A high-power ternary positive electrode material and preparation method thereof

By coating the surface of the ternary cathode material with a boron coating and controlling the migration of boron, the problem of reduced cycle life and high-temperature performance of high-nickel materials when the rate performance is improved is solved, and the stability and performance of the material are comprehensively improved.

CN118507694BActive Publication Date: 2024-10-29YINGDE KEHENG NEW ENERGY TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410911749.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-29
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

While existing high-nickel ternary cathode materials improve rate performance, they easily lead to a decrease in cycle life and high-temperature performance, making it difficult to achieve both stability and performance improvement.

Method used

By coating the surface of the ternary cathode material with a boron coating layer and controlling the amount of boron added and the sintering temperature, boron migrates into the material to form shallow doping, thereby improving the material's stability, rate performance and cycle performance.

Benefits of technology

The conductivity and surface density of the cathode material are improved, which significantly improves the stability and cycle performance while avoiding the decline in rate performance and high temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118507694B_ABST
    Figure CN118507694B_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of cathode material preparation, and discloses a high-power ternary cathode material, wherein the high-power ternary cathode material comprises a core layer, a boron coating layer and a silicon coating layer sequentially coated on the outer surface of the core layer, wherein the core layer is doped with boron element, wherein the boron element doped in the core layer is obtained by the migration of the boron element in the boron coating layer into the core layer during the sintering process, and the total molar number of boron in the high-power ternary cathode material is equal to the total molar number of boron in the core layer LiNi (1‑x‑y) Co x Mn y The molar ratio of O2 is 0.018~0.045:1, and the sintering temperature is 700~900℃. Through the above design, the thickness of the boron coating layer on the surface of the core layer is reduced and the unevenness on the surface of the core layer is gradually filled, thereby increasing the bonding ability of the silicon coating layer, thereby improving the stability of the positive electrode material. In addition, the application also discloses a method for preparing a high-power ternary positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cathode material preparation, and in particular to a high-power ternary cathode material and a preparation method thereof. Background Art

[0002] High-power high-nickel ternary cathode materials have attracted wide attention due to their high energy density, large discharge current and high rate, and are widely used in various high-end aircraft models, drones, car models and other products. Studies have shown that with the increase of nickel content, high-nickel ternary materials are prone to have essential properties such as poor cycle life and poor high-temperature performance. However, the measures to improve high-temperature performance are exactly the opposite of the measures to improve rate performance.

[0003] Common methods for improving the rate performance of high nickel materials include: reducing the primary grain and secondary particle size of high nickel ternary materials, coating the surface with materials with better ionic conductivity or electronic conductivity, and designing the morphology of material powder to be loose and porous to facilitate Li + Insertion and extraction during charge and discharge, etc. However, while the above methods improve the rate performance, they tend to increase the specific surface area of ​​the material, increase the contact area between the material and the electrolyte, and make the cycle life of the material worse, especially the high-temperature performance is seriously reduced. Therefore, in order to improve the rate performance while taking into account the cycle performance and high-temperature performance, it is necessary to make major improvements to the high-nickel positive electrode material.

[0004] Prior art 1: 202311483740.0 discloses a high-nickel ternary positive electrode material and a preparation method and application thereof, wherein the preparation method of the high-nickel ternary positive electrode material comprises: mixing a high-nickel precursor, a lithium source and an additive, sintering once, and crushing to obtain a sintered material;

[0005] Obtaining a silicate solution;

[0006] A sintered material is immersed in a silicate solution for coating treatment to obtain a silicate-coated high-nickel material, and then the silicate-coated high-nickel material is mixed with boric acid and subjected to secondary sintering to obtain the obtained material.

[0007] This scheme first uses silicate to modify the surface of the high-nickel ternary positive electrode material, so that the positive electrode material produces a textured network structure, fixes the primary particles, inhibits the precipitation of lithium ions in the internal structure, delays the evolution of cracks, and alleviates the internal strain from the anisotropic volume change; then boric acid is used for further modification to enhance the material's high temperature resistance, increase the lattice stability of the high-nickel material, and improve the material's cycle performance.

[0008] Through careful observation of the above scheme, it can be seen that the structure of the high-nickel ternary positive electrode material obtained is a core-shell structure with a high-nickel ternary positive electrode material precursor as a core layer and a silicate as a coating layer. At the same time, boric acid is further used to modify the high-nickel ternary positive electrode material coated with silicate to obtain a high-nickel ternary positive electrode material. Although this scheme improves the stability, high temperature resistance and cycle performance of the positive electrode material through the above design, it can be seen that the structure of the ternary positive electrode material of this scheme is essentially different from that of the present application.

[0009] Prior art 2: 202310488200.5 discloses a lithium-ion secondary battery, comprising a positive electrode plate, a negative electrode plate, an electrolyte and a separator; the positive electrode plate comprises a positive electrode current collector, a positive electrode active material layer and a protective film layer; the protective film layer contains a boron compound; the positive electrode active material layer comprises a lithium-cobalt-based ternary material; the mass percentage of the boron compound in the positive electrode active material layer is b, 0<b≤0.05%; the mass percentage of the boron compound in the electrolyte is a, 0.1%≤a≤12%; the mass concentration λ of the boron element and the mass concentration ε of the cobalt element in the positive electrode material layer satisfy: 750-λ≤32.54ln(ε)≤1400-λ, and the units of λ and ε are ppm;

[0010] The scheme controls the mass concentration λ of the boron element and the mass concentration ε of the cobalt element in the positive electrode material layer to meet 750-λ≤32.54ln(ε)≤1400-λ, where the units of λ and ε are ppm, to ensure that the lithium-ion secondary battery has good structural stability, dynamic performance, cycle performance, storage performance and safety performance.

[0011] At the same time, it can be seen from the scheme that the positive electrode active material of the lithium ion secondary battery in the scheme is doped with a compound containing boron, and at the same time, its protective film layer, i.e., the coating layer, contains a boron compound;

[0012] And from observing this scheme, it can be seen that the electrolyte of this scheme needs to contain boron compounds. Based on the total mass of the electrolyte, the mass percentage of the boron compound in the electrolyte is a, 0.1%≤a≤12%, and the present application does not have too many requirements for the electrolyte.

[0013] The problem that this solution needs to solve is: how to provide a ternary positive electrode material with high power. Summary of the invention

[0014] The purpose of the present application is to provide a ternary positive electrode material with high power, wherein the ternary positive electrode material is coated with a boron coating layer on the surface of the ternary positive electrode material, and the boron is allowed to migrate and enter the interior of the ternary positive electrode material to form a shallow layer of boron doping by controlling the amount of boron added and the sintering temperature, thereby improving the stability, rate performance and cycle performance of the positive electrode material;

[0015] Another object of the present application is to provide a method for preparing a ternary positive electrode material with high power;

[0016] To achieve the above-mentioned purpose, the present application discloses a high-power ternary positive electrode material, the high-power ternary positive electrode material comprising a core layer and a boron coating layer and a silicon coating layer sequentially coated on the outer surface of the core layer, wherein the core layer is doped with boron element;

[0017] The boron element doped in the core layer is obtained by the migration of the boron element into the core layer during the sintering process of the boron coating layer;

[0018] The ratio of the total molar amount of boron in the high-power ternary cathode material to the molar amount of the core layer is 0.018 to 0.045:1.

[0019] The temperature of the sintering process is 700-900°C.

[0020] Preferably, the core layer is LiNi (1-x-y) Co x Mn y O2, where x>0, y>0, x+y<1.

[0021] Preferably, the core layer is LiNi (1-x-y) Co x Mn y O2, where x>0, y>0, x+y≤0.2.

[0022] Preferably, the core layer is LiNi (1-x-y) Co x Mn y O2, where x>0, y>0, x+y=0.17.

[0023] In addition, the present application also discloses a method for preparing the above-mentioned high-power ternary cathode material, comprising the following steps:

[0024] Step 1: Mixing, sintering and crushing the ternary cathode material precursor and the compound containing lithium element to obtain a core layer;

[0025] Step 2: mixing the compound containing boron with the core layer obtained in step 1, sintering, and cooling to obtain an intermediate having a core layer doped with boron and a boron coating layer;

[0026] Step 3: coating the surface of the intermediate obtained in step 2 with silicon to obtain a high-power ternary cathode material;

[0027] The ratio of the molar amount of boron in the compound containing the boron element to the molar amount of the core layer is 0.018-0.045:1;

[0028] The temperature of the sintering process in step 2 is 700-900°C.

[0029] It should be further explained that, since the ternary positive electrode material has different sintering temperatures under different nickel contents, in the art, as the nickel content decreases, the sintering temperature should be increased accordingly. Therefore, in step 1, when the ternary positive electrode material precursor is Ni (1-x-y) Co x Mn y O2, where x>0, y>0;

[0030] And when 0.4<x+y<0.5, the sintering temperature in step 1 is recommended to be adjusted to 850~900℃;

[0031] When 0.2<x+y<0.4, the sintering temperature in step 1 is recommended to be adjusted to 800~850℃;

[0032] When 0<x+y<0.2, the sintering temperature in step 1 is recommended to be adjusted to 700~800℃;

[0033] Preferably, the ternary cathode material precursor is Ni (1-x-y) Co x Mn y O2, where x>0, y>0, x+y<1;

[0034] The compound containing lithium is selected from at least one of lithium hydroxide, lithium carbonate, lithium sulfate and lithium chloride;

[0035] The ratio of the molar amount of lithium element in the compound containing lithium element to the total molar amount of nickel, cobalt and manganese elements is 1:1.03-1.05.

[0036] Preferably, the compound containing boron is selected from at least one of lithium bis(oxalatoborate), lithium tetrafluoroborate, boric acid and lithium borate.

[0037] Preferably, the compound containing boron is lithium bis(oxalatoborate).

[0038] Preferably, the step 3 specifically comprises: placing the intermediate obtained in step 2 in an aqueous solution containing silica sol, stirring, centrifuging, drying, and heat treating to obtain a high-power ternary positive electrode material;

[0039] The mass ratio of the intermediate to the silica sol is 500:0.8-1.2.

[0040] Preferably, in step 2, the sintering process is specifically as follows: heating the mixture of the compound containing the boron element and the core layer to 700-900° C. and keeping the temperature for 6-8 hours, cooling after the heat preservation, and obtaining an intermediate having the core layer doped with the boron element and the boron coating layer;

[0041] The heat treatment temperature in step 3 is 280-320° C. and the time is 4-8 hours.

[0042] The beneficial effect of the present application is as follows: the present application coats a boron coating layer on the surface of the ternary positive electrode material, and by controlling the amount of boron added and the sintering temperature, the boron migrates and enters the interior of the ternary positive electrode material to form a shallow boron doping; at the same time, as the boron in the boron coating layer migrates into the interior of the ternary positive electrode material, the thickness of the boron coating layer decreases, so that the low-thickness boron coating layer can not only improve the conductivity of the positive electrode material, but also play a role in leveling the surface depressions of the material, thereby to a certain extent improving the density and bonding strength of the silicon coating layer in the later silicon coating process, thereby improving the stability, rate performance and cycle performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is an electron microscope image of the high-power ternary positive electrode material prepared in Example 1;

[0044] Figure 2 This is an electron microscope image of the intermediate obtained in step 2 of Example 1;

[0045] Figure 3 This is an electron microscope image of the intermediate obtained in step 2 of comparative example 3. DETAILED DESCRIPTION

[0046] The present application will be described clearly and completely below in conjunction with the examples of the present application. In the description of the present application, it should be noted that if the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0047] Example 1

[0048] Step 1: Prepare the ternary cathode material precursor (Ni 0.83 Co 0.12 Mn 0.05 O2) is mixed with a compound containing lithium, sintered at 750℃ for 15h and then broken to obtain a core layer;

[0049] The compound containing lithium element is lithium hydroxide;

[0050] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1.04:1;

[0051] Step 2: Mix the compound containing the boron element with the core layer and heat the mixture of the compound containing the boron element and the core layer to 750° C. and keep it warm for 7 hours. After the heat preservation is completed, cool it to obtain an intermediate with the core layer doped with boron element and a boron coating layer;

[0052] The ratio of the molar amount of boron in the intermediate having a boron coating layer and a core layer is 0.0315:1, and the compound containing boron is lithium bis(oxalatoborate);

[0053] Step 3: placing the intermediate obtained in step 2 in an aqueous solution containing silica sol, stirring, centrifuging, and drying at a temperature of 300° C. for 6 hours to obtain a high-power ternary cathode material;

[0054] The mass ratio of the intermediate to the silica sol is 500:1.

[0055] Example 2

[0056] The method is basically the same as Example 1, except that the molar ratio of boron in lithium bis(oxalatoborate) to the molar ratio of the core layer is 0.018:1.

[0057] Example 3

[0058] The method is basically the same as Example 1, except that the molar ratio of boron in lithium bis(oxalatoborate) to the molar ratio of the core layer is 0.045:1.

[0059] Example 4

[0060] The method is basically the same as Example 1, except that step 2 is: mixing the compound containing the boron element with the core layer, heating the mixture of the compound containing the boron element and the core layer to 700° C. and keeping the temperature for 7 hours, cooling after the heat preservation, and obtaining an intermediate having a core layer doped with the boron element and a boron coating layer;

[0061] The molar ratio of boron in the compound containing boron element to the molar ratio of the core layer is 0.0315:1.

[0062] Example 5

[0063] The method is basically the same as Example 1, except that step 2 is: mixing the compound containing the boron element with the core layer, heating the mixture of the compound containing the boron element and the core layer to 900° C. and keeping the mixture for 7 hours, cooling the mixture after the heat preservation, and obtaining an intermediate having a core layer doped with the boron element and a boron coating layer;

[0064] The molar ratio of boron in the compound containing boron element to the molar ratio of the core layer is 0.0315:1.

[0065] Example 6

[0066] It is basically the same as Example 1, except that the precursor of the ternary positive electrode material is Ni 0.88 Co 0.09 Mn 0.03 O2.

[0067] Example 7

[0068] It is basically the same as Example 1, except that the precursor of the ternary positive electrode material is Ni 0.88 Co 0.09 Al 0.03 O2.

[0069] Example 8

[0070] It is basically the same as Example 1, except that the precursor of the ternary positive electrode material is Ni 0.6 Co 0.2 Mn 0.2 O2.

[0071] Example 9

[0072] It is basically the same as Example 1, except that the precursor of the ternary positive electrode material is Ni 0.5 Co 0.2 Mn 0.3 O2.

[0073] It should be noted that, since the ternary cathode material has different sintering temperatures under different nickel contents, in the art, as the nickel content decreases, the sintering temperature should be increased accordingly. Therefore, in step 1, when the ternary cathode material precursor is Ni (1-x-y) Co x Mn y O2, where x>0, y>0;

[0074] And when 0.4<x+y<0.5, the sintering temperature in step 1 should be adjusted to 850~900℃;

[0075] When 0.2<x+y<0.4, the sintering temperature in step 1 should be adjusted to 800~850℃;

[0076] When 0<x+y<0.2, the sintering temperature in step 1 should be adjusted to 700~800℃;

[0077] Therefore, the sintering temperature in step 1 of Examples 6 and 7 is 700°C, the sintering temperature in step 1 of Example 8 is 850°C, and the sintering temperature in step 1 of Example 9 is 900°C.

[0078] Example 10

[0079] Step 1: Prepare the ternary cathode material precursor (Ni 0.83 Co 0.12 Mn 0.05 O2) is mixed with a compound containing lithium, sintered, and crushed to obtain a core layer;

[0080] The compound containing lithium element is lithium hydroxide;

[0081] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1.03:1;

[0082] Step 2: Mix the compound containing boron with the core layer, heat the mixture of the compound containing boron and the core layer to 750° C. and keep it for 7 hours, and cool it after the heat preservation to obtain an intermediate with a core layer doped with boron and a boron coating layer;

[0083] The mass ratio of boron in the compound containing boron to the mass ratio of the core layer is 0.0315:1, and the compound containing boron is lithium tetrafluoroborate;

[0084] Step 3: placing the intermediate obtained in step 2 in an aqueous solution containing silica sol, stirring, centrifuging, and drying at a temperature of 280° C. for 8 hours to obtain a high-power ternary cathode material;

[0085] The mass ratio of the intermediate to the silica sol is 500:0.8.

[0086] Embodiment 11

[0087] Step 1: Prepare the ternary cathode material precursor (Ni 0.83 Co 0.12 Mn 0.05 O2) is mixed with a compound containing lithium, sintered, and crushed to obtain a core layer;

[0088] The compound containing lithium element is lithium hydroxide;

[0089] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1.05:1;

[0090] Step 2: Mix the compound containing boron with the core layer, heat the mixture of the compound containing boron and the core layer to 750° C. and keep it for 7 hours, and cool it after the heat preservation to obtain an intermediate with a core layer doped with boron and a boron coating layer;

[0091] The molar ratio of boron in the compound containing boron to the molar ratio of the core layer is 0.0315:1, and the compound containing boron is boric acid;

[0092] Step 3: placing the intermediate obtained in step 2 in an aqueous solution containing silica sol, stirring, centrifuging, and drying at a temperature of 320° C. for 4 hours to obtain a high-power ternary cathode material;

[0093] The mass ratio of the intermediate to the silica sol is 500:1.2.

[0094] Comparative Example 1

[0095] The method is basically the same as Example 1, except that the molar ratio of boron in the compound containing boron element to the molar ratio of the core layer is 0.01:1.

[0096] Comparative Example 2

[0097] The method is basically the same as Example 1, except that the molar ratio of boron in the compound containing boron element to the molar ratio of the core layer is 0.06:1.

[0098] Comparative Example 3

[0099] The method is basically the same as Example 1, except that step 2 is specifically to crush the core layer obtained in step 1 to obtain a powder, then mix the compound containing the boron element with the powder, heat the mixture of the compound containing the boron element and the powder to 600°C and keep it warm for 7 hours, and cool it after the insulation to obtain an intermediate with a core layer doped with boron and a boron coating layer.

[0100] Comparative Example 4

[0101] The method is basically the same as Example 1, except that step 2 is specifically to crush the core layer obtained in step 1 to obtain a powder, then mix the compound containing the boron element with the powder, heat the mixture of the compound containing the boron element and the powder to 1000°C and keep it warm for 7 hours, and cool it after the insulation to obtain an intermediate with a core layer doped with boron and a boron coating layer.

[0102] Comparative Example 5

[0103] It is basically the same as Example 1, except that no boron coating and doping are performed, that is:

[0104] Step 1: Mixing and sintering the ternary cathode material precursor and the compound containing lithium to obtain a core layer;

[0105] The compound containing lithium element is lithium hydroxide;

[0106] The ratio of the molar amount of lithium element in the lithium-containing compound to the total molar amount of nickel, cobalt and manganese elements is 1.04:1;

[0107] Step 2: placing the core layer obtained in step 1 in an aqueous solution containing silica sol, stirring, centrifuging, and drying at a temperature of 300° C. for 6 hours to obtain a ternary positive electrode material;

[0108] The mass ratio of the core layer to the silica sol is 500:1.

[0109] Comparative Example 6

[0110] The method is basically the same as Example 1, except that the silicon element is not coated, that is:

[0111] Step 1: Prepare the ternary cathode material precursor (Ni 0.83 Co 0.12 Mn 0.05 O2) is mixed with a compound containing lithium, sintered, and crushed to obtain a core layer;

[0112] The compound containing lithium element is lithium hydroxide;

[0113] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1.04:1;

[0114] Step 2: Mix the compound containing the boron element with the core layer, heat the mixture of the compound containing the boron element and the core layer to 750°C and keep it warm for 7 hours, and cool it after the insulation to obtain a ternary positive electrode material.

[0115] Comparative Example 7

[0116] Step 1: Mixing and sintering the ternary cathode material precursor and the compound containing lithium to obtain a core layer;

[0117] The compound containing lithium element is lithium hydroxide;

[0118] The ratio of the molar amount of lithium element in the lithium-containing compound to the total molar amount of nickel, cobalt and manganese elements is 1.04:1;

[0119] Step 2: placing the core layer obtained in step 1 in an aqueous solution containing silica sol, stirring, centrifuging, and drying at a temperature of 300° C. for 6 hours to obtain an intermediate having a silicon coating layer;

[0120] The mass ratio of the core layer to the silica sol is 500:1;

[0121] Step 3: Crush the intermediate with a silicon coating layer obtained in step 2 to obtain a powder, and then mix the compound containing the boron element with the powder. First, heat the mixture of the compound containing the boron element and the powder to 750°C and keep it warm for 7 hours. After the insulation is completed, cool it to obtain a ternary positive electrode material.

[0122] Comparative Example 8

[0123] The method is basically the same as Example 1, except that the boron coating and boron doping in step 2 are carried out in two steps, namely:

[0124] Step 1: Prepare the ternary cathode material precursor (Ni 0.83 Co 0.12 Mn 0.05 O2) is mixed with a compound containing lithium element and lithium bis(oxalatoborate), sintered, and crushed to obtain a core layer doped with boron element, wherein the molar ratio of boron in the lithium bis(oxalatoborate) to the core layer is 0.01575:1;

[0125] The compound containing lithium element is lithium hydroxide;

[0126] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1.04:1;

[0127] Step 2: mixing lithium bis(oxalatoborate) with the core layer, heating the mixture of lithium bis(oxalatoborate) and the core layer to 700° C. and keeping the temperature for 7 hours, cooling after the heat preservation, and obtaining an intermediate in which the core layer is doped with boron element and has a boron coating layer;

[0128] The mass ratio of the boron coating layer to the core layer is 0.01575:1;

[0129] Step 3: placing the intermediate obtained in step 2 in an aqueous solution containing silica sol, stirring, centrifuging, and drying at a temperature of 300° C. for 6 hours to obtain a high-power ternary cathode material;

[0130] The mass ratio of the intermediate to the silica sol is 500:1.

[0131] Comparative Example 9

[0132] It is basically the same as Example 1, except that in step 2, zirconium oxide is used instead of the compound containing boron element, and the molar amount of zirconium element in zirconium oxide is the same as that of boron element.

[0133] Comparative Example 10

[0134] The method is basically the same as Example 1, except that in step 3, aluminum sol is used instead of silica sol.

[0135] Comparative Example 11

[0136] The ternary cathode material precursor (Ni 0.83 Co 0.12 Mn 0.05 O2) is mixed with a compound containing lithium, sintered, and crushed to obtain a positive electrode material;

[0137] The compound containing lithium element is lithium hydroxide;

[0138] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1:1.04.

[0139] Comparative Example 12

[0140] The ternary cathode material precursor (Ni 0.88 Co 0.09 Mn 0.03 O2) is mixed with a compound containing lithium, sintered, and crushed to obtain a positive electrode material;

[0141] The compound containing lithium element is lithium hydroxide;

[0142] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1:1.04.

[0143] Comparative Example 13

[0144] The ternary cathode material precursor (Ni 0.88 Co 0.09 Al 0.03 O2) is mixed with a compound containing lithium, sintered, and crushed to obtain a positive electrode material;

[0145] The compound containing lithium element is lithium hydroxide;

[0146] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1:1.04.

[0147] Comparative Example 14

[0148] The ternary cathode material precursor (Ni 0.6 Co 0.2 Mn 0.2 O2) is mixed with a compound containing lithium, sintered, and crushed to obtain a positive electrode material;

[0149] The compound containing lithium element is lithium hydroxide;

[0150] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1:1.04.

[0151] Comparative Example 15

[0152] The ternary cathode material precursor (Ni 0.5 Co 0.2 Mn 0.3 O2) is mixed with a compound containing lithium, sintered, and crushed to obtain a positive electrode material;

[0153] The compound containing lithium element is lithium hydroxide;

[0154] The ratio of the molar amount of lithium element in the lithium hydroxide to the total molar amount of nickel, cobalt and manganese elements is 1:1.04.

[0155] It should be noted that, since the ternary cathode material has different sintering temperatures under different nickel contents, in the art, as the nickel content decreases, the sintering temperature should be increased accordingly. Therefore, in step 1, when the ternary cathode material precursor is Ni (1-x-y) Co x Mn y O2, where x>0, y>0;

[0156] And when 0.4<x+y<0.5, the sintering temperature in step 1 should be adjusted to 850~900℃;

[0157] When 0.2<x+y<0.4, the sintering temperature in step 1 should be adjusted to 800~850℃;

[0158] When 0<x+y<0.2, the sintering temperature in step 1 should be adjusted to 700~800℃;

[0159] Therefore, the sintering temperature in step 1 of Comparative Examples 12 and 13 is 700°C, the sintering temperature in step 1 of Comparative Example 14 is 850°C, and the sintering temperature in step 1 of Comparative Example 15 is 900°C.

[0160] Performance Testing

[0161] Test method:

[0162] 1. The preparation method of button half-cell is as follows: the active positive electrode material, PVDF and carbon black are mixed in a mass ratio of 94:3:3, and a proper amount of NMP is added and stirred to form a battery slurry. Subsequently, the slurry is evenly coated on an aluminum foil and placed in a 120°C oven for 3 to 10 hours. After drying, the positive electrode sheets are cut into uniform sizes, and the loading amount of active substances on the electrode sheets is 8 to 20 mg / cm 2 The prepared positive electrode sheet was placed in a vacuum glove box, and the metal lithium sheet was used as the negative electrode, and assembled with the separator, electrolyte and other components into a button-type half-cell. After the assembly was completed, the battery was placed on a battery tester for electrical performance testing.

[0163] 2. Rate test: After three cycles of 0.1C at 3.0-4.2V, room temperature 25°C, charge and discharge at different rates of 0.1C / 0.1C, 0.2C / 0.2C, 0.5C / 0.5C, 1C / 1C, 1C / 3C, 1C / 5C, 1C / 8C. Record the discharge capacity at different rates, and calculate the ratio of 8C discharge capacity to 0.1C discharge capacity.

[0164] 3.50th / 1st cycle test: 3.0-4.2V, at room temperature 25℃, cycle at 0.1C rate for three weeks, then charge and discharge at 1C / 1C rate for 50 cycles. Record the ratio of the discharge capacity of each cycle to the discharge capacity of the first week.

[0165] The test results are shown in Table 1:

[0166] Table 1

[0167] Group Ternary Types Coating and doping elements 8C / 0.1C (%) 50th / 1st (%) Example 1 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 75.23 99.18 Example 2 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 73.54 98.33 Example 3 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 72.15 97.54 Example 4 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 68.77 82.33 Example 5 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 67.28 82.15 Example 6 <![CDATA[LiNi 0.88 What 0.09 Mn 0.03 O2]]> Boron, Silicon 72.21 93.32 Example 7 <![CDATA[LiNi 0.88 Yes 0.09 Al 0.03 O2]]> Boron, Silicon 70.14 92.17 Example 8 <![CDATA[LiNi 0.6 Co0.2Mn 0.2 O2]]> Boron, Silicon 62.33 91.54 Example 9 <![CDATA[LiNi 0.5 What 0.2 Mn 0.3 O2]]> Boron, Silicon 60.58 91.04 Example 10 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 75.04 99.14 Embodiment 11 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 74.98 98.94 Comparative Example 1 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 63.14 89.01 Comparative Example 2 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 61.47 88.77 Comparative Example 3 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 28.22 34.13 Comparative Example 4 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 21.14 11.51 Comparative Example 5 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 58.77 92.12 Comparative Example 6 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 65.88 94.15 Comparative Example 7 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 51.25 85.33 Comparative Example 8 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, Silicon 67.25 93.62 Comparative Example 9 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Zirconium, Silicon 57.14 94.63 Comparative Example 10 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> Boron, aluminum 56.11 90.14 Comparative Example 11 <![CDATA[LiNi 0.83 What 0.12 Mn 0.05 O2]]> \ 58.11 91.54 Comparative Example 12 <![CDATA[LiNi 0.88 What 0.09 Mn 0.03 O2]]> \ 57.21 89.33 Comparative Example 13 <![CDATA[LiNi 0.88 Yes 0.09 Al 0.03 O2]]> \ 56.46 88.27 Comparative Example 14 <![CDATA[LiNi 0.6 Co0.2Mn 0.2 O2]]> \ 50.15 87.14 Comparative Example 15 <![CDATA[LiNi 0.5 What 0.2 Mn 0.3 O2]]> \ 48.11 87.05

[0168] Result analysis:

[0169] 1. It can be seen from Examples 1-3 that when the mass ratio of boron to the mass ratio of the core layer in the present application is 0.0315:1, the rate performance and cycle performance of the prepared positive electrode material are better than those of Examples 2 and 3. Therefore, we believe that when the mass ratio of boron to the mass ratio of the core layer is 0.0315:1, the amount of boron added is the optimal amount. At the same time, we speculate that the reason for the phenomenon may be that when the mass ratio of boron to the mass ratio of the core layer is 0.0315:1, the thickness of the boron coating layer formed and the doping depth of boron are more advantageous than those of Examples 2 and 3. On the one hand, the doping depth of boron in this state is more conducive to the formation of a stable solid solution of boron and transition metal cations, thereby inhibiting cation mixing and reducing the volume change of the crystal structure during charging and discharging, thereby improving the cyclability;

[0170] On the other hand, in this state, the thickness of the boron coating layer increases the bonding strength between the silicon coating layer and the boron coating layer, thereby improving the stability and rate performance of the positive electrode material.

[0171] 2. It can be seen from Example 1 and Examples 4-5 that when the temperature is 750°C during the sintering process of step 2, it is better than Examples 4 and 5. Therefore, we believe that when the temperature is 750°C during the sintering process of step 2, it is the optimal sintering temperature. At the same time, in the actual operation process, we found that the temperature also has a certain influence on the amount of migration of the boron coating layer into the interior of the ternary positive electrode material. When the sintering temperature is low, the migration of boron is low, which leads to insufficient boron doping in the core layer and a thicker boron coating layer; when the sintering temperature is high, the migration of boron increases accordingly, which leads to excessive boron doping in the core layer and a lower boron coating layer.

[0172] 3. It can be seen from Example 1 and Examples 6-9 and Comparative Examples 11-15 that when the positive electrode material is prepared by the boron doping plus boron coating plus silicon coating method described in this application, when the core layer is LiNi 0.83 Co 0.12 Mn 0.05 O2, its ability to improve the rate performance and cycle performance of the positive electrode material is significantly higher than other types of ternary materials. It can be seen that when the method described in this application is applied to LiNi 0.83 Co 0.12 Mn 0.05 O2, its ability to enhance the positive electrode material can be more fully exerted.

[0173] 4. It can be seen from Example 1 and Comparative Examples 1-2 that when the amount of boron added is greatly adjusted, the rate performance and cycle performance of the positive electrode material show a significant downward trend. We speculate that the reason for this phenomenon may be that the boron coating layer of the positive electrode material obtained in Comparative Examples 1 and 2 is too thin, which leads to a decrease in the rate performance and cycle performance of the positive electrode material;

[0174] On the one hand, when the boron coating of the positive electrode material is too thin, the boron coating cannot supplement the unevenness of the material surface, which leads to the poor bonding strength of the silicon coating and the shedding of the silicon coating during subsequent use.

[0175] On the other hand, when the boron coating layer of the positive electrode material is too thick, the boron coating layer of the positive electrode material will fall off during the subsequent silicon coating process or the slurry preparation process, which will lead to deterioration of rate performance and cycle performance.

[0176] 5. It can be seen from Example 1 and Comparative Examples 3-4 that when the temperature changes significantly, the rate performance and cycle performance of the positive electrode material also decline to a certain extent. We believe that this downward trend is also directly caused by the change in the thickness of the boron coating layer.

[0177] 6. It can be seen from Example 1 and Comparative Examples 5-6 that when boron or silicon is not added during the preparation of the positive electrode material, the rate performance and cycle performance of the positive electrode material will show a certain downward trend. We believe that the reason for this phenomenon is that when boron doping and boron coating are not performed, on the one hand, the cation mixing phenomenon in the positive electrode material is aggravated, resulting in a decrease in its cycle performance, and on the other hand, the binding force of the silicon coating layer is significantly reduced, and the silicon coating layer falls off during subsequent use, which further reduces its rate performance and cycle performance;

[0178] When silicon coating is not performed, the reason for the decline in rate performance and cycle performance may be: the structure is unstable at high temperatures and thermal decomposition is prone to occur, especially under conditions of rapid charging and discharging (high rate), which increases heat generation, aggravating the thermal stability problem of the material and affecting the cycle life.

[0179] 7. It can be seen from Example 1 and Comparative Examples 7-8 that when the order of adding boron and silicon is changed, the rate performance of the positive electrode material declines significantly. We believe that the reason for this phenomenon may be that the bonding ability between the silicon coating layer and the core layer is weak, which causes the silicon-boron coating layer to fall off during use, thereby causing the rate performance and cycle performance of the positive electrode material to decline;

[0180] When boron coating and boron doping are carried out in two steps, since the boron in the core layer is not migrated or diffused inward from the coating layer, the bonding force between the boron coating layer and the core layer decreases, which makes the boron coating layer easier to fall off, thereby reducing the rate performance and cycle performance of the material to a certain extent.

[0181] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.

Claims

1. A high-power ternary cathode material, characterized in that: The high-power ternary positive electrode material comprises a core layer and a boron coating layer and a silicon coating layer sequentially coated on the outer surface of the core layer, wherein the core layer is doped with boron element; The boron element doped in the core layer is obtained by the migration of the boron element into the core layer during the sintering process of the boron coating layer; The ratio of the total molar amount of boron in the high-power ternary cathode material to the molar amount of the core layer is 0.018 to 0.045:

1. The temperature of the sintering process is 700-900°C; The compound providing the boron element is selected from at least one of lithium bis(oxalatoborate), lithium tetrafluoroborate, boric acid, and lithium borate; The substance that provides the silicon element in the silicon coating layer is silica sol.

2. The high-power ternary cathode material according to claim 1, characterized in that: The core layer is LiNi (1−x−y) Co x Mn y O2, where x>0, y>0, x+y<1.

3. The high-power ternary cathode material according to claim 1, characterized in that: The core layer is LiNi (1−x−y) Co x Mn y O2, where x>0, y>0, x+y≤0.

2.

4. The high-power ternary cathode material according to claim 1, characterized in that: The core layer is LiNi (1−x−y) Co x Mn y O2, where x>0, y>0, x+y=0.

17.

5. A method for preparing the high-power ternary cathode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: Mixing, sintering and crushing the ternary cathode material precursor and the compound containing lithium element to obtain a core layer; Step 2: mixing the compound containing boron with the core layer obtained in step 1, sintering, and cooling to obtain an intermediate having a core layer doped with boron and a boron coating layer; Step 3: coating the surface of the intermediate obtained in step 2 with silicon to obtain a high-power ternary cathode material; The ratio of the molar amount of boron in the compound containing the boron element to the molar amount of the core layer is 0.018-0.045:1; The temperature of the sintering process in step 2 is 700-900°C.

6. The method for preparing a high-power ternary cathode material according to claim 5, characterized in that: The ternary cathode material precursor is Ni (1−x−y) Co x Mn y O2, where x>0, y>0, x+y<1; The compound containing lithium is selected from at least one of lithium hydroxide, lithium carbonate, lithium sulfate and lithium chloride; The ratio of the molar amount of lithium element in the lithium-containing compound to the total molar amount of nickel, cobalt and manganese elements in the ternary positive electrode material precursor is 1.03-1.05:

1.

7. The method for preparing a high-power ternary cathode material according to claim 5, characterized in that: The compound containing boron element is lithium bis(oxalatoborate).

8. The method for preparing a high-power ternary cathode material according to claim 5, characterized in that: The step 3 specifically comprises: placing the intermediate obtained in the step 2 in an aqueous solution containing silica sol, stirring, centrifuging, drying, and heat treating to obtain a high-power ternary positive electrode material; The mass ratio of the intermediate to the silica sol is 500:0.8-1.

2.

9. The method for preparing a high-power ternary cathode material according to claim 8, characterized in that: In step 2, the sintering process is specifically as follows: heating the mixture of the compound containing the boron element and the core layer to 700-900° C. and keeping the temperature for 6-8 hours, cooling after the heat preservation, and obtaining an intermediate having the core layer doped with the boron element and the boron coating layer; The heat treatment temperature in step 3 is 280-320° C. and the time is 4-8 hours.

Citation Information

Patent Citations

  • Lithium ion secondary battery, design method thereof and electric device

    CN116470125A

  • High-nickel lithium ion battery positive electrode material, preparation method thereof and lithium ion battery

    CN108987728A

  • Cobalt-free layered positive electrode material, preparation method and lithium ion battery

    CN111434618A

  • High-safety double-doped high-nickel ternary positive electrode material, preparation method thereof and lithium ion battery

    CN111646523A

  • Ternary material, preparation method and battery

    CN113363497A