5-dicarboxylate 1-10 parts, gemini sulfonate 10-30 parts; The method for preparing the third extractant specifically comprises: Take toluene and butene, put them into the reactor, carry out nuclear olefination reaction, generate 1,3-dimethyl-4-vinylbenzene, and then cinnamic acid, unsaturated -Hydroxy acid is put into the reactor and the reactor is heated at a temperature of 70-80°C; The obtained 1,3-dimethyl-4-vinylbenzene is reacted with catechol to generate an intermediate of octylphenol polyoxyethylene ether, and then the octylphenol polyoxyethylene ether intermediate is subjected to a dehydration reaction to obtain octylphenol polyoxyethylene ether; Mix dimethylglyoxime and pyridine-3,5-dicarboxylate, then add tetrahydrofuran to the mixture, mix at 80-90° C. for 2-3 hours, wash the mixture, evaporate the solvent, and vacuum dry at 90-100° C. for 3 hours to obtain an extractant intermediate; Taking sodium 2-chloroethylsulfonate, 1,3-propylenediamine and epichlorohydrin as raw materials for synthesizing gemini sulfonate, using sodium 2-chloroethylsulfonate as a substituent, carrying out a substitution reaction on 1,3-propylenediamine with the assistance of a palladium catalyst, then adding epichlorohydrin for a ring-opening reaction to obtain a sulfonate intermediate, and then adding sulfuric acid for a sulfonation reaction to obtain gemini sulfonate; Octylphenol polyoxyethylene ether, gemini sulfonate and the extractant intermediate are mixed in a nitrogen-deoxygenated reactor, and then aviation kerosene is added and mixed at 65-70° C. for 3 hours to obtain a third extractant; The co-solvent comprises the following raw materials in weight percentage: Propylene glycol: 10% Glycol: 5% Tridecylmethylammonium bromide: 15% Tetrabutylammonium hydrogen sulfate: 30% Eucalyptus oil: 20% L-Menthol: 20% The auxiliary separation agent is a mixture of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate, and the mass ratio of N, N-dimethyltetradecylcarboxybetaine, 1, 2-decanediol, and sodium dodecyl sulfate is 1:2:
1.
2. The method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate according to claim 1, Features: The method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate also includes: The fourth aqueous phase is obtained, the third extractant and the auxiliary separation agent are added to the fourth aqueous phase, and the fourth aqueous phase is subjected to a fifth extraction to obtain a fifth loaded organic phase and a fifth aqueous phase, wherein the fifth loaded organic phase is a lithium loaded organic phase.
3. The method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate as claimed in claim 2, Features: The method of performing a first extraction on the precipitated residual liquid by using a first extractant specifically comprises: The precipitated residual liquid is injected into the extraction tank, and the pH value of the precipitated residual liquid is adjusted by 30% NaOH so that the pH value of the precipitated residual liquid is controlled to be 5.8-6.2; Compounding the first extractant, taking the first extractant and the diluent, compounding the first extractant and the diluent so that the volume fraction of the first extractant is 40-45%, and then performing the first extraction with the ratio of the organic phase to the aqueous phase being 1-3:2, the extraction temperature being controlled at 30-45° C., and the extraction time being 40-50 min; After the first extraction is completed, the mixture is allowed to stand for 10-15 minutes and then separated to obtain a first loaded organic phase and a first aqueous phase, wherein the first loaded organic phase is a manganese loaded organic phase, and the first loaded organic phase is subjected to five-stage countercurrent water washing with a manganese acid solution containing 0.1-0.4 g / L to obtain a manganese-rich organic phase and a manganese-poor aqueous phase, and the manganese-poor aqueous phase is refluxed to the first aqueous phase; Obtaining a manganese-rich organic phase, and stripping the manganese-rich organic phase with an organic acid, wherein the stripping time is 20-30 minutes, the stripping temperature is 30-40° C., and the ratio of the manganese-rich organic phase to the organic acid is controlled to be 8-10:1, to obtain a manganese-rich aqueous phase and a manganese-poor organic phase; Obtain a manganese-rich aqueous phase, inject the manganese-rich aqueous phase into a precipitation tank, maintain the temperature of the precipitation tank at 65-70°C, adjust the pH value of the manganese-rich aqueous phase to 5.5-6 with an organic acid, and simultaneously add magnesium carbonate and an auxiliary separation agent into the precipitation tank to precipitate a manganese-enriched product.
4. The method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate as claimed in claim 3, Features: The method of performing a second extraction on the first aqueous phase by using a first extractant, a second extractant, and an auxiliary separation agent specifically comprises: Inject the first aqueous phase into the extraction tank, and adjust the pH value of the first aqueous phase by 30% NaOH so that the pH value of the first aqueous phase is controlled to be 6-6.4; Compounding the first extractant, the second extractant, and the auxiliary separation agent, taking the first extractant, the second extractant, the auxiliary separation agent and the diluent, compounding the first extractant, the second extractant, the auxiliary separation agent and the diluent, so that the volume fraction of the first extractant, the second extractant and the auxiliary separation agent is 55-65% of the total volume, and then performing the second extraction with the ratio of the organic phase to the aqueous phase being 4-8:1, the extraction temperature being controlled at 60-75° C., and the extraction time being 20-40 min; After the second extraction is completed, the mixture is allowed to stand for 20-25 minutes and then separated to obtain a second loaded organic phase and a second aqueous phase, wherein the second loaded organic phase is a copper loaded organic phase, and the second loaded organic phase is subjected to a three-stage countercurrent water wash with a copper acid solution containing 0.1-0.4 g / L to obtain a copper-rich organic phase and a copper-poor aqueous phase, and the copper-poor aqueous phase is refluxed to the second aqueous phase; A copper-rich organic phase is obtained, and an organic acid is used to perform three-stage stripping on the copper-rich organic phase, wherein the stripping time is 40-50 minutes, the stripping temperature is 55-60° C., and the ratio of the copper-rich organic phase to the organic acid is controlled to be 5-6:1, to obtain a copper-rich aqueous phase and a copper-poor organic phase.
5. The method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate as claimed in claim 4, Features: The method of performing a third extraction on the second aqueous phase by using a third extractant, a co-solvent and an auxiliary separation agent specifically comprises: The second aqueous phase is injected into the extraction tank, and the pH value of the second aqueous phase is adjusted by 30% NaOH so that the pH value of the second aqueous phase is controlled to be 7-7.4; Compounding a third extractant, a co-solvent and an auxiliary separation agent, taking a third extractant, a co-solvent, an auxiliary separation agent and a diluent, compounding the third extractant, a co-solvent, an auxiliary separation agent and a diluent, so that the volume fraction of the third extractant, the co-solvent and the auxiliary separation agent is 50-55% of the total volume, and then performing a third extraction with a ratio of organic phase to aqueous phase of 2-3:1, an extraction temperature of 70-75° C., and an extraction time of 40-50 min; After the third extraction is completed, the mixture is allowed to stand for 20-25 minutes and then separated to obtain a third loaded organic phase and a third aqueous phase, wherein the third loaded organic phase is a cobalt loaded organic phase, and the third loaded organic phase is subjected to five-stage countercurrent water washing with a cobalt acid solution containing 0.5-1 g / L to obtain a cobalt-rich organic phase and a cobalt-depleted aqueous phase, and the cobalt-depleted aqueous phase is refluxed to the third aqueous phase; A cobalt-rich organic phase is obtained, and the cobalt-rich organic phase is subjected to three-stage stripping with an organic acid, wherein the stripping time is 15-20 minutes, the stripping temperature is 75-80° C., and the ratio of the cobalt-rich organic phase to the organic acid is controlled to be 2:1, to obtain a cobalt-rich aqueous phase and a cobalt-poor organic phase.
6. The method for synchronously recovering nickel, cobalt and manganese from waste lithium battery leachate as claimed in claim 5, Features: The method of adding a de-impurity precipitant to a lithium battery leachate to complete the precipitation and de-impurity of iron ions specifically comprises: Obtain lithium battery leachate, add ethanol to the lithium battery leachate, mix by ultrasonication for 30 minutes, and then place in a water bath at 65° C. for 20 minutes; Add the pre-prepared impurity removal precipitant to the lithium battery leachate at a temperature of 50-60° C., while maintaining a stirring speed of 200-250 r / min, and stop adding the impurity removal precipitant when the pH value of the lithium battery leachate reaches 5.2-5.5; The stirring speed was reduced to 100-150 r / min, and after aging for 50 minutes, the stirring was stopped. After standing for 20 minutes, the lithium battery leachate was filtered and separated to obtain precipitated iron slag and precipitated residual liquid.