A flash-steamed nonwoven fabric-metal composite sheet and preparation method thereof

By coating the flash evaporated non-woven fabric with aluminum film and adding nano-cerium dioxide composite particles, the longitudinal nail rod tear strength and thermal aging performance of the flash evaporated polyethylene material are improved, which solves the problem of insufficient performance in the existing technology. Efficient preparation technology and low-cost production are achieved.

CN118497978BActive Publication Date: 2024-10-22JIANGSU QINGYUN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970857.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-22
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Existing flash evaporated polyethylene materials cannot meet the requirements of high longitudinal nail rod tear strength and good thermal aging resistance at the same time in application, and the modification method of introducing polymer materials makes the flash evaporation process unable to be applied.

Method used

The surface or bottom of the flash-evaporated non-woven fabric is coated with a metallic aluminum film, and nano-cerium dioxide composite particles are added to the raw material. The nail rod tear strength and thermal aging performance of the material are improved through a specific preparation process, including soaking and heating. , cooling the nanorods to prepare composite particles, mixing the spinning solution and performing flash spinning, hot rolling, and vacuum evaporation processes to prepare composite sheets.

Benefits of technology

It achieves high longitudinal nail rod tear strength and improved thermal aging performance of the composite sheet. The weight is less than 300g/m2, the longitudinal nail rod tear strength is greater than 260N/50mm, and the maximum tensile force retention rate during thermal aging is greater than 85%. The process is simple. , low cost and suitable for large-scale promotion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of flash-steamed polyethylene, and in particular to a flash-steamed non-woven fabric-metal composite sheet and a preparation method thereof. Aiming at the problem that flash-steamed polyethylene in the prior art often fails to meet the requirements of strength and heat aging resistance, the present invention provides a flash-steamed non-woven fabric-metal composite sheet and a preparation method thereof, wherein a metal aluminum film is plated on the surface or bottom surface of the flash-steamed non-woven fabric; the raw materials of the flash-steamed non-woven fabric are polyethylene and composite particles; the gram weight of the composite sheet is less than 300g / m2; the thickness of the metal aluminum film is in a ratio of 0.1:1 to 0.5:1 to the thickness of the composite sheet; the longitudinal nail rod tear strength is greater than 260N / 50mm; and the longitudinal heat aging maximum tensile retention rate is greater than 85%. The present invention adds composite particles to the flash-steamed raw materials, thereby improving the nail rod tear strength and heat aging resistance of the obtained composite sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flash-evaporated polyethylene, and in particular relates to a flash-evaporated non-woven fabric-metal composite sheet and a preparation method thereof. Background Art

[0002] Aluminum has good light reflection properties. Aluminum-plated flash non-woven fabrics can reflect most of the light and heat and can be used as thermal insulation materials, such as tents, parasol fabrics, sunscreen fabrics, etc., to reduce heat transfer and keep the interior cool. In such application scenarios, the flash-steamed polyethylene substrate is required to have good resistance to heat aging. At the same time, since there are often installation requirements in such application scenarios, the flash-steamed polyethylene substrate also has a requirement for higher longitudinal nail rod tear strength. The flash-steamed polyethylene in the prior art often cannot meet the above requirements.

[0003] In response to this problem, people have also conducted exploration and research in long-term production and life practices. A Chinese invention patent application discloses a production process of polyethylene aluminum-plated film [application number: 201510711568.9]. The invention patent application includes the following steps: a catalytic step, using a metallocene catalyst to catalyze a polypropylene resin material to form a metallocene copolymer polyethylene; an aluminum plating step, aluminum is plated on the surface of the polypropylene resin material to form an aluminum-plated polyethylene; an extrusion step, the metallocene copolymer polyethylene, the polypropylene resin material and the aluminum-plated polyethylene are co-extruded in an extruder to obtain a three-layer melt of a metallocene copolymer polyethylene layer, a polypropylene layer and an aluminum-plated polyethylene layer in contact; a casting step, the three-layer melt is quickly cooled and shaped into a three-layer film by the action of a casting roller; a corona step, an oxidized polarization base is formed on the surface of the three-layer film, so that the surface of the three-layer film has polarity, which is convenient for the adsorption of printing ink; a trimming step, using a wind knife to process the three-layer film to a desired shape in a vacuum box; a film collection step, the three-layer film is curled on the film collection roller.

[0004] This invention patent application uses a metallocene catalyst to catalyze polypropylene resin materials to form metallocene copolymer polyethylene, making it a good aluminum-plated substrate. However, this modification method introduces polymer materials other than polyethylene, and also makes the flash evaporation process unusable. Summary of the invention

[0005] The object of the present invention is to provide a flash nonwoven fabric-metal composite sheet with good strength and heat aging performance in view of the above problems.

[0006] Another object of the present invention is to provide a method for preparing a flash-steamed nonwoven fabric-metal composite sheet with good strength and thermal aging performance in order to solve the above-mentioned problems.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A flash nonwoven fabric-metal composite sheet, wherein a metal aluminum film is plated on the surface or bottom surface of the flash nonwoven fabric; the raw materials of the flash nonwoven fabric are polyethylene and composite particles;

[0009] The weight of the composite sheet is less than 300g / m 2 ;

[0010] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.1:1 and 0.5:1;

[0011] The longitudinal nail rod tear strength is greater than 260N / 50mm;

[0012] The maximum tensile retention rate of longitudinal heat aging is greater than 85%;

[0013] The test standard for nail rod tear strength is GB / T 328.18-2007;

[0014] The test standard for thermal aging maximum tensile retention rate and thermal aging impermeability retention rate is JC / T 2291-2014.

[0015] In the above-mentioned flash-steamed nonwoven fabric-metal composite sheet, the longitudinal nail rod tear strength of the flash-steamed nonwoven fabric-metal composite sheet is 265-275N / 50mm.

[0016] In the above-mentioned flash-steamed nonwoven fabric-metal composite sheet, the longitudinal nail rod tear strength of the flash-steamed nonwoven fabric-metal composite sheet is 275-285N / 50mm.

[0017] In the above-mentioned flash-steamed nonwoven fabric-metal composite sheet, the longitudinal nail rod tear strength of the flash-steamed nonwoven fabric-metal composite sheet is 285-295N / 50mm.

[0018] In the above-mentioned flash-steamed nonwoven fabric-metal composite sheet, the longitudinal nail rod tear strength of the flash-steamed nonwoven fabric-metal composite sheet is 295-305N / 50mm.

[0019] In the above-mentioned flash-steamed nonwoven fabric-metal composite sheet, the maximum tensile force retention rate of the flash-steamed nonwoven fabric-metal composite sheet in the longitudinal direction after heat aging is greater than 88%.

[0020] In the above-mentioned flash-steamed nonwoven fabric-metal composite sheet, the longitudinal heat aging maximum tensile force retention rate of the flash-steamed nonwoven fabric-metal composite sheet is above 90%.

[0021] In the above-mentioned flash-steamed nonwoven fabric-metal composite sheet, the longitudinal heat aging maximum tensile force retention rate of the flash-steamed nonwoven fabric-metal composite sheet is above 95%.

[0022] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.1:1 and 0.2:1.

[0023] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.2:1 and 0.3:1.

[0024] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.3:1 and 0.4:1.

[0025] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.4:1 and 0.5:1.

[0026] The weight of the composite sheet is less than 300g / m 2 .

[0027] The weight of the composite sheet is less than 270g / m 2 .

[0028] The weight of the composite sheet is less than 240g / m 2 .

[0029] The weight of the composite sheet is less than 210g / m 2 .

[0030] The weight of the composite sheet is less than 180g / m 2 .

[0031] In the above-mentioned flash-steamed nonwoven fabric-metal composite sheet, the composite particles are prepared by the following method:

[0032] Step A: taking cerium dioxide nanorods with a diameter of 150 nm and a length of 2-2.5 μm and soaking them in a 1 mol / L sodium hydroxide solution for 2-4 hours to obtain alkaline cerium dioxide nanorods;

[0033] Step B: The alkaline cerium dioxide nanorods prepared in step A are heated to 1000-1200° C. in an argon atmosphere, kept warm for 30-90 minutes, and then cooled to below 30° C. within 60-100 seconds to obtain composite particles.

[0034] A method for preparing the above-mentioned flash-steamed nonwoven fabric-metal composite sheet comprises the following steps:

[0035] Step 1: Add composite particles, spinning solvent and polyethylene into a mixing kettle at a temperature of 180-200°C and a pressure of 200-210 bar to obtain a spinning solution; the mass fraction of polyethylene in the spinning solution is 8-13%; the amount of composite particles added is 2-3% of the mass fraction of polyethylene

[0036] The spinning solvent is aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, unsaturated hydrocarbons, halogenated hydrocarbons and the like.

[0037] Step 2: flash spinning the spinning solution obtained in step 1 at a spinning temperature of 200 to 220° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 105 to 115° C. to obtain flash polyethylene substrates;

[0038] Step 3: The flash-evaporated polyethylene substrate obtained in step 2 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1000-1200°C and the vacuum degree is 2-4×10 -4 MPa, the wire feeding speed of the aluminum wire is 800-1200 mm / min, and the moving speed of the flash-evaporated polyethylene substrate is 300-400 m / min, so as to obtain a flash-evaporated non-woven fabric-metal composite sheet.

[0039] Compared with the prior art, the advantages of the present invention are:

[0040] 1. The present invention adds composite particles to the flash raw materials, thereby improving the nail rod tear strength and heat aging resistance of the prepared composite sheet.

[0041] 2. The present invention uses nano-cerium dioxide as the raw material for preparing composite particles. Nano-cerium dioxide has unique oxygen vacancies, can absorb and transform free radicals, and can effectively improve the thermal aging resistance of polyethylene. At the same time, after the nano-cerium dioxide is alkalized, it is subjected to heat treatment and rapid cooling to improve the roughness of the surface of the nano-cerium dioxide to increase its surface area, so that the nano-particles have stronger adhesion and better interface interaction with the flash polyethylene matrix, thereby further improving the comprehensive performance of the composite material.

[0042] 3. The process flow of the present invention is simple, the operation is convenient, the production cost is low, and it is suitable for large-scale promotion and use. DETAILED DESCRIPTION

[0043] The present invention is further described in detail below in conjunction with specific implementation methods.

[0044] Example 1

[0045] This embodiment provides a method for preparing a flash-evaporated nonwoven fabric-metal composite sheet, comprising the following steps:

[0046] Step 1: Take cerium dioxide nanorods, the diameter of the cerium dioxide nanorods is 150nm, the length is in the range of 2-2.5μm, soak them in 1mol / L sodium hydroxide solution, soak for 2h to obtain alkaline cerium dioxide nanorods;

[0047] Step 2: heating the alkaline cerium dioxide nanorods prepared in step 1 to 1000° C. in an argon atmosphere, keeping the temperature for 30 minutes, and then cooling to below 30° C. within 60 seconds to obtain composite particles;

[0048] Step 3: Add the composite particles, spinning solvent and polyethylene into a mixing kettle, the mass of the composite particles added is 2.5% of the mass of polyethylene, the temperature of the mixing kettle is 180°C, the pressure is 200 bar, and a spinning solution is obtained; the mass fraction of polyethylene in the spinning solution is 8%;

[0049] Step 4: flash spinning the spinning solution obtained in step 3 at a spinning temperature of 200° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 105° C. to obtain flash polyethylene substrates;

[0050] Step 5: The flash-evaporated polyethylene substrate obtained in step 4 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1000°C and the vacuum degree is 2×10 -4 MPa, the wire feeding speed of the aluminum wire is 800 mm / min, and the moving speed of the flash polyethylene substrate is 300 m / min to obtain a composite sheet.

[0051] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is 0.1:1.

[0052] The weight of the composite sheet is 95g / m 2 ; The longitudinal nail rod tear strength is 272N / 50mm; The maximum tensile force retention rate of longitudinal heat aging is 95.7%.

[0053] The test standard for nail rod tear strength is GB / T 328.18-2007; the test standard for heat aging maximum tensile retention rate and heat aging impermeability retention rate is JC / T 2291-2014.

[0054] The cerium dioxide nanorods used in the embodiments and comparative examples of the present invention were purchased from Beijing Beike New Materials Technology Co., Ltd., with the product number: BKDY000673-01.

[0055] Example 2

[0056] This embodiment provides a method for preparing a flash-evaporated nonwoven fabric-metal composite sheet, comprising the following steps:

[0057] Step 1: Take cerium dioxide nanorods, the diameter of the cerium dioxide nanorods is 150nm, the length is in the range of 2-2.5μm, soak them in 1mol / L sodium hydroxide solution, soak for 4h to obtain alkaline cerium dioxide nanorods;

[0058] Step 2: heating the alkaline cerium dioxide nanorods prepared in step 1 to 1200° C. in an argon atmosphere, keeping the temperature for 90 minutes, and then cooling to below 30° C. within 100 seconds to obtain composite particles;

[0059] Step 3: Add the composite particles, spinning solvent and polyethylene into a mixing kettle, the mass of the composite particles added is 2.5% of the mass of polyethylene, the temperature of the mixing kettle is 200°C, the pressure is 210 bar, and a spinning solution is obtained; the mass fraction of polyethylene in the spinning solution is 13%;

[0060] Step 4: flash spinning the spinning solution obtained in step 3 at a spinning temperature of 220° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 115° C. to obtain flash polyethylene substrates;

[0061] Step 5: The flash-evaporated polyethylene substrate obtained in step 4 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1200°C and the vacuum degree is 4×10 -4 MPa, the wire feeding speed of the aluminum wire is 1200 mm / min, and the moving speed of the flash polyethylene substrate is 400 m / min to obtain a composite sheet.

[0062] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is 0.5:1.

[0063] The weight of the composite sheet is 275g / m 2 ; The longitudinal nail rod tear strength is 301N / 50mm; The maximum tensile retention rate of longitudinal heat aging is 96.3%.

[0064] The test standard for nail rod tear strength is GB / T 328.18-2007; the test standard for heat aging maximum tensile retention rate and heat aging impermeability retention rate is JC / T 2291-2014.

[0065] Example 3

[0066] This embodiment provides a method for preparing a flash-evaporated nonwoven fabric-metal composite sheet, comprising the following steps:

[0067] Step 1: Take cerium dioxide nanorods, the diameter of the cerium dioxide nanorods is 150nm, the length is in the range of 2-2.5μm, soak them in 1mol / L sodium hydroxide solution, soak for 3h to obtain alkaline cerium dioxide nanorods;

[0068] Step 2: heating the alkaline cerium dioxide nanorods prepared in step 1 to 1100° C. in an argon atmosphere, keeping the temperature for 60 minutes, and then cooling to below 30° C. within 80 seconds to obtain composite particles;

[0069] Step 3: Add the composite particles, spinning solvent and polyethylene into a mixing kettle, the mass of the composite particles added is 2.5% of the mass of polyethylene, the temperature of the mixing kettle is 190°C, the pressure is 205 bar, and a spinning solution is obtained; the mass fraction of polyethylene in the spinning solution is 10%;

[0070] Step 4: flash spinning the spinning solution obtained in step 3 at a spinning temperature of 210° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 110° C. to obtain flash polyethylene substrates;

[0071] Step 5: The flash-evaporated polyethylene substrate obtained in step 4 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1100°C and the vacuum degree is 3×10 -4 MPa, the wire feeding speed of the aluminum wire is 1000 mm / min, and the moving speed of the flash polyethylene substrate is 350 m / min to obtain a composite sheet.

[0072] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is 0.3:1.

[0073] The weight of the composite sheet is 185g / m 2 ; The longitudinal nail rod tear strength is 285N / 50mm; The maximum tensile retention rate of longitudinal heat aging is 96.0%.

[0074] The test standard for nail rod tear strength is GB / T 328.18-2007; the test standard for heat aging maximum tensile retention rate and heat aging impermeability retention rate is JC / T 2291-2014.

[0075] Comparative Example 1

[0076] This comparative example provides a method for preparing a flash-evaporated nonwoven fabric-metal composite sheet, comprising the following steps:

[0077] Step 1: Add spinning solvent and polyethylene into a mixing kettle at a temperature of 190°C and a pressure of 205 bar to obtain a spinning solution;

[0078] Step 2: flash spinning the spinning solution obtained in step 1 at a spinning temperature of 210° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 110° C. to obtain flash polyethylene substrates;

[0079] Step 3: The flash-evaporated polyethylene substrate obtained in step 2 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1100°C and the vacuum degree is 3×10 -4 MPa, the wire feeding speed of the aluminum wire is 1000 mm / min, and the moving speed of the flash polyethylene substrate is 350 m / min to obtain a composite sheet.

[0080] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is 0.3:1.

[0081] The weight of the composite sheet is 184g / m2 ; The longitudinal nail rod tear strength is 243N / 50mm; The maximum tensile force retention rate of longitudinal heat aging is 82.7%.

[0082] The test standard for nail rod tear strength is GB / T 328.18-2007; the test standard for heat aging maximum tensile retention rate and heat aging impermeability retention rate is JC / T 2291-2014.

[0083] Comparative Example 2

[0084] This comparative example provides a method for preparing a flash-evaporated nonwoven fabric-metal composite sheet, comprising the following steps:

[0085] Step 1: Take cerium dioxide nanorods, the diameter of which is 150 nm and the length of which is in the range of 2-2.5 μm, soak them in a 1 mol / L sodium hydroxide solution, and filter and dry them after soaking for 3 hours to obtain composite particles;

[0086] Step 2: Add composite particles, spinning solvent and polyethylene into a mixing kettle, the mass of the composite particles added is 2.5% of the mass of polyethylene, the temperature of the mixing kettle is 190°C, the pressure is 205 bar, and a spinning solution is obtained; the mass fraction of polyethylene in the spinning solution is 10%;

[0087] Step 3: flash spinning the spinning solution obtained in step 2 at a spinning temperature of 210° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 110° C. to obtain flash polyethylene substrates;

[0088] Step 4: The flash-evaporated polyethylene substrate obtained in step 3 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1100°C and the vacuum degree is 3×10 -4 MPa, the wire feeding speed of the aluminum wire is 1000 mm / min, and the moving speed of the flash polyethylene substrate is 350 m / min to obtain a composite sheet.

[0089] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is 0.3:1.

[0090] The weight of the composite sheet is 185g / m 2 ; The longitudinal nail rod tear strength is 279N / 50mm; The maximum tensile force retention rate of longitudinal heat aging is 95.8%.

[0091] The test standard for nail rod tear strength is GB / T 328.18-2007; the test standard for heat aging maximum tensile retention rate and heat aging impermeability retention rate is JC / T 2291-2014.

[0092] Comparative Example 3

[0093] This comparative example provides a method for preparing a flash-evaporated nonwoven fabric-metal composite sheet, comprising the following steps:

[0094] Step 1: Take the cerium dioxide nanorods and heat them to 1100°C in an argon atmosphere, keep them warm for 60 minutes, and then cool them to below 30°C within 80 seconds to obtain composite particles;

[0095] Step 2: Add composite particles, spinning solvent and polyethylene into a mixing kettle, the mass of the composite particles added is 2.5% of the mass of polyethylene, the temperature of the mixing kettle is 190°C, the pressure is 205 bar, and a spinning solution is obtained; the mass fraction of polyethylene in the spinning solution is 10%;

[0096] Step 3: flash spinning the spinning solution obtained in step 2 at a spinning temperature of 210° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 110° C. to obtain flash polyethylene substrates;

[0097] Step 4: The flash-evaporated polyethylene substrate obtained in step 3 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1100°C and the vacuum degree is 3×10 -4 MPa, the wire feeding speed of the aluminum wire is 1000 mm / min, and the moving speed of the flash polyethylene substrate is 350 m / min to obtain a composite sheet.

[0098] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is 0.3:1.

[0099] The weight of the composite sheet is 185g / m 2 ; The longitudinal nail rod tear strength is 277N / 50mm; The maximum tensile force retention rate of longitudinal heat aging is 95.8%.

[0100] The test standard for nail rod tear strength is GB / T 328.18-2007; the test standard for heat aging maximum tensile retention rate and heat aging impermeability retention rate is JC / T 2291-2014.

[0101] Comparative Example 4

[0102] This comparative example provides a method for preparing a flash-evaporated nonwoven fabric-metal composite sheet, comprising the following steps:

[0103] Step 1: Take nano-silicon dioxide and soak it in 1 mol / L sodium hydroxide solution for 3 hours to obtain alkaline nano-silicon dioxide;

[0104] Step 2: heating the alkaline nano-silicon dioxide obtained in step 1 to 1100° C. in an argon atmosphere, keeping the temperature for 60 minutes, and then cooling to below 30° C. within 80 seconds to obtain composite particles;

[0105] Step 3: Add the composite particles, spinning solvent and polyethylene into a mixing kettle, the mass of the composite particles added is 2.5% of the mass of polyethylene, the temperature of the mixing kettle is 190°C, the pressure is 205 bar, and a spinning solution is obtained; the mass fraction of polyethylene in the spinning solution is 10%;

[0106] Step 4: flash spinning the spinning solution obtained in step 3 at a spinning temperature of 210° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 110° C. to obtain flash polyethylene substrates;

[0107] Step 5: The flash-evaporated polyethylene substrate obtained in step 4 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1100°C and the vacuum degree is 3×10 -4 MPa, the wire feeding speed of the aluminum wire is 1000 mm / min, and the moving speed of the flash polyethylene substrate is 350 m / min to obtain a composite sheet.

[0108] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is 0.3:1.

[0109] The weight of the composite sheet is 183g / m 2 ; The longitudinal nail rod tear strength is 263N / 50mm; The maximum tensile force retention rate of longitudinal heat aging is 92.7%.

[0110] The test standard for nail rod tear strength is GB / T 328.18-2007; the test standard for heat aging maximum tensile retention rate and heat aging impermeability retention rate is JC / T 2291-2014.

[0111] Comparative Example 5

[0112] This comparative example provides a method for preparing a flash-evaporated nonwoven fabric-metal composite sheet, comprising the following steps:

[0113] Step 1: Take nano cerium dioxide powder, soak it in 1 mol / L sodium hydroxide solution, and soak it for 3 hours to obtain alkaline nano cerium dioxide powder;

[0114] Step 2: heating the alkaline nano-cerium dioxide powder obtained in step 1 to 1100° C. in an argon atmosphere, keeping the temperature for 60 minutes, and then cooling to below 30° C. within 80 seconds to obtain composite particles;

[0115] Step 3: Add the composite particles, spinning solvent and polyethylene into a mixing kettle, the mass of the composite particles added is 2.5% of the mass of polyethylene, the temperature of the mixing kettle is 190°C, the pressure is 205 bar, and a spinning solution is obtained; the mass fraction of polyethylene in the spinning solution is 10%;

[0116] Step 4: flash spinning the spinning solution obtained in step 3 at a spinning temperature of 210° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 110° C. to obtain flash polyethylene substrates;

[0117] Step 5: The flash-evaporated polyethylene substrate obtained in step 4 is subjected to vacuum evaporation to deposit a metal aluminum film. The evaporation boat is preheated to 1100°C and the vacuum degree is 3×10 -4 MPa, the wire feeding speed of the aluminum wire is 1000 mm / min, and the moving speed of the flash polyethylene substrate is 350 m / min to obtain a composite sheet.

[0118] The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is 0.3:1.

[0119] The weight of the composite sheet is 185g / m 2 ; The longitudinal nail rod tear strength is 267N / 50mm; The maximum tensile force retention rate of longitudinal heat aging is 94.9%.

[0120] The test standard for nail rod tear strength is GB / T 328.18-2007; the test standard for heat aging maximum tensile retention rate and heat aging impermeability retention rate is JC / T 2291-2014.

[0121] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways without departing from the spirit of the present invention.

Claims

1. A flash nonwoven fabric-metal composite sheet, characterized in that: A metal aluminum film is plated on the surface or bottom of the flash non-woven fabric; the raw materials of the flash non-woven fabric are polyethylene and composite particles; The weight of the composite sheet is less than 300g / m 2 ; The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.1:1 and 0.5:1; The longitudinal nail rod tear strength is greater than 260N / 50mm; The maximum tensile retention rate of longitudinal heat aging is greater than 85%; The test standard for nail rod tear strength is GB / T 328.18-2007; The test standard for the maximum tensile retention rate of heat aging and the water-impermeability retention rate of heat aging is JC / T 2291-2014; The composite particles are prepared by the following method: Step A: taking cerium dioxide nanorods with a diameter of 150 nm and a length of 2-2.5 μm and soaking them in a 1 mol / L sodium hydroxide solution for 2-4 hours to obtain alkaline cerium dioxide nanorods; Step B: The alkaline cerium dioxide nanorods prepared in step A are heated to 1000-1200° C. in an argon atmosphere, kept warm for 30-90 minutes, and then cooled to below 30° C. within 60-100 seconds to obtain composite particles.

2. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The longitudinal nail rod tear strength of the flash nonwoven fabric-metal composite sheet is 265-275N / 50mm.

3. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The longitudinal nail rod tear strength of the flash nonwoven fabric-metal composite sheet is 275-285N / 50mm.

4. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The longitudinal nail rod tear strength of the flash nonwoven fabric-metal composite sheet is 285-295N / 50mm.

5. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The longitudinal nail rod tear strength of the flash nonwoven fabric-metal composite sheet is 295-305N / 50mm.

6. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The maximum tensile retention rate of the flash nonwoven fabric-metal composite sheet during longitudinal heat aging is above 88%.

7. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The maximum longitudinal heat aging tensile retention rate of the flash nonwoven fabric-metal composite sheet is more than 90%.

8. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The maximum tensile retention rate of longitudinal heat aging of the flash nonwoven fabric-metal composite sheet is more than 95%.

9. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.1:1 and 0.2:

1.

10. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.2:1 and 0.3:

1.

11. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.3:1 and 0.4:

1.

12. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The ratio of the thickness of the metal aluminum film to the thickness of the composite sheet is between 0.4:1 and 0.5:

1.

13. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The weight of the composite sheet is less than 300g / m 2 .

14. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The weight of the composite sheet is less than 270g / m 2 .

15. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The weight of the composite sheet is less than 240g / m 2 .

16. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The weight of the composite sheet is less than 210g / m 2 .

17. The flash-steamed nonwoven fabric-metal composite sheet according to claim 1, characterized in that: The weight of the composite sheet is less than 180g / m 2 .

18. A method for preparing a flash-evaporated nonwoven fabric-metal composite sheet as claimed in claim 1, characterized in that: The following steps are involved: Step 1: Add the composite particles, spinning solvent and polyethylene into a mixing kettle at a temperature of 180-200° C. and a pressure of 200-210 bar to obtain a spinning solution; Step 2: flash spinning the spinning solution obtained in step 1 at a spinning temperature of 200 to 220° C. to obtain flash fibers, and web laying and hot rolling the flash fibers at a hot rolling temperature of 105 to 115° C. to obtain flash polyethylene substrates; Step three: The flash-evaporated polyethylene substrate obtained in step two is subjected to vacuum evaporation to deposit a metal aluminum film to obtain a composite sheet.

19. A method for flash-evaporating a nonwoven fabric-metal composite sheet according to claim 18, characterized in that: In step 3, the process parameters of the evaporation process are: the evaporation boat preheating temperature is 1000-1200℃, the vacuum degree is 2-4×10 -4 MPa, the wire feeding speed of the aluminum wire is 800-1200mm / min, and the moving speed of the flash polyethylene substrate is 300-400m / min.