Preparation of a visual on-site detection kit for detecting TNT based on magnetic core-shell nanospheres
Through a visual detection kit based on magnetic core-shell nanospheres, combined with tapioca starch and TMB/H2O2 chemiluminescence system, the problems of environmental hazards, complex operations and low detection accuracy of the existing TNT detection methods are solved, achieving high sensitivity, Low-cost TNT testing meets on-site rapid testing needs.
Patent Information
- Application Number
- CN202410958253.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Existing TNT detection methods have problems such as environmental hazards, complex operations, high costs, low detection accuracy, and lack of on-site rapid detection methods. In particular, the traditional visual sensor substrate is not biodegradable and cannot perform quantitative detection.
A visual detection kit based on magnetic core-shell nanospheres was used to prepare gel using Fe3O4@PDA-Co2+ nanospheres and TMB/H2O2 chemiluminescence system combined with cassava starch. The RGB values of the chromogenic gel were extracted and grayscaled through smartphone software. Degree value conversion enables semi-quantitative on-site rapid detection of TNT.
It realizes TNT detection that is environmentally friendly, low-cost, simple to operate, highly selective and highly sensitive, and can accurately detect TNT in the range of 0.2-23 μM, meeting the detection needs of trace amounts and above of trace amounts of TNT in the environment, and providing a portable On-site rapid detection method.
Smart Images

Figure CN118501133B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nitro compound detection, and is a preparation method for a visualized on-site detection kit for detecting TNT based on magnetic core-shell nanospheres. Background Art
[0002] As a kind of high-energy explosive, nitroaromatic compounds (NACs) play an important role in the production and life of modern society. Its use has brought great convenience to mankind and promoted the progress and development of society. However, TNT and its derivatives remaining in the environment can easily affect human health through the food chain, causing headaches, anemia, cataracts, toxic hepatitis and other diseases, and even induce cancer and death in severe cases. Therefore, accurate detection of TNT in the environment is of great significance to the ecological environment and human health. The traditional detection methods of TNT mainly include high-performance liquid chromatography-mass spectrometry (GC-MS), gas chromatography, etc. New detection methods include fluorescence, electrochemical method, Raman spectroscopy, etc. These detection methods have their own disadvantages, such as complex pre-treatment, time-consuming, expensive large instruments, inconvenient on-site detection, and need for professional technicians to operate.
[0003] The visualization method can directly observe the color change of the solution with the naked eye. Compared with other analytical methods, it has a series of significant advantages such as low dependence on analytical instruments, rapidity, low cost, and simple operation. These advantages make this method have great practical application potential in the field of on-site detection. Usually, the substrate preparation of the visualization sensor uses PVA and other substances. Although such substances have good cost-effectiveness, their non-biodegradability will cause environmental harm, limiting the practical application of this method; in addition, the detection type of the visualization sensor is generally qualitative detection, which is not conducive to the accurate detection of TNT in a large range.
[0004] In view of the above problems, a visual detection kit for detecting TNT that is environmentally friendly, easy to operate, highly selective and highly sensitive is urgently needed in the industry. Summary of the invention
[0005] In view of the above shortcomings, the present invention provides a visualization detection kit for detecting TNT based on magnetic core-shell nanospheres. The visualization detection kit uses environmentally friendly and harmless cassava starch combined with the visualization sensor to prepare a portable visualization gel kit, and further uses the smart phone Color Coll software to extract the RGB value of the color gel and convert it into a grayscale value to quantitatively detect TNT to solve the core technical problems that the existing TNT visualization sensor substrate preparation material is environmentally harmful, the sensor cannot perform quantitative detection, and the detection accuracy is low, and it also makes up for the key technical problem of the lack of on-site rapid detection methods for TNT in the past. The present invention is achieved through the following technical solutions:
[0006] The present invention first discloses a visualization detection kit for detecting TNT based on magnetic core-shell nanospheres, comprising: a visualization sensor and a gel substrate, wherein:
[0007] The visual sensor comprises: core-shell Fe3O4@PDA-Co 2+ Nanospheres and TMB (3,3',5,5'-tetramethylbenzidine) / H2O2 chemiluminescent system;
[0008] The gel base is prepared from cassava starch.
[0009] The raw materials used in the present invention are all conventional raw materials, which can greatly save costs compared with existing TNT detection materials.
[0010] The principle of the present invention is: using nano-iron oxide particles (Fe3O4) as the core, dopamine (DA) self-aggregates into polydopamine (PDA) on its surface to form Fe3O4@PDA nanospheres with core-shell structure; adding divalent cobalt ions (Co 2+ ) after that, the catechol groups on the PDA surface can bind Co 2+ Fixed on the surface of the material to synthesize Fe3O4@PDA-Co 2+ Nanospheres. Fe3O4@PDA-Co 2+Nanospheres are added as catalysts to the TMB / H2O2 color development system, which can catalyze the production of a large number of hydroxyl free radicals to oxidize colorless TMB into blue oxTMB, thereby increasing the degree to which the solution turns blue. Using a UV-visible spectrophotometer to assist in detection, it can be found that the absorbance signal of TMB at a wavelength of 652 nm increases. At this time, nucleophilic reaction will occur between the electron-rich amino group and the electron-deficient nitro aromatic ring of TNT, which will form a Meisenheimer complex with TMB and weaken or even prevent the oxidation color development of TMB. Based on the principle that the higher the TNT concentration, the lower the degree of TMB oxidation, and the lighter the color of the solution, the RGB value of the color development is recorded using a smartphone color picking software and converted into a grayscale value. A visual sensor is constructed through the change of grayscale value to achieve semi-quantitative on-site rapid detection of TNT in the environment.
[0011] The present invention also discloses a method for preparing a visualization detection kit for detecting TNT based on magnetic core-shell nanospheres, comprising the following steps:
[0012] (1) Core-shell Fe3O4@PDA-Co 2+ Nanospheres:
[0013] A certain amount of Fe3O4@PDA powder was weighed and dissolved in CoCl2·6H2O solution and mechanically stirred at room temperature for 0.5 h to obtain Fe3O4@PDA-Co 2+ The nanosphere solution was washed alternately with ultrapure water and ethanol and then dispersed in ultrapure water. The solution was centrifuged at high speed and then placed in a drying oven for vacuum drying for 8 h to obtain the core-shell Fe3O4@PDA-Co 2+ Nano balls are spare;
[0014] (2) Prepare TMB / H2O2 chemiluminescence system.
[0015] (3) Preparation of visualization kit:
[0016] The TMB solution was added to the centrifuge tube, and the starch gel was transferred to the centrifuge tube cap by a large syringe. The tube cap was closed and frozen for storage. The preparation and storage of the visualization kit using the centrifuge tube as the reaction vessel was completed.
[0017] Furthermore, the Fe3O4@PDA powder in step (1) is prepared by the following method:
[0018] Fe3O4 and dopamine were added to Tris-HCl buffer solution, and mechanical stirring was performed at room temperature for 6 h to obtain Fe3O4@PDA nanosphere solution. The solution was washed alternately with ultrapure water and ethanol and then dispersed in ultrapure water. After high-speed centrifugation, it was placed in a drying oven and vacuum dried to obtain Fe3O4@PDA powder, which was ground for later use.
[0019] Furthermore, the Tris-HCl buffer solution has a concentration of 10 mM, pH=8.5, and is stored at room temperature; the mass ratio of Fe3O4 to dopamine (DA) is 1:1.
[0020] Furthermore, the rotation speed of the high-speed centrifugal separation is 8000 rpm, the time is 10 min, and the drying condition of the Fe3O4@PDA powder is vacuum drying at 60-80°C for 8 h.
[0021] Furthermore, in step (2), the TMB concentration used was 2.5 mM, which was accurately prepared with DMSO and stored in a refrigerator at 4°C; the H2O2 concentration used was 12 mM, which was prepared fresh for each experiment.
[0022] Furthermore, the starch gel in step (3) is prepared by the following method:
[0023] Add cassava starch, H2O2 solution, Fe3O4@PDA-Co 2+ The nanosphere solution and acetate buffer solution are added, and the resulting milky white mixture is continuously stirred in a water bath until it becomes a transparent starch gel.
[0024] Furthermore, the concentration of H2O2 is 12 mM, which is ready for use; Fe3O4@PDA-Co 2+ The concentration of the nanosphere solution was 1.5 mg / mL; the concentration of the acetate buffer was 0.1 M, and the pH was 4.0.
[0025] Furthermore, the dosage ratio of the cassava starch to the H2O2 solution is 1g:1mL.
[0026] Furthermore, the cassava starch and Fe3O4@PDA-Co 2+ The dosage ratio of the nanosphere solution is 1 g:1 mL.
[0027] Furthermore, the usage ratio of the cassava starch to the acetate buffer is 1 g:2 ml.
[0028] Furthermore, the water bath temperature is 80° C. and the stirring time is 10 min.
[0029] Furthermore, in step (3), the TMB concentration is 2.5 mM, and the added volume is 50 μL.
[0030] Furthermore, the storage temperature of the final centrifuge tube in step (3) is 4°C.
[0031] The present invention also discloses a visualization detection kit for detecting TNT based on magnetic core-shell nanospheres, which is prepared according to any of the above preparation methods.
[0032] The present invention also discloses a method for using the above-mentioned visualization detection kit for detecting TNT based on magnetic core-shell nanospheres, comprising the following steps:
[0033] Take out a prepared visualization detection kit based on magnetic core-shell nanospheres to detect TNT, add TMB solution and the sample to be tested into the centrifuge tube at a volume ratio of 1:1, invert the centrifuge tube and wait for the reaction for 30 minutes. After collecting the image of the color starch gel on the tube cap through the smartphone, use the Color Coll application to capture the color image of the starch gel, convert it into grayscale value, and read the data.
[0034] Furthermore, the concentration of the TMB solution is 2.5 mM.
[0035] In summary, compared with the prior art, the present invention has the following advantages and beneficial effects:
[0036] 1. The visualized gel kit synthesized by the present invention is prepared in situ using cassava starch. The reagent is green, environmentally friendly, biodegradable, and environmentally friendly;
[0037] 2. The present invention is simple to operate, fast to detect, and low in cost. The visualization kit provided by the present invention is easy to carry and has good selectivity;
[0038] 3. High sensitivity, with a linear range of 0.2-23 μM and a detection limit of 14.3 nM, which meets the detection requirements of the maximum residue limit of TNT in soil (300 mg / kg) stipulated by EPA. It can detect both lower concentrations of TNT and accurate detection of concentrations close to the microgram level, providing a new method for on-site detection and analysis of trace and above-trace TNT in the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] FIG1 is a schematic diagram showing the principle of detecting TNT by a visualization detection kit provided by the present invention;
[0040] Figure 2 shows Fe3O4@PDA-Co prepared in Example 1 2+ Scanning electron microscope (SEM) images of the materials;
[0041] FIG3 is a graph showing absorbance curves of different materials in a color development system;
[0042] FIG4 is a histogram showing the color development of different reagents;
[0043] Figure 5 is a linear study diagram of the color development of the kit-TNT concentration, wherein a is a schematic diagram of the color development of the kit, and b is a linear relationship diagram between the gray value and the TNT concentration. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and various embodiments and verification examples. It should be understood that the specific embodiments and verification examples described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments.
[0045] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this method adopt conventional test methods in the art. The terms described in the present invention are only for describing specific implementation methods and are not intended to limit the content disclosed in the present invention.
[0046] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the invention belongs; other raw materials, reagents, experimental methods and technical means not specifically specified in the present invention refer to the raw materials and reagents commonly used by ordinary technicians in the field, as well as the commonly used experimental methods and technical means.
[0047] Example 1
[0048] Figure 1 The schematic diagram of the visual detection kit provided by the present invention for detecting TNT; this example discusses the preparation, feasibility, selectivity, detection range, etc. of the kit provided by the present invention, and the specific contents are as follows:
[0049] (1) Fe3O4@PDA-Co 2+ Preparation of nanospheres:
[0050] 1 g of Fe3O4 nanomaterials and 1 g of dopamine were dissolved in 500 ml of Tris-HCl buffer solution (10 mM, pH = 8.5), and mechanically stirred continuously for 6 h. The solution was washed alternately with ultrapure water and ethanol three times to obtain Fe3O4@PDA nanosphere solution. The solution was placed in a drying oven at 60°C and vacuum dried for 8 h to obtain Fe3O4@PDA powder, which was ground for later use. 1.1897 g of CoCl2·6H2O was weighed in a volumetric flask and diluted to 50 ml with the above Tris-HCl solution to prepare 50 mM Co 2 + solution, in which Co2+ 50 mg Fe3O4@PDA powder was added to the solution and mechanical stirring was continued for 0.5 h to prepare Fe3O4@PDA-Co 2 + The nanosphere solution was washed alternately with ultrapure water and ethanol three times and dried under vacuum at 40 °C for 8 h to obtain Fe3O4@PDA-Co 2+ The nanosphere powder is ground and used for later use. Its SEM is shown in Figure 2.
[0051] (2) Configure the TMB color development system and verify its color development:
[0052] Add 50 μL of TMB solution (2.5 mM) and 250 μL of acetate buffer (pH = 4.0, 0.1 M) to the microplate. After waiting for 8 min, take visual photos with a camera, record the absorbance curve of the solution at 500-800 nm with a UV-visible spectrophotometer, and record the absorbance value of TMB at 652 nm.
[0053] (3) Prepare TMB / H2O2 color development system and verify its color development:
[0054] Add 50 μL of TMB solution (2.5 mM), 50 μL of H2O2 solution (12 mM), and 200 μL of acetate buffer (pH=4.0, 0.1 M) to the well plate. After waiting for 8 min, take visual photos with a camera, record the absorbance curve of the solution at 500-800 nm with a UV-visible spectrophotometer, and record the absorbance value of TMB at 652 nm.
[0055] (4) Fe3O4@PDA-Co 2+ Nanosphere catalytic color development verification:
[0056] Add 50 μL of TMB solution (2.5 mM), 50 μL of H2O2 solution (12 mM), and 150 μL of acetate buffer (pH = 4.0, 0.1 M) to the well plate, and then add 50 μL of Fe3O4@PDA-Co 2+ Nanosphere solution (1.5 mg / mL), wait for 8 min, take visual photos with a camera, record the absorbance curve of the solution from 500 to 800 nm with a UV-visible spectrophotometer, and record the absorbance value of TMB at 652 nm.
[0057] (5) Construction of visual sensor:
[0058] First, 50 μL of H2O2 solution (12 mM), 100 μL of acetate buffer (pH = 4.0, 0.1 M), and 50 μL of Fe3O4@PDA-Co 2+ nanosphere solution (1.5 mg / mL), followed by 50 μL of TNT solution (300 nM), and finally 50 μL of TMB solution (2.5 mM). After waiting for 8 min, a visual photograph was taken with a camera, and the absorbance curve of the solution from 500 to 800 nm was recorded with a UV-visible spectrophotometer, and the absorbance value of TMB at 652 nm was recorded.
[0059] Prepare TNT solutions of different concentrations, add 50 μL of TNT solution to each visualization kit, then add 50 μL of TMB solution (2.5 mM) to the reaction system and invert for 30 minutes. After collecting images of the color-developed starch gel on the tube cap using a smartphone, use the Color Coll application to capture the color image of the starch gel, read the R, G, and B values of each pixel point in turn, perform grayscale conversion, and read the value. The grayscale conversion formula is: Grey=0.299* R +0.587* G +0.114* B , where R is red, G is green, and B is blue.
[0060] like Figure 3 As shown in the figure, the luminescence curves measured by (2) to (5), where a: TMB solution; b: TMB-H2O2 mixed solution; c: Fe3O4@PDA-Co 2+ Nanospheres, TMB-H2O2 mixed solution; d: TNT, Fe3O4@PDA-Co 2+ Nanospheres, TMB-H2O2 mixed solution, it is not difficult to see that compared with Fe3O4@PDA-Co 2+ The color change catalyzed by nanospheres was not obvious in TMB solution alone and TMB-H2O2 mixed solution. 2+ The catalytic performance of Fe3O4@PDA was significantly enhanced, and when TNT was present, its color development signal was significantly increased to below the baseline, indicating that the presence of TNT can significantly inhibit the color development of the color development system. This verifies the principle hypothesis of the present invention.
[0061] As shown in FIG. 4 , when TNT in (5) is replaced with other samples to be tested, it can be seen that the sensor obtained by the present invention has obvious specificity for the detection of TNT.
[0062] As shown in Figure 5, the TNT concentration in (5) is replaced and studied. It can be seen that within the range of 0.2-23 μM, as the TNT concentration continues to increase, the visualized gel color is shown in Figure 5 (a). When the TNT concentration is 0.2 μM, the gel color is the darkest; when the TNT concentration increases to 1.0 μM, the gel color gradually becomes lighter. When the TNT concentration is 23 μM, the gel fades, and within this range, there is a good linear relationship between the TNT concentration and the grayscale value, as shown in Figure 5 (b). The linear equation is y =183.38866-2.33368 C TNT (µM).
[0063] The above examples and verification examples only express the specific implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of protection of the present application. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, which all belong to the scope of protection of the present application.
Claims
1. A method for using a visual on-site detection kit for detecting TNT based on magnetic core-shell nanospheres, the method comprising: Take out a visual on-site detection kit based on magnetic core-shell nanospheres to detect TNT, add a 2.5mM TMB solution and the sample to be tested in a volume ratio of 1:1 into a centrifuge tube, invert the centrifuge tube and wait for the reaction for 30 minutes, collect the image of the color starch gel on the tube cap through a smartphone, use the Color Coll application to capture the color image of the starch gel, convert it into grayscale value, and read the data; where: The visual on-site detection kit for detecting TNT based on magnetic core-shell nanospheres includes a visual sensor and a gel substrate; Visual sensors include: core-shell Fe3O4@PDA-Co 2+ Nanospheres and TMB / H2O2 chemiluminescent system; The gel base is made from tapioca starch; The core-shell Fe3O4@PDA-Co 2+ The nanospheres were prepared by the following method: Fe3O4@PDA powder was weighed and dissolved in CoCl2·6H2O solution and mechanically stirred at room temperature for 0.5 h to obtain Fe3O4@PDA-Co 2+ The nanosphere solution was washed alternately with ultrapure water and ethanol and then dispersed in ultrapure water. The solution was centrifuged at high speed and then placed in a drying oven for vacuum drying for 8 h to obtain the core-shell Fe3O4@PDA-Co 2+ Nano balls are spare; The TMB / H2O2 chemiluminescent system was prepared as follows: Use 2.5 mM TMB and 12 mM H2O2 to prepare the TMB / H2O2 chemiluminescent system, and prepare it fresh for use each time; The starch gel is prepared by the following method: In a 100 mL beaker, add 1 g of cassava starch, 1 mL of H2O2 solution, and 1 mL of Fe3O4@PDA-Co 2+ The nanosphere solution and 2 mL of acetate buffer were added, and the resulting mixture was continuously stirred in a water bath at 80°C for 10 min until it became transparent, and the starch gel was obtained for use; The visualization kit is prepared by the following method: Add 50 μL of TMB solution with a concentration of 2.5 mM into a centrifuge tube, and use a large syringe to transfer the starch gel to the cap of the centrifuge tube. Cover the tube with the cap and store it in a freezer at 4°C.
2. The method of use according to claim 1, wherein: The Fe3O4@PDA powder is prepared by the following method: Fe3O4 and dopamine were added to Tris-HCl buffer solution, and mechanical stirring was performed at room temperature for 6 hours to obtain Fe3O4@PDA nanosphere solution; the Fe3O4@PDA nanosphere solution was washed alternately with ultrapure water and ethanol, dispersed in ultrapure water, separated by high-speed centrifugation, and placed in a drying oven for vacuum drying to obtain Fe3O4@PDA powder, which was ground for later use.
3. The method of use according to claim 2, wherein: The Tris-HCl buffer solution has a concentration of 10 mM, pH=8.5, and is stored at room temperature; The mass ratio of Fe3O4 to dopamine is 1:1; The speed of the high-speed centrifugation is 8000 rpm, and the centrifugation time is 10 min; The drying condition is vacuum drying at 60-80°C for 8 h.
